A low-resistance NTC thermistor and its preparation method and application
By preparing NTC ceramic substrates with specific compositions and adding compounded fatty alcohol polyoxyethylene ether to ruthenium electrode paste, the high resistivity and stability problems of NTC thermistors were solved, resulting in NTC thermistors with low resistivity and high stability, thus expanding their application range.
Patent Information
- Application Number
- CN202410573915.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-05-09
AI Technical Summary
Existing NTC thermistors have high resistivity and poor stability, which limits their application areas and service life.
NTC ceramic substrates were prepared using a specific ratio of Mn3O4, NiO, Ni2O3, CuO, SiO2, CoO and Al2O3, and a compounded fatty alcohol polyoxyethylene ether was added to the ruthenium electrode paste to form a multilayer thin film to improve stability and reduce resistivity.
This achieves low resistivity and low resistance B value, improving the stability and lifespan of NTC thermistors and expanding their application areas.
Smart Images

Figure BDA0004833294600000111 
Figure BDA0004833294600000121
Abstract
Description
Technical Field
[0001] The invention relates to the field of thermistors, and in particular to a low-resistance NTC thermistor and a preparation method and application thereof. Background Art
[0002] Thermistors are a type of sensitive components, which are divided into PTC (Positive Temperature Coefficient) thermistors and NTC (Negative Temperature Coefficient) thermistors according to their temperature coefficients. The typical feature of thermistors is that they are sensitive to temperature and show different resistance values at different temperatures. The higher the temperature, the greater the resistance of the PTC thermistor, while the higher the temperature, the lower the resistance of the NTC thermistor. They are both semiconductor devices.
[0003] NTC thermistor is a thermistor material with a negative temperature coefficient, whose resistance decreases exponentially as the temperature rises. NTC thermistor has the advantages of high sensitivity, fast response speed, small size, and easy remote control and measurement. It is widely used in household appliances, medical instruments, auto parts, fire warning and other fields.
[0004] At present, although the NTC thermistors on the market have good negative temperature characteristics, their overall stability is still poor, and because of the main raw materials, the resistivity of the thermistor is relatively large. The greater the resistivity of the thermistor, the greater the material characteristic constant B value of the thermistor will be, and the greater the material characteristic constant B value of the thermistor, the greater the resistance value will be at the same temperature.
[0005] Therefore, in order to solve the above problems, the present invention provides a low-resistance NTC thermistor and a preparation method thereof. The NTC thermistor prepared by the present invention not only has excellent low resistivity and low resistance B value, but also has good overall self-stability, can greatly improve the performance and service life of the NTC thermistor, performs well in aging resistance tests, has a very outstanding market prospect, and greatly expands the application field and application environment of the NTC thermistor. Summary of the invention
[0006] In order to solve the above problems, the first aspect of the present invention provides a low-resistance NTC thermistor, which includes an NTC ceramic body, a ruthenium electrode arranged on the surface of the ceramic body, and an outer electrode on the surface of the ruthenium electrode.
[0007] As a preferred technical solution, the raw materials of the NTC ceramic sheet include, by mass, 40 to 45 parts of Mn3O4, 10 to 14 parts of NiO, 6 to 10 parts of Ni2O3, 12 to 18 parts of CuO, 2 to 5 parts of SiO2, 3 to 6 parts of CoO and 1 to 3 parts of Al2O3.
[0008] As a preferred technical solution, the mass ratio of Mn3O4, NiO, Ni2O3, CuO, SiO2, CoO and Al2O3 is (42-44): (11-13): (8-10): (14-16): (3-4): (4-5): (1-2).
[0009] As a preferred technical solution, the mass ratio of Mn3O4, NiO, Ni2O3, CuO, SiO2, CoO and Al2O3 is 43.5:12:10:15:3.5:5:1.
[0010] As a preferred technical solution, the preparation method of the NTC ceramic sheet includes the following steps: S1: Mn3O4, NiO, Ni2O3, CuO, SiO2, CoO and Al2O3 are mixed evenly, and added into a wet ball mill for ball milling to obtain NTC powder; S2: A binder is added to the NTC powder after ball milling, and the mixture is mixed to obtain NTC ceramic particles; S3: The NTC ceramic particles are dry-pressed into sheets and pre-sintered at 700-850°C for 1-4 hours, and then the temperature is raised to 1100-1300°C and sintered for 3-6 hours. After completion, the NTC ceramic sheet is obtained.
[0011] As a preferred technical solution, the adhesive is at least one of polyvinyl alcohol, carboxymethyl cellulose, polyvinyl acetate, and water glass.
[0012] As a preferred technical solution, the adhesive is carboxymethyl cellulose.
[0013] As a preferred technical solution, the amount of the binder added is 2-5% of the total mass of the NTC powder.
[0014] As a preferred technical solution, the average particle size D of the NTC powder is 50 1~4.5μm.
[0015] As a preferred technical solution, the average particle size D of the NTC powder is 50 1~2.5μm.
[0016] As a preferred technical solution, the raw materials of the ruthenium electrode include, by weight: 25 to 35 parts of ruthenium dioxide, 15 to 20 parts of glass powder, 15 to 25 parts of mixed metal powder, 1 to 10 parts of additives, and 30 to 40 parts of solvent.
[0017] As a preferred technical solution, the mass ratio of ruthenium dioxide, glass powder, mixed metal powder and additive is (26-30): (16-20): (15-20): (2-8).
[0018] As a preferred technical solution, the mass ratio of ruthenium dioxide, glass powder, mixed metal powder and additive is (26-28): (16-18): (15-16): (3-6).
[0019] As a preferred technical solution, the mass ratio of ruthenium dioxide, glass powder, mixed metal powder and additive is 27:18:15:5.
[0020] As a preferred technical solution, the raw materials of the glass powder, calculated by mass, include: 50 to 60 parts of Bi2O3, 10 to 15 parts of SiO2, 20 to 30 parts of CuO, 5 to 10 parts of CaO, and 1 to 5 parts of B2O3.
[0021] As a preferred technical solution, the mass ratio of Bi2O3, SiO2, CuO, CaO and B2O3 is (52-55): (12-14): (22-26): (6-8): (3-4).
[0022] As a preferred technical solution, the preparation method of the glass powder includes the following steps: S1: heating to 700-800°C and adding raw materials required for glass powder for smelting to obtain a glass solution; S2: rapidly cooling the glass solution to obtain glass particles, ball-milling and drying the glass particles and passing them through a 200-400 mesh sieve to obtain glass powder.
[0023] As a preferred technical solution, the mixed metal powder is an alloy metal powder of silver and palladium.
[0024] As a preferred technical solution, the mass ratio of silver to palladium in the silver and palladium alloy metal powder is (4-5):1.
[0025] As a preferred technical solution, the auxiliary agent is fatty alcohol polyoxyethylene ether.
[0026] As a preferred technical solution, the fatty alcohol polyoxyethylene ether is a composition of isomeric C13 fatty alcohol polyoxyethylene ether and cetearyl alcohol polyoxyethylene ether.
[0027] As a preferred technical solution, the mass ratio of the isomeric C13 fatty alcohol polyoxyethylene ether to the cetearyl alcohol polyoxyethylene ether is (1-3):(5-6).
[0028] As a preferred technical solution, the hydroxyl value of the isomeric C13 fatty alcohol polyoxyethylene ether is 150-200 mgKOH / g.
[0029] As a preferred technical solution, the hydroxyl value of the cetearyl alcohol polyoxyethylene ether is 30 to 100 mgKOH / g.
[0030] In the present invention, by using the above-mentioned compounded fatty alcohol polyoxyethylene ether in the slurry of the ruthenium electrode, the stability of the NTC thermistor can be stably improved, and the resistivity and B value of the NTC thermistor can be helped to be reduced. The above-mentioned compound fatty alcohol polyoxyethylene ether can effectively form a micro multilayer structure film on the surface of the ruthenium dioxide powder during the mixing process of the slurry. The presence of the film can greatly reduce the surface group connection phenomenon between the ruthenium dioxide powders, thereby greatly reducing its spontaneous aggregation, so that the slurry has very excellent uniformity; and in the printing process, the presence of the multilayer structure film can better combine the powder with the glass powder, thereby strengthening the bonding strength of the ruthenium dioxide powder on the surface of the NTC ceramic body, thereby greatly improving the stability of the overall resistance and reducing the resistivity and B value.
[0031] As a preferred technical solution, the solvent is any one of diethylene glycol butyl ether, benzyl alcohol, acetone, methanol, and dibutyl phthalate.
[0032] As a preferred technical solution, the solvent is diethylene glycol butyl ether.
[0033] As a preferred technical solution, the method for preparing the ruthenium electrode slurry includes the following steps: mixing the raw materials required for the ruthenium electrode, stirring the mixture at a speed of 200 to 300 r / min, and after stirring, ultrasonically treating the mixture at a power of 500 to 800 w for 2 to 3 hours to obtain the ruthenium electrode slurry.
[0034] As a preferred technical solution, the outer electrode is a silver electrode.
[0035] The second aspect of the present invention provides a method for preparing the above-mentioned low-resistance NTC thermistor, and the preparation method comprises the following steps: S1: flattening the prepared NTC ceramic sheet, and then printing the ruthenium electrode slurry on both sides of the NTC ceramic sheet, sintering at high temperature, and the thickness of the ruthenium electrode after sintering is 4 to 6 μm; S2: printing the silver electrode slurry on the surface of the ruthenium electrode, sintering at high temperature, and the thickness of the ruthenium electrode after sintering is 4 to 6 μm, and the preparation method is completed.
[0036] As a preferred solution, the high temperature sintering temperature in S1 is 900-1200°C.
[0037] As a preferred solution, the high temperature sintering temperature in S2 is 700-900°C.
[0038] A third aspect of the present invention provides an application of the low-resistance NTC thermistor, including application of the low-resistance NTC thermistor in household appliances, auto parts, medical instruments, and disaster warning.
[0039] The present invention has the beneficial effects:
[0040] 1. The low-resistance NTC thermistor provided in the present invention not only has excellent low resistivity and low resistance B value, but also has good overall stability, which can greatly improve the performance and service life of the NTC thermistor, and performs well in the aging resistance test. It has a very outstanding market prospect and greatly expands the application field and application environment of the NTC thermistor.
[0041] 2. A low-resistance NTC thermistor provided in the present invention can stably improve the stability of the NTC thermistor and help reduce the resistivity and B value of the NTC thermistor by adding fatty alcohol polyoxyethylene ether with specific hydroxyl value selection and compounding ratio to ruthenium electrode slurry; the composite fatty alcohol polyoxyethylene ether can effectively form a micro multilayer structure film on the surface of ruthenium dioxide powder during the mixing process of the slurry, and the presence of the film can greatly reduce the surface group connection phenomenon between ruthenium dioxide powders, thereby greatly reducing its spontaneous aggregation, so that the slurry has very excellent uniformity; and during the printing process, the presence of the multilayer structure film can better combine the powder with the glass powder, thereby strengthening the bonding strength of the ruthenium dioxide powder on the surface of the NTC ceramic sheet.
[0042] 3. The low-resistance NTC thermistor provided in the present invention has a simple preparation method, simple equipment operation, and easy-to-obtain raw materials. It can effectively reduce the raw material cost of existing NTC resistors and does not involve complex chemical reactions. In the later large-scale production, it can effectively reduce equipment maintenance and labor costs, and has a very excellent market prospect. DETAILED DESCRIPTION
[0043] The technical solutions in the above invention contents of the present invention will be further described and demonstrated in the form of specific implementation schemes below. The following embodiments are only practical examples used to illustrate and explain the contents of the technical solutions in the specification and should not limit the scope of the claims to be protected by the present invention. All technical products based on the technical solutions described in the invention contents of the present invention should be included in the scope to be protected by the present invention.
[0044] In the following examples, unless otherwise specified, the raw materials are all commercially available products, or can be prepared by methods well known to those skilled in the art.
[0045] Example 1
[0046] Embodiment 1 A first aspect provides a low-resistance NTC thermistor, which includes an NTC ceramic body, a ruthenium electrode disposed on the surface of the ceramic body, and an outer electrode on the surface of the ruthenium electrode.
[0047] The raw materials of the NTC ceramic sheet include, by mass, 43.5 parts of Mn3O4, 12 parts of NiO, 10 parts of Ni2O3, 15 parts of CuO, 3.5 parts of SiO2, 5 parts of CoO and 1 part of Al2O3.
[0048] The preparation method of the NTC ceramic sheet includes the following steps: S1: Mn3O4, NiO, Ni2O3, CuO, SiO2, CoO and Al2O3 are mixed evenly, and added into a wet ball mill for ball milling to obtain NTC powder; S2: A binder is added to the NTC powder after ball milling, and the mixture is mixed to obtain NTC ceramic particles; S3: The NTC ceramic particles are dry-pressed into sheets, and then pre-sintered at 800°C for 2 hours, and then the temperature is raised to 1250°C and sintered for 4 hours. After completion, the NTC ceramic sheet is obtained.
[0049] The binder is carboxymethyl cellulose; the added amount of the binder is 4% of the total mass of the NTC powder.
[0050] The average particle size of NTC powder is D 50 is 2μm.
[0051] The raw materials of the ruthenium electrode include, by weight: 27 parts of ruthenium dioxide, 18 parts of glass powder, 15 parts of mixed metal powder, 5 parts of additives, and 40 parts of solvent.
[0052] The raw materials of the glass powder, calculated by mass, include: 54 parts of Bi2O3, 13 parts of SiO2, 24 parts of CuO, 6 parts of CaO, and 3 parts of B2O3.
[0053] The preparation method of glass powder comprises the following steps: S1: heating to 750°C and adding raw materials required for glass powder for smelting to obtain glass solution; S2: rapidly cooling the glass solution to obtain glass particles, ball-milling and drying the glass particles and passing through a 325-mesh sieve to obtain glass powder.
[0054] The mixed metal powder is an alloy metal powder of silver and palladium; the mass ratio of silver to palladium in the alloy metal powder of silver and palladium is 4:1.
[0055] The auxiliary agent is a composition of isomeric C13 fatty alcohol polyoxyethylene ether and cetearyl alcohol polyoxyethylene ether, and the mass ratio of the two is 2:5.5. Isomeric C13 fatty alcohol polyoxyethylene ether is purchased from Haian Guoyun Chemical Co., Ltd. E-1302, with a hydroxyl value of 195 mgKOH / g; cetearyl alcohol polyoxyethylene ether is purchased from Haian Guoyun Chemical Co., Ltd. O-9, with a hydroxyl value of 86 mgKOH / g.
[0056] The solvent is diethylene glycol butyl ether.
[0057] The method for preparing the ruthenium electrode slurry includes the following steps: mixing the raw materials required for the ruthenium electrode, stirring the mixture at a speed of 220r / min, and ultrasonically treating the mixture at a power of 600w for 2h after the stirring is completed, so as to obtain the ruthenium electrode slurry.
[0058] The outer electrode is a silver electrode, and the silver electrode slurry is purchased from the silver electrode slurry product for resistor electrodes sold by Dongguan Beiteli New Materials Co., Ltd.
[0059] The second aspect of this embodiment provides a method for preparing the above-mentioned low-resistance NTC thermistor, and the preparation method includes the following steps: S1: flattening the prepared NTC ceramic sheet, and then printing the ruthenium electrode slurry on both sides of the NTC ceramic sheet, sintering at high temperature, and the thickness of the ruthenium electrode after sintering is 4.5μm; S2: printing the silver electrode slurry on the surface of the ruthenium electrode, sintering at high temperature, and the thickness of the ruthenium electrode after sintering is 4μm, and the result is obtained after completion.
[0060] Example 2
[0061] Embodiment 2 A first aspect provides a low-resistance NTC thermistor, which includes an NTC ceramic body, a ruthenium electrode disposed on the surface of the ceramic body, and an outer electrode on the surface of the ruthenium electrode.
[0062] The raw materials of the NTC ceramic sheet body include, by mass, 42 parts of Mn3O4, 11 parts of NiO, 8 parts of Ni2O3, 16 parts of CuO, 4 parts of SiO2, 4 parts of CoO and 2 parts of Al2O3.
[0063] The preparation method of the NTC ceramic sheet includes the following steps: S1: Mn3O4, NiO, Ni2O3, CuO, SiO2, CoO and Al2O3 are mixed evenly, and added into a wet ball mill for ball milling to obtain NTC powder; S2: A binder is added to the NTC powder after ball milling, and the mixture is mixed to obtain NTC ceramic particles; S3: The NTC ceramic particles are dry-pressed into sheets, and then pre-sintered at 800°C for 2h, and then the temperature is raised to 1250°C and sintered for 4h. After completion, the NTC ceramic sheet is obtained.
[0064] The binder is carboxymethyl cellulose; the added amount of the binder is 4% of the total mass of the NTC powder.
[0065] Average particle size D of NTC powder after wet ball milling 50 is 2μm.
[0066] The raw materials of the ruthenium electrode include, by weight: 27 parts of ruthenium dioxide, 18 parts of glass powder, 15 parts of mixed metal powder, 5 parts of auxiliary agent, and 40 parts of solvent.
[0067] The raw materials of the glass powder, calculated by mass, include: 54 parts of Bi2O3, 13 parts of SiO2, 24 parts of CuO, 6 parts of CaO, and 3 parts of B2O3.
[0068] The preparation method of glass powder comprises the following steps: S1: heating to 750°C and adding raw materials required for glass powder for smelting to obtain glass solution; S2: rapidly cooling the glass solution to obtain glass particles, ball-milling and drying the glass particles and passing through a 325-mesh sieve to obtain glass powder.
[0069] The mixed metal powder is an alloy metal powder of silver and palladium; the mass ratio of silver to palladium in the alloy metal powder of silver and palladium is 4:1.
[0070] The auxiliary agent is a composition of isomeric C13 fatty alcohol polyoxyethylene ether and cetearyl alcohol polyoxyethylene ether, and the mass ratio of the two is 2:5.5. Isomeric C13 fatty alcohol polyoxyethylene ether is purchased from Haian Guoyun Chemical Co., Ltd. E-1302, with a hydroxyl value of 195 mgKOH / g; cetearyl alcohol polyoxyethylene ether is purchased from Haian Guoyun Chemical Co., Ltd. O-9, with a hydroxyl value of 86 mgKOH / g.
[0071] The solvent is diethylene glycol butyl ether.
[0072] The method for preparing the ruthenium electrode slurry includes the following steps: mixing the raw materials required for the ruthenium electrode, stirring the mixture at a speed of 220r / min, and ultrasonically treating the mixture at a power of 600w for 2h after the stirring is completed, so as to obtain the ruthenium electrode slurry.
[0073] The outer electrode is a silver electrode, and the silver electrode slurry is purchased from the silver electrode slurry product for resistor electrodes sold by Dongguan Beiteli New Materials Co., Ltd.
[0074] The second aspect of this embodiment provides a method for preparing the above-mentioned low-resistance NTC thermistor, and the preparation method includes the following steps: S1: flattening the prepared NTC ceramic sheet, and then printing the ruthenium electrode slurry on both sides of the NTC ceramic sheet, sintering at high temperature, and the thickness of the ruthenium electrode after sintering is 4.5μm; S2: printing the silver electrode slurry on the surface of the ruthenium electrode, sintering at high temperature, and the thickness of the ruthenium electrode after sintering is 4μm, and the result is obtained after completion.
[0075] Comparative Example 1
[0076] The specific implementation of this comparative example is basically the same as that of Example 1, except that the raw materials of the NTC ceramic sheet, by mass, include: 35 parts of Mn3O4, 20 parts of NiO, 3 parts of Ni2O3, 25 parts of CuO, 1 part of SiO2, 1 part of CoO and 5 parts of Al2O3.
[0077] Comparative Example 2
[0078] The specific implementation of this comparative example is basically the same as that of Example 1, except that the average particle size D of the NTC powder after wet ball milling is 50 It is 5.5μm.
[0079] Comparative Example 3
[0080] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the raw materials of the ruthenium electrode, in parts by mass, include: 40 parts of ruthenium dioxide, 10 parts of glass powder, 20 parts of mixed metal powder, 3 parts of additives, and 40 parts of solvent.
[0081] Comparative Example 4
[0082] The specific implementation of this comparative example is basically the same as that of Example 1, except that the mass ratio of isomeric C13 fatty alcohol polyoxyethylene ether to cetearyl alcohol polyoxyethylene ether is 1:1.
[0083] Comparative Example 5
[0084] The specific implementation of this comparative example is basically the same as that of Example 1, except that: Cetearyl alcohol polyoxyethylene ether was purchased from Hai'an Guoyun Chemical Co., Ltd. O-3, and the hydroxyl value was 145 mgKOH / g.
[0085] Performance Evaluation
[0086] 1. Resistivity and B value: The NTC thermistors prepared in the examples and comparative examples were placed in a 25°C thermostat for resistance testing. After measuring their resistance at 25°C, they were placed in a 90°C thermostat for high temperature resistance testing again. The resistivity and B value of the NTC thermistor were calculated from the two resistance values. The average value of 10 tests was recorded in Table 1.
[0087] 2. Stability: The NTC thermistors prepared in the examples and comparative examples were aged in air at 125°C for 1000 hours, and their resistivity was tested again using the method of performance evaluation 1. The rate of increase of their resistivity relative to the corresponding resistivity in performance evaluation 1 was calculated, and the average value of the measured results of 10 tests was recorded in Table 1.
[0088] Table 1 Performance evaluation
[0089]
[0090]
[0091] It can be seen from the embodiments of the present invention, the comparative examples and the data results in Table 1 that embodiments 1 and 2 can achieve excellent results in resistivity, B value and aging resistance / stability by adopting the necessary technical solutions defined in the present invention. This is mainly because the specific ceramic sheet body and ruthenium electrode raw material solutions in the present invention enhance the bonding strength between the electrode raw material and the ceramic sheet body and its own dispersion uniformity; while comparative examples 1 to 5 do not adopt the necessary technical solutions, resulting in their corresponding performance tests being significantly worse than embodiments 1 to 3, which further proves the importance of the technical solutions defined in the present invention to its technical effects.
Claims
1. A low-resistance NTC thermistor, characterized in that: The low-resistance NTC thermistor comprises an NTC ceramic body, a ruthenium electrode arranged on the surface of the ceramic body, and an outer electrode on the surface of the ruthenium electrode; The raw materials of the NTC ceramic sheet body include, by mass, 42-44 parts of Mn3O4, 11-13 parts of NiO, 8-10 parts of Ni2O3, 14-16 parts of CuO, 3-4 parts of SiO2, 4-5 parts of CoO and 1-2 parts of Al2O3; The preparation method of the NTC ceramic sheet comprises the following steps: S1: Mn3O4, NiO, Ni2O3, CuO, SiO2, CoO and Al2O3 are mixed evenly, and added into a wet ball mill for ball milling to obtain NTC powder; S2: a binder is added to the NTC powder after ball milling, and the mixture is mixed to obtain NTC ceramic particles; S3: the NTC ceramic particles are dry-pressed into sheets, and then pre-sintered at 700-850°C for 1-4 hours, and then the temperature is raised to 1100-1300°C and sintered for 3-6 hours, and the NTC ceramic sheet is obtained after the pre-sintering is completed; The binder is at least one of polyvinyl alcohol, carboxymethyl cellulose, polyvinyl acetate, and water glass; The amount of the binder added is 2-5% of the total mass of the NTC powder; The average particle size D of the NTC powder 50 1~4.5μm; The ruthenium electrode comprises, by weight, 25 to 35 parts of ruthenium dioxide, 15 to 20 parts of glass powder, 15 to 25 parts of mixed metal powder, 1 to 10 parts of auxiliary agent, and 30 to 40 parts of solvent; The auxiliary agent is fatty alcohol polyoxyethylene ether; the fatty alcohol polyoxyethylene ether is a composition of isomeric C13 fatty alcohol polyoxyethylene ether and cetearyl alcohol polyoxyethylene ether; the mass ratio of the isomeric C13 fatty alcohol polyoxyethylene ether and cetearyl alcohol polyoxyethylene ether is (1-3): (5-6).
2. The low-resistance NTC thermistor according to claim 1, characterized in that: The mass ratio of the ruthenium dioxide, the glass powder, the mixed metal powder and the additive is (26-30): (16-20): (15-20): (2-8).
3. The low-resistance NTC thermistor according to claim 2, characterized in that: The raw materials of the glass powder include, by mass, 50-60 parts of Bi2O3, 10-15 parts of SiO2, 20-30 parts of CuO, 5-10 parts of CaO, and 1-5 parts of B2O3.
4. The low-resistance NTC thermistor according to claim 3, characterized in that: The mass ratio of Bi2O3, SiO2, CuO, CaO and B2O3 is (52~55):(12~14):(22~26):(6~8):(3~4).
5. The low-resistance NTC thermistor according to claim 4, characterized in that: Preparation method of the glass powder The following steps are involved: S1: heating to 700-800°C and adding raw materials required for glass powder for smelting to obtain glass solution; S2: Rapidly cool the glass solution to obtain glass particles, ball-mill and dry the glass particles, and sieve through a 200-400 mesh sieve to obtain glass powder.
6. The low-resistance NTC thermistor according to claim 5, characterized in that: The mixed metal powder is an alloy metal powder of silver and palladium; the mass ratio of silver to palladium in the alloy metal powder of silver and palladium is (4-5):
1.
7. A method for preparing a low-resistance NTC thermistor according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: Flatten the prepared NTC ceramic sheet, then print the ruthenium electrode slurry on both sides of the NTC ceramic sheet, and sinter at high temperature. The thickness of the ruthenium electrode after sintering is 4~6μm; S2: Print the silver electrode slurry on the surface of the ruthenium electrode and sinter it at high temperature. The thickness of the ruthenium electrode after sintering is 4~6μm.
8. Application of the low-resistance NTC thermistor according to any one of claims 1 to 6 in household appliances, auto parts, medical instruments, and disaster warning.