Insulating epoxy resin encapsulation adhesive and preparation method thereof

By using modified polyamide and SiC/Mg(OH)2 nanomaterials in epoxy resin packaging glue, the problem of poor toughness and thermal conductivity after curing is solved, and higher mechanical properties and thermal conductivity are achieved and flame retardant, suitable for the packaging needs of modern electronic products.

CN118308055BActive Publication Date: 2024-12-06JIAXING LIBEIDE FUR APPARELS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410496976.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-24
Publication Date
2024-12-06
Estimated Expiration
2044-04-24

AI Technical Summary

Technical Problem

After curing, epoxy resin packaging glue has high rigidity, poor toughness, brittleness, low thermal conductivity and poor flame retardant performance, which cannot meet the needs of modern electronic products to improve the many performance indicators of packaging materials.

Method used

Modified polyamide and SiC/Mg(OH)2 nanomaterials are used to improve the toughness of the cured substance by modifying polyamide, and the thermal conductivity, insulation and flame retardant of the packaging glue are enhanced by SiC/Mg(OH)2 nanomaterials. sex.

Benefits of technology

The toughness, thermal conductivity, insulation and flame retardancy of packaging glue is improved, making it more widely used in the field of electronic packaging, and meets the needs of modern electronic products to improve the performance of packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GHA0000006567440000101
    Figure GHA0000006567440000101
  • Figure GHA0000006567440000111
    Figure GHA0000006567440000111
Patent Text Reader

Abstract

This invention relates to the field of epoxy resin encapsulants, and discloses an insulating epoxy resin encapsulant and its preparation method. The epoxy resin encapsulant prepared by this invention comprises the following raw materials by weight: 40-60 parts epoxy resin, 10-20 parts curing agent, 5-10 parts modified polyamide, 2-3 parts accelerator, 0.2-1 part defoamer, 10-15 parts SiC / Mg(OH)2 nanomaterials, and 1-2 parts antioxidant. It uses epoxy resin as a raw material, adds polyamide, and modifies it to improve the toughness of the encapsulant, effectively avoiding the brittleness that occurs after curing. The addition of SiC / Mg(OH)2 nanomaterials improves the thermal conductivity, insulation, and flame retardancy of the encapsulant, enabling its wider application in the field of electronic packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of epoxy resin packaging adhesive, and in particular to an insulating epoxy resin packaging adhesive and a preparation method thereof. Background Art

[0002] As electronic products continue to pursue the goals of being light, thin, short and small, chip circuits are highly integrated, wiring is refined, and electronic components are moving towards miniaturization and thinness, which puts higher requirements on the performance indicators of packaging materials, requiring them to have excellent thermal conductivity, mechanical properties, insulation properties, flame retardancy and other indicators. As an indispensable part of electronic products, encapsulation glue has a good encapsulation effect. Common encapsulation glues mainly include epoxy resin encapsulation glue, silicone encapsulation glue and polyurethane encapsulation glue. Epoxy resin encapsulation glue is the most commonly used encapsulation glue and has good insulation, heat dissipation, dustproof and other effects.

[0003] However, with the improvement of electronic product performance, the performance of epoxy resin encapsulant no longer meets the needs of practical applications. For example, after curing, epoxy resin encapsulant has high rigidity, poor toughness, brittleness, low thermal conductivity, poor flame retardancy, etc. Therefore, it is necessary to modify the epoxy resin encapsulant to improve the insulation, thermal conductivity, mechanical properties and flame retardancy of the encapsulant. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides an insulating epoxy resin packaging adhesive and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] An insulating epoxy resin encapsulation adhesive comprises the following raw materials by weight: 40-60 parts of epoxy resin, 10-20 parts of curing agent, 5-10 parts of modified polyamide, 2-3 parts of accelerator, 0.2-1 part of defoamer, 10-15 parts of SiC / Mg(OH)2 nanomaterial, and 1-2 parts of antioxidant;

[0007] The modified polyamide is prepared by the following steps:

[0008] Step A1, add ethylenediamine and methanol into a flask and stir to mix evenly, slowly add methyl acrylate dropwise using a constant pressure dropping funnel, then stir evenly in an ice water bath and nitrogen, complete the dropwise addition within 2 hours, then increase the system temperature to 30-40°C to react for 18-24 hours, and after the reaction is completed, perform reduced pressure distillation to obtain a polyamide precursor;

[0009] Furthermore, the mass ratio of ethylenediamine, methanol and methyl acrylate is 1.35-4.05:5.4-16.2:18.3-54.9.

[0010] Step A2, adding polyamide precursor and methanol into a flask and stirring evenly, slowly adding 3,3'-diaminodipropylamine dropwise in an ice-water bath and nitrogen, and continuing the reaction at room temperature for 24 hours. After the reaction is completed, performing reduced pressure distillation to obtain a hyperbranched polyamide;

[0011] Furthermore, the usage ratio of the polyamide precursor, methanol and 3,3'-diaminodipropylamine is 1.5-4.5 g: 7-21 g: 4.5-13.5 g.

[0012] Step A3, adding a hyperbranched polyamide to a flask containing N,N-dimethylformamide, slowly adding glutaric acid, raising the system temperature to 50-60° C., and continuing the reaction for 8-12 hours. After the reaction is completed, lowering the system temperature to 30° C., adding γ-methacryloxypropyltrimethoxysilane, stirring and reacting for 4-6 hours, and after the reaction is completed, distilling under reduced pressure, washing, filtering, and drying to obtain a modified polyamide;

[0013] Furthermore, the usage ratio of hyperbranched polyamide, N,N-dimethylformamide, glutaric acid and γ-methacryloxypropyltrimethoxysilane is 1-2 g: 50 mL: 2.5-6 g: 0.5-1.5 mL.

[0014] The SiC / Mg(OH)2 nanomaterial is prepared by the following steps:

[0015] Step B1, adding silicon carbide nanosheets to a 5 mol / L potassium hydroxide solution, stirring and mixing evenly, and soaking for 8-12 hours, and then centrifuging, washing, and drying at 40° C. for 12 hours to obtain pre-treated silicon carbide;

[0016] Furthermore, the mass ratio of the silicon carbide nanosheets to the potassium hydroxide solution is 1:20.

[0017] Step B2, dispersing the pre-treated silicon carbide in deionized water, ultrasonically treating for 2 hours, adding melamine and dicyclohexylcarbodiimide, and raising the system temperature to 100-120° C., keeping the temperature for reaction for 5-7 hours, and after the reaction is completed, washing, filtering, and drying to obtain grafted modified silicon carbide;

[0018] Furthermore, the usage ratio of pre-treated silicon carbide, deionized water, melamine and dicyclohexylcarbodiimide is 2-4 g: 50-100 mL: 5-10 g: 5-10 g.

[0019] Step B3, ethanol and γ-glycidyloxypropyltrimethoxysilane are mixed and stirred at 60°C for 30 minutes, then the system temperature is increased to 80-90°C, nano magnesium hydroxide and deionized water are added, and the reaction is stirred for 3-5 hours. After the reaction is completed, centrifugation, washing, and drying are performed to obtain modified magnesium hydroxide;

[0020] Furthermore, the usage ratio of ethanol, γ-glycidyloxypropyltrimethoxysilane, nano-magnesium hydroxide and deionized water is 120 mL: 3-5 mL: 8-15 g: 10 mL.

[0021] Step B4, dispersing the grafted modified silicon carbide and modified magnesium hydroxide in ethanol, stirring for 10-20 minutes, then raising the system temperature to 85-95°C, and stirring the reaction at a speed of 1000-1200 rpm for 12 hours. After the reaction is completed, cooling to room temperature, collecting the solid, washing, filtering, and drying, to obtain SiC / Mg(OH)2 nanomaterials;

[0022] Furthermore, the mass ratio of the grafted modified silicon carbide, the modified magnesium hydroxide and the ethanol is 1:0.5-1.5:10.

[0023] A method for preparing an insulating epoxy resin encapsulation adhesive comprises the following steps:

[0024] The raw materials are weighed by weight, and epoxy resin, modified polyamide, SiC / Mg(OH)2 nanomaterial, defoamer, antioxidant, curing agent and accelerator are added into the reactor. Under vacuum conditions, the mixture is stirred at a speed of 800-1000 rpm for 1-2 hours to obtain an insulating epoxy resin encapsulation adhesive.

[0025] Beneficial effects of the present invention:

[0026] The epoxy resin encapsulating adhesive prepared by the present invention uses epoxy resin as raw material, adds polyamide, and modifies the epoxy resin, thereby improving the toughness of the encapsulating adhesive and effectively avoiding the brittle phenomenon after the encapsulating adhesive is cured; SiC / Mg(OH)2 nanomaterials are added to improve the thermal conductivity, insulation and flame retardancy of the encapsulating adhesive, so that the encapsulating adhesive has a wider application in the field of electronic packaging.

[0027] In the modified polyamide, firstly, methyl acrylate and ethylenediamine are used as raw materials, and a polyamide precursor containing a terminal ester group is synthesized by utilizing the reaction between an amino group and a double bond; secondly, the terminal ester group in the polyamide precursor is reacted with an amino group in 3,3'-diaminodipropylamine to generate a hyperbranched polyamide containing a hyperbranched structure; finally, the amino group in the hyperbranched polyamide is reacted with a carboxyl group in glutaric acid, and then γ-methacryloxypropyltrimethoxysilane is added, and the double bond in the silane coupling agent is reacted with a secondary amine in the hyperbranched polyamide, thereby introducing silicone to obtain the modified polyamide. Modified polyamide is a polymer with a hyperbranched structure. After the hyperbranched structure is introduced into the curing system, the intramolecular holes it contains can increase the free volume fraction of the cured product, and the high free volume fraction can easily cause matrix deformation and slow down the expansion of cracks, thereby improving the toughness of the cured product; the terminal carboxyl group contained in the modified polyamide can react with the epoxy resin at the initial stage of the reaction, allowing it to enter the cross-linking network of the resin to avoid phase separation. After entering the cross-linking network, the modified polyamide also plays the role of a hyperbranched cross-linking point, thereby inducing stress dissipation and redistribution, inducing collective plastic deformation, and further improving the toughness of the matrix; in addition, the introduction of silane coupling agent also increases the cross-linking density of the matrix, thereby improving the toughness of the matrix.

[0028] When preparing SiC / Mg(OH)2 nanomaterials, first, silicon carbide nanosheets are etched in molten potassium hydroxide to introduce a large number of hydroxyl groups onto their surfaces to obtain pre-treated silicon carbide; secondly, the hydroxyl groups on the surface of the pre-treated silicon carbide are reacted with the amino groups in melamine to synthesize grafted modified silicon carbide; thirdly, the surface of nano-magnesium hydroxide is modified by a silane coupling agent to synthesize modified magnesium hydroxide containing terminal epoxy groups; finally, the free amino groups on the surface of the grafted modified silicon carbide are reacted with the amino groups on the surface of the modified magnesium hydroxide to synthesize SiC / Mg(OH)2 nanomaterials. The nanomaterial uses silicon carbide nanosheets and nano magnesium hydroxide with excellent thermal conductivity and insulation as thermal conductive and insulating fillers, and utilizes the reaction of melamine grafted on the surface of silicon carbide and the epoxy group on the surface of magnesium hydroxide to combine the two to form a composite filler. This mechanism enhances the compatibility of the two fillers in the matrix. The good compatibility of nanomaterials and epoxy resins makes the gaps at the interface between the two very small, effectively reduces the interfacial thermal resistance between the filler and the resin, efficiently constructs a thermal conduction path, and improves the thermal conductivity of the matrix. The addition of nanomaterials also increases the volume resistivity of the matrix, which is because the addition of wide energy bandgap silicon carbide hinders the migration of carriers in the matrix, and the introduction of magnesium hydroxide and melamine further improves the insulation performance of the matrix. In addition, the use of melamine introduces a triazine structure into the matrix, and the triazine structure and magnesium hydroxide work synergistically to improve the flame retardant properties of the matrix. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] 1) The modified polyamide is prepared by the following steps:

[0032] Step A1, add 1.35g of ethylenediamine and 5.4g of methanol into a flask and stir to mix evenly, slowly add 18.3g of methyl acrylate using a constant pressure dropping funnel, and then stir evenly in an ice water bath and nitrogen conditions, and complete the dropwise addition within 2h, then increase the system temperature to 30°C to react for 18h, and after the reaction is completed, perform reduced pressure distillation to obtain a polyamide precursor;

[0033] Step A2, 1.5 g of polyamide precursor and 7 g of methanol were added into a flask and stirred evenly, 4.5 g of 3,3'-diaminodipropylamine was slowly added dropwise in an ice-water bath and nitrogen atmosphere, and the reaction was continued at room temperature for 24 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain a hyperbranched polyamide;

[0034] Step A3, add 1 g of hyperbranched polyamide to a flask containing 50 mL of N,N-dimethylformamide, slowly add 2.5 g of glutaric acid, raise the system temperature to 50° C., continue the reaction for 8 hours, after the reaction is completed, lower the system temperature to 30° C., add 0.5 mL of γ-methacryloxypropyltrimethoxysilane, stir and react for 4 hours, after the reaction is completed, distill under reduced pressure, wash, filter and dry to obtain modified polyamide;

[0035] 2) SiC / Mg(OH)2 nanomaterials are prepared by the following steps:

[0036] Step B1, adding silicon carbide nanosheets to a 5 mol / L potassium hydroxide solution, stirring and mixing, and soaking for 8 hours, and then centrifuging, washing, and drying at 40° C. for 12 hours to obtain pre-treated silicon carbide, wherein the mass ratio of silicon carbide nanosheets to potassium hydroxide solution is 1:20;

[0037] Step B2, dispersing 2 g of pre-treated silicon carbide in 50 mL of deionized water, ultrasonically treating for 2 h, adding 5 g of melamine and 5 g of dicyclohexylcarbodiimide, and raising the system temperature to 100 ° C., keeping the temperature for 5 h, after the reaction is completed, washing, filtering, and drying to obtain grafted modified silicon carbide;

[0038] Step B3, 120 mL of ethanol and 3 mL of γ-glycidyloxypropyltrimethoxysilane were mixed and stirred at 60° C. for 30 min, then the system temperature was increased to 80° C., 8 g of nano magnesium hydroxide and 10 mL of deionized water were added, and the reaction was stirred for 3 h. After the reaction was completed, the mixture was centrifuged, washed, and dried to obtain modified magnesium hydroxide;

[0039] Step B4, disperse the grafted modified silicon carbide and modified magnesium hydroxide in ethanol, stir for 10 minutes, then increase the system temperature to 85°C, and stir the reaction at a speed of 1000 rpm for 12 hours. After the reaction is completed, cool to room temperature, collect the solid, wash, filter, and dry to obtain SiC / Mg(OH)2 nanomaterials. The mass ratio of grafted modified silicon carbide, modified magnesium hydroxide and ethanol is 1:0.5:10.

[0040] Example 2

[0041] 1) The modified polyamide is prepared by the following steps:

[0042] Step A1, add 2.7g of ethylenediamine and 10.8g of methanol into a flask and stir to mix evenly, slowly add 36.6g of methyl acrylate using a constant pressure dropping funnel, and then stir evenly in an ice water bath and nitrogen conditions, and complete the dropwise addition within 2h, then increase the system temperature to 35°C to react for 21h, and after the reaction is completed, perform reduced pressure distillation to obtain a polyamide precursor;

[0043] Step A2, 3 g of polyamide precursor and 14 g of methanol were added into a flask and stirred evenly, 9 g of 3,3'-diaminodipropylamine was slowly added dropwise in an ice-water bath and nitrogen atmosphere, and the reaction was continued at room temperature for 24 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain a hyperbranched polyamide;

[0044] Step A3, adding 1.5 g of hyperbranched polyamide to a flask containing 50 mL of N,N-dimethylformamide, slowly adding 4 g of glutaric acid, raising the system temperature to 55° C., and continuing the reaction for 10 h. After the reaction is completed, lowering the system temperature to 30° C., adding 1 mL of γ-methacryloxypropyltrimethoxysilane, stirring and reacting for 5 h, and after the reaction is completed, distilling under reduced pressure, washing, filtering, and drying to obtain a modified polyamide;

[0045] 2) SiC / Mg(OH)2 nanomaterials are prepared by the following steps:

[0046] Step B1, adding silicon carbide nanosheets to a 5 mol / L potassium hydroxide solution, stirring and mixing, and soaking for 10 hours, and then centrifuging, washing, and drying at 40° C. for 12 hours to obtain pre-treated silicon carbide, wherein the mass ratio of silicon carbide nanosheets to potassium hydroxide solution is 1:20;

[0047] Step B2, disperse 3g of pre-treated silicon carbide in 75mL of deionized water, ultrasonically treat for 2h, add 7.5g of melamine and 7.5g of dicyclohexylcarbodiimide, and raise the system temperature to 110°C, keep the reaction for 6h, and after the reaction is completed, wash, filter and dry to obtain grafted modified silicon carbide;

[0048] Step B3, 120 mL of ethanol and 4 mL of γ-glycidyloxypropyltrimethoxysilane were mixed and stirred at 60 ° C for 30 min, then the system temperature was increased to 85 ° C, 11.5 g of nano magnesium hydroxide and 10 mL of deionized water were added, and the reaction was stirred for 4 h. After the reaction was completed, centrifugation, washing, and drying were performed to obtain modified magnesium hydroxide;

[0049] Step B4, disperse the grafted modified silicon carbide and modified magnesium hydroxide in ethanol, stir for 15 minutes, then increase the system temperature to 90°C, and stir the reaction at a speed of 1100 rpm for 12 hours. After the reaction is completed, cool to room temperature, collect the solid, wash, filter, and dry to obtain SiC / Mg(OH)2 nanomaterials. The mass ratio of grafted modified silicon carbide, modified magnesium hydroxide and ethanol is 1:1:10.

[0050] Example 3

[0051] 1) The modified polyamide is prepared by the following steps:

[0052] Step A1, add 4.05g of ethylenediamine and 16.2g of methanol into a flask and stir to mix evenly, slowly add 54.9g of methyl acrylate using a constant pressure dropping funnel, and then stir evenly in an ice water bath and nitrogen conditions, and complete the dropwise addition within 2h, then increase the system temperature to 40°C to react for 24h, and after the reaction is completed, perform reduced pressure distillation to obtain a polyamide precursor;

[0053] Step A2, adding 4.5 g of polyamide precursor and 21 g of methanol into a flask and stirring evenly, slowly dropping 13.5 g of 3,3'-diaminodipropylamine in an ice-water bath and nitrogen, and continuing the reaction at room temperature for 24 h. After the reaction is completed, vacuum distillation is performed to obtain a hyperbranched polyamide;

[0054] Step A3, adding 2 g of hyperbranched polyamide to a flask containing 50 mL of N,N-dimethylformamide, slowly adding 6 g of glutaric acid, raising the system temperature to 60° C., and continuing the reaction for 12 h. After the reaction is completed, lowering the system temperature to 30° C., adding 1.5 mL of γ-methacryloxypropyltrimethoxysilane, stirring and reacting for 6 h, and after the reaction is completed, distilling under reduced pressure, washing, filtering, and drying to obtain modified polyamide;

[0055] 2) SiC / Mg(OH)2 nanomaterials are prepared by the following steps:

[0056] Step B1, adding silicon carbide nanosheets to a 5 mol / L potassium hydroxide solution, stirring and mixing, and soaking for 12 hours, and then centrifuging, washing, and drying at 40° C. for 12 hours to obtain pre-treated silicon carbide, wherein the mass ratio of the silicon carbide nanosheets to the potassium hydroxide solution is 1:20;

[0057] Step B2, disperse 4 g of pre-treated silicon carbide in 100 mL of deionized water, perform ultrasonic treatment for 2 h, add 10 g of melamine and 10 g of dicyclohexylcarbodiimide, and raise the system temperature to 120° C., keep the reaction for 7 h, and after the reaction is completed, wash, filter, and dry to obtain grafted modified silicon carbide;

[0058] Step B3, 120 mL of ethanol and 5 mL of γ-glycidyloxypropyltrimethoxysilane were mixed and stirred at 60° C. for 30 min, then the system temperature was increased to 90° C., 15 g of nano magnesium hydroxide and 10 mL of deionized water were added, and the reaction was stirred for 5 h. After the reaction was completed, the mixture was centrifuged, washed, and dried to obtain modified magnesium hydroxide;

[0059] Step B4, disperse the grafted modified silicon carbide and modified magnesium hydroxide in ethanol, stir for 20 minutes, then increase the system temperature to 95°C, and stir the reaction at a speed of 1200rpm for 12 hours. After the reaction is completed, cool to room temperature, collect the solid, wash, filter, and dry to obtain SiC / Mg(OH)2 nanomaterials. The mass ratio of grafted modified silicon carbide, modified magnesium hydroxide and ethanol is 1:1.5:10.

[0060] Example 4

[0061] A method for preparing an insulating epoxy resin encapsulation adhesive comprises the following steps:

[0062] 40 parts of bisphenol A epoxy resin, 10 parts of 1,3,4,6-tetrakis(3-mercaptopropyl)glycoluril, 5 parts of modified polyamide prepared in Example 1, 2 parts of 2-methylimidazole, 0.2 parts of methyl alkyl polysiloxane, 10 parts of SiC / Mg(OH)2 nanomaterial prepared in Example 1, and 1 part of 2,6-di-tert-butyl-4-methylphenol;

[0063] The raw materials were weighed in parts by weight, and bisphenol A epoxy resin, the modified polyamide prepared in Example 1, the SiC / Mg(OH)2 nanomaterial prepared in Example 1, methyl alkyl polysiloxane, 2,6-di-tert-butyl-4-methylphenol, 1,3,4,6-tetrakis(3-mercaptopropyl)glycoluril and 2-methylimidazole were added into a reactor, and stirred at a speed of 800 rpm for 1 hour under vacuum conditions to obtain an insulating epoxy resin encapsulation adhesive.

[0064] Example 5

[0065] A method for preparing an insulating epoxy resin encapsulation adhesive comprises the following steps:

[0066] 50 parts of bisphenol A epoxy resin, 15 parts of 1,3,4,6-tetrakis(3-mercaptopropyl)glycoluril, 7 parts of modified polyamide prepared in Example 2, 2.5 parts of 2-methylimidazole, 0.5 parts of methyl alkyl polysiloxane, 12 parts of SiC / Mg(OH)2 nanomaterial prepared in Example 2, and 1.5 parts of 2,6-di-tert-butyl-4-methylphenol;

[0067] The raw materials were weighed in parts by weight, and bisphenol A epoxy resin, the modified polyamide prepared in Example 2, the SiC / Mg(OH)2 nanomaterial prepared in Example 2, methyl alkyl polysiloxane, 2,6-di-tert-butyl-4-methylphenol, 1,3,4,6-tetrakis(3-mercaptopropyl)glycoluril and 2-methylimidazole were added into a reactor, and stirred at a speed of 900 rpm for 1.5 h under vacuum conditions to obtain an insulating epoxy resin encapsulation adhesive.

[0068] Example 6

[0069] A method for preparing an insulating epoxy resin encapsulation adhesive comprises the following steps:

[0070] 60 parts of bisphenol A epoxy resin, 20 parts of 1,3,4,6-tetrakis(3-mercaptopropyl)glycoluril, 10 parts of modified polyamide prepared in Example 3, 3 parts of 2-methylimidazole, 1 part of methyl alkyl polysiloxane, 15 parts of SiC / Mg(OH)2 nanomaterial prepared in Example 3, and 2 parts of 2,6-di-tert-butyl-4-methylphenol;

[0071] The raw materials were weighed in parts by weight, and bisphenol A epoxy resin, the modified polyamide prepared in Example 3, the SiC / Mg(OH)2 nanomaterial prepared in Example 3, methyl alkyl polysiloxane, 2,6-di-tert-butyl-4-methylphenol, 1,3,4,6-tetrakis(3-mercaptopropyl)glycoluril and 2-methylimidazole were added into a reactor, and stirred at a speed of 1000 rpm for 2 hours under vacuum conditions to obtain an insulating epoxy resin encapsulation adhesive.

[0072] Comparative Example 1

[0073] This comparative example is an epoxy resin encapsulation adhesive, which differs from Example 6 in that an equal amount of polyamide (synthesized using sebacic acid and dodecanediamine as raw materials) is used to replace the modified polyamide prepared in Example 3, and the rest are the same.

[0074] Comparative Example 2

[0075] This comparative example is an epoxy resin encapsulation adhesive, which differs from Example 6 in that an equal amount of silicon carbide is used to replace the SiC / Mg(OH)2 nanomaterial, and the rest are the same.

[0076] The encapsulation adhesives prepared in Examples 4-6 and Comparative Examples 1-2 were cured at 100° C. for 2 h to obtain adhesive films, and performance tests were performed on the films:

[0077] Mechanical properties test: Test the tensile strength and elongation at break of the film according to GB / T 528-2009;

[0078] Thermal conductivity test: Test the thermal conductivity of the encapsulant according to ASTM D 5470 standard;

[0079] Volume resistivity test: Test volume resistivity according to GB / T1692-2008;

[0080] Flame retardancy test: Test the flame retardancy level according to UL 94; the test results are shown in the following table:

[0081]

[0082]

[0083] It can be seen from the above table that the epoxy resin encapsulation adhesive prepared by the present invention has excellent mechanical properties, thermal conductivity, insulation and flame retardancy, and can be widely used in electronic packaging technology.

[0084] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.

Claims

1. An insulating epoxy resin encapsulation adhesive, It is characterized in that The following raw materials are included by weight: 40-60 parts of epoxy resin, 10-20 parts of curing agent, 5-10 parts of modified polyamide, 2-3 parts of accelerator, 0.2-1 parts of defoamer, SiC / Mg(OH) 2 10-15 parts of nanomaterials, 1-2 parts of antioxidants; The modified polyamide is prepared by the following steps: Step A1, adding ethylenediamine and methanol into a flask and stirring to mix evenly, slowly adding methyl acrylate dropwise using a constant pressure dropping funnel, and then stirring evenly in an ice water bath and nitrogen conditions, the dropping is completed within 2 hours, and then the system temperature is increased to 30-40°C to react for 18-24 hours, and after the reaction is completed, the polyamide precursor is obtained by vacuum distillation, and the mass ratio of ethylenediamine, methanol and methyl acrylate is 1.35-4.05:5.4-16.2:18.3-54.9; Step A2, adding polyamide precursor and methanol into a flask and stirring evenly, slowly adding 3,3'-diaminodipropylamine dropwise in an ice-water bath and nitrogen, and continuing the reaction at room temperature for 24 hours. After the reaction is completed, distilling under reduced pressure to obtain hyperbranched polyamide, the amount ratio of polyamide precursor, methanol and 3,3'-diaminodipropylamine is 1.5-4.5g:7-21g:4.5-13.5g; Step A3, adding the hyperbranched polyamide to a flask containing N,N-dimethylformamide, slowly adding glutaric acid, raising the system temperature to 50-60°C, continuing the reaction for 8-12 hours, and after the reaction is completed, lowering the system temperature to 30°C, and then adding γ-methacryloxypropyltrimethoxysilane and stirring to react for 4-6 hours. After the reaction is completed, distilling under reduced pressure, washing, filtering, and drying to obtain modified polyamide, the amount ratio of hyperbranched polyamide, N,N-dimethylformamide, glutaric acid and γ-methacryloxypropyltrimethoxysilane is 1-2g:50mL:2.5-6g:0.5-1.5mL; The SiC / Mg(OH) 2 Nanomaterials are prepared by the following steps: Step B1, adding silicon carbide nanosheets to a 5 mol / L potassium hydroxide solution, stirring and mixing, and soaking for 8-12 hours, and then centrifuging, washing, and drying at 40° C. for 12 hours to obtain pre-treated silicon carbide, wherein the mass ratio of silicon carbide nanosheets to potassium hydroxide solution is 1:20; Step B2, dispersing the pretreated silicon carbide in deionized water, ultrasonically treating for 2 hours, adding melamine and dicyclohexylcarbodiimide, and raising the system temperature to 100-120°C, keeping the temperature for reaction for 5-7 hours, after the reaction is completed, washing, filtering and drying to obtain grafted modified silicon carbide, the amount ratio of pretreated silicon carbide, deionized water, melamine and dicyclohexylcarbodiimide is 2-4g: 50-100mL: 5-10g: 5-10g; Step B3, ethanol and γ-glycidyloxypropyltrimethoxysilane are mixed and stirred at 60°C for 30 minutes, then the system temperature is increased to 80-90°C, nano magnesium hydroxide and deionized water are added, and the reaction is stirred for 3-5 hours. After the reaction is completed, centrifugation, washing and drying are performed to obtain modified magnesium hydroxide. The dosage ratio of ethanol, γ-glycidyloxypropyltrimethoxysilane, nano magnesium hydroxide and deionized water is 120mL: 3-5mL: 8-15g: 10mL; Step B4, dispersing the grafted modified silicon carbide and modified magnesium hydroxide in ethanol, stirring for 10-20 minutes, then raising the system temperature to 85-95°C, and stirring at a speed of 1000-1200 rpm for 12 hours. After the reaction is completed, cooling to room temperature, collecting the solid, washing, filtering, and drying, to obtain SiC / Mg(OH) 2 The mass ratio of the nanomaterial, the grafted modified silicon carbide, the modified magnesium hydroxide and the ethanol is 1:0.5-1.5:

10.

2. A method for preparing an insulating epoxy resin encapsulation adhesive according to claim 1, It is characterized in that The following steps are involved: Weigh the raw materials according to weight, epoxy resin, modified polyamide, SiC / Mg(OH) 2 Nanomaterials, defoamers, antioxidants, curing agents and accelerators are added into a reactor, and stirred at a speed of 800-1000 rpm for 1-2 hours under vacuum conditions to obtain insulating epoxy resin encapsulation adhesive.

Citation Information

Patent Citations

  • Threaded locking sealing gum and preparation method thereof

    CN102352209A

  • Melamine flame retardant graft modified carbon nanotube and manufacturing method thereof

    CN103881137A

  • Self-healing supermolecule polyamide adhesive as well as preparation method and application thereof

    CN108865046A

  • Force-induced responsive polymer based on reversible free radical type force-sensitive group

    CN111378158A

  • Epoxy resin-silicon carbide wear-resistant flame-retardant composite material and preparation method thereof

    CN112876815A