A recyclable polyvinyl alcohol resin packaging material and preparation method thereof
By adding materials such as graphene oxide, amino-terminated polyamide-amine and sodium alginate to the polyvinyl alcohol film, and compounding it with bio-based polyester, combined with microwave curing technology, a packaging material with high barrier properties and high mechanical strength is formed. , solves the hydrophilicity problem of polyvinyl alcohol film, is suitable for food and industrial packaging, and realizes environmentally friendly recycling of materials.
Patent Information
- Application Number
- CN202410481274.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-04-22
AI Technical Summary
Due to its strong hydrophilicity and water solubility, existing polyvinyl alcohol films lack waterproofness, which limits their application in food packaging and other fields.
A packaging material including a polyvinyl alcohol sheet body and a polyester layer coated on its surface is used, and graphene oxide, amino-terminated polyamide-amine, sodium alginate and nanofillers are added to the polyvinyl alcohol. It is compounded with materials such as bio-based polyester and thermosetting carboxyl-terminated polyester resin to form a network structure and micro-nano filler attachment, and combined with microwave curing technology to enhance its barrier properties.
It has achieved packaging materials with high barrier properties and high mechanical strength, with good water and oxygen barrier effects. It is suitable for food and industrial packaging, and the material is recyclable and environmentally friendly.
Smart Images

Figure CN118325162B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of packaging materials, and in particular to a recyclable polyvinyl alcohol resin packaging material and a preparation method thereof. Background Art
[0002] Polyvinyl alcohol is a water-soluble polymer obtained by alkali-catalyzed alcoholysis of polyvinyl acetate. As a polyhydroxyl strong polar water-soluble polymer, it has excellent comprehensive properties. For example, its mechanical properties and heat resistance are better than those of polyolefins and are comparable to those of engineering plastics. It is widely used in food packaging, industrial product packaging, daily chemical product packaging and other industries.
[0003] As people's quality of life continues to improve, they pay more and more attention to the living environment. Polyvinyl alcohol, as a biodegradable material, is a non-toxic, non-corrosive, environmentally friendly organic polymer with good recyclability and broad application prospects.
[0004] However, the hydroxyl groups in the polyvinyl alcohol molecular chain are prone to form a large number of hydrogen bonds between and within the molecules. Although the strong polarity of polyvinyl alcohol can give it good compatibility with inorganic fillers, in the actual production process, when the inorganic filler content is high, it is difficult to achieve good dispersion in the matrix. At the same time, due to the multi-hydroxyl and strong hydrogen bond structure characteristics of polyvinyl alcohol, it has strong hydrophilicity and water solubility after film formation. Therefore, the existing polyvinyl alcohol film lacks waterproofness, which limits its application in food packaging. Summary of the invention
[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a recyclable polyvinyl alcohol resin packaging material and a preparation method thereof.
[0006] A recyclable polyvinyl alcohol resin packaging material comprises: a polyvinyl alcohol sheet blank, and a polyester layer coated on one side of the polyvinyl alcohol sheet blank; the raw materials of the polyvinyl alcohol sheet blank comprise: 50-150 parts of polyvinyl alcohol, 10-50 parts of filler, 2-6 parts of graphene oxide, 1-2 parts of amino-terminated polyamide-amine, 1-2 parts of sodium alginate, 0.01-0.1 parts of N-hydroxysuccinimide, and 1-2 parts of calcium chloride; the raw materials of the polyester layer comprise: 10-20 parts of bio-based polyester, 5-15 parts of thermosetting carboxyl-terminated polyester resin, 1-5 parts of polyacrylic acid, 2-10 parts of nano silicon carbide powder, and 0.1-1 part of hydroxyalkylamide.
[0007] Preferably, the polyvinyl alcohol is Nichigo G-Polymer TM .
[0008] NichigoG-Polymer TMIt is a biodegradable vinyl alcohol-based resin with excellent water solubility, gas barrier properties and melt formability. It is used as a barrier material and can be dissolved in water and coated on a film. It is well utilized in barrier packaging materials for dry foods and biodegradable barrier packaging materials in combination with biodegradable resins such as biopolyester.
[0009] Preferably, the bio-based polyester is at least one of polylactic acid, polyhydroxyalkanoate, and polybutylene succinate.
[0010] Preferably, the filler is at least one of nano bentonite, nano calcium carbonate and nano white carbon black.
[0011] The method for preparing the above-mentioned recyclable polyvinyl alcohol resin packaging material comprises the following steps:
[0012] S1, adding graphene oxide to water and ultrasonically dispersing for 5-15 minutes, adding amino-terminated polyamide-amine and sodium alginate thereto and continuing ultrasonication for 1-5 minutes, adding N-hydroxysuccinimide and stirring for 1-5 minutes to obtain preform a;
[0013] S2, adding calcium chloride into deionized water and stirring evenly to obtain a premixed solution b;
[0014] S3, adding polyvinyl alcohol to deionized water, stirring at 60-70° C. for 10-30 min to obtain pre-dispersed polyvinyl alcohol; adding premixed liquid a, premixed liquid b, and filler to the pre-dispersed polyvinyl alcohol in sequence under stirring, stirring at 70-80° C. for 10-40 min, rolling into a sheet, and drying to obtain a sheet blank;
[0015] S4. Add bio-based polyester, thermosetting end-carboxyl polyester resin, polyacrylic acid, nano-silicon carbide powder and hydroxyalkylamide into the organic solution and mix evenly to obtain a premixed liquid c; spray the premixed liquid c onto one surface of the sheet blank under high pressure, air-dry naturally to constant weight, cure by microwave heating for 1-5 hours, and cool to room temperature.
[0016] Preferably, in S1, the ultrasonic dispersion frequency is 10-20 kHz.
[0017] Preferably, in S1, after adding N-hydroxysuccinimide, stirring is performed at a speed of 100-500 r / min for 1-5 min.
[0018] Preferably, in S3, the drying temperature is 50-70°C and the drying time is 10-20h.
[0019] Preferably, in S4, the organic solution is at least one of ethyl acetate, dimethylformamide and dimethylacetamide.
[0020] Preferably, in S4, the microwave power is 320-360W.
[0021] Beneficial effects:
[0022] The packaging material obtained by the present invention is an environmentally friendly material, has biodegradability, is easy to recycle and reuse, and the raw materials used have the advantages of being non-toxic and environmentally friendly and having good degradability. At the same time, the packaging material has high barrier properties, excellent water and oxygen barrier effects, high mechanical strength, is suitable for mass industrial production, and can meet the requirements of industries such as food packaging.
[0023] The present invention grafts the dendritic polyamide-amine onto the graphene oxide sheet structure, and then compounded with sodium alginate and combined in polyvinyl alcohol to form a network structure similar to a reinforcing rib structure, which has excellent water-barrier and oxygen-barrier properties; at the same time, the polyamide-amine surface has a large number of active amino groups, which can form hydrogen bonds with sodium alginate, significantly enhancing the good dispersion of fillers in the system, and after curing, not only significantly enhancing the crosslinking density of the blank, enhancing the mechanical strength, but also further enhancing its barrier properties.
[0024] The bio-based polyester is compounded with thermosetting carboxyl-terminated polyester resin and polyacrylic acid, and the hydroxyalkylamide can promote the uniform deposition and attachment of nano-silicon carbide powder to one side of the sheet blank. With microwave curing, the polyacrylic acid and the polyvinyl alcohol sheet blank are cross-linked and bonded, and the bonding strength is extremely high. After testing, one side of the packaging material can continue to maintain its hydrophilic properties, while the other side has excellent hydrophobic effect, and the hydrophobic contact angle can reach more than 150°, which can be widely used in the field of waterproof packaging materials.
[0025] The preparation process of the invention is simple, the raw materials are easy to control, the repeatability is good, the output is high, and it is easy to realize industrial production; the packaging material has excellent comprehensive performance and excellent mechanical properties, has potential application value in the fields of food packaging, industrial product packaging, daily chemical product packaging, etc., and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a comparison chart of the tensile strength and elongation at break of the packaging materials obtained in Example 5 and Comparative Examples 1-2.
[0027] Figure 2 This is a comparison chart of the static water contact angle values of the polyester layer of the packaging material obtained in Example 5 and Comparative Examples 1-2 before and after abrasion.
[0028] Figure 3 It is a comparison chart of the barrier properties of the packaging materials obtained in Example 5 and Comparative Examples 1-2. DETAILED DESCRIPTION
[0029] The present invention will be further explained below in conjunction with specific embodiments.
[0030] Example 1
[0031] A recyclable polyvinyl alcohol resin packaging material comprises a polyvinyl alcohol sheet blank and a polyester layer coated on one side of the polyvinyl alcohol sheet blank.
[0032] The raw materials of the polyvinyl alcohol sheet blank include: 50kg of polyvinyl alcohol, 5kg of nano-bentonite, 5kg of nano-calcium carbonate, 2kg of graphene oxide, 1kg of amino-terminated polyamide-amine, 1kg of sodium alginate, 0.01kg of N-hydroxysuccinimide and 1kg of calcium chloride.
[0033] The raw materials of the polyester layer include: 8kg of polylactic acid, 2kg of polyhydroxyalkanoate, 5kg of thermosetting carboxyl-terminated polyester resin, 1kg of polyacrylic acid, 2kg of nano silicon carbide powder, and 0.1kg of hydroxyalkylamide.
[0034] The method for preparing the above-mentioned recyclable polyvinyl alcohol resin packaging material comprises the following steps:
[0035] S1. Add graphene oxide to 20 kg of water, and ultrasonically disperse for 5 min at a frequency of 10 kHz. Add amino-terminated polyamide-amine and sodium alginate and continue ultrasonicating for 1 min. Add N-hydroxysuccinimide and stir at a speed of 100 r / min for 1 min to obtain preform a.
[0036] S2, adding calcium chloride to 20 kg of deionized water and stirring evenly to obtain a premixed solution b;
[0037] S3, adding polyvinyl alcohol to 200 kg of deionized water, stirring at a temperature of 60° C. for 10 min to obtain pre-dispersed polyvinyl alcohol; adding premixed liquid a, premixed liquid b, nano-bentonite, and nano-calcium carbonate to the pre-dispersed polyvinyl alcohol in sequence under stirring, stirring at a temperature of 70° C. for 10 min, rolling into a sheet, and drying at 50° C. for 10 h to obtain a sheet blank;
[0038] S4. Add polylactic acid, polyhydroxyalkanoate, thermosetting end-carboxyl polyester resin, polyacrylic acid, nano-silicon carbide powder and hydroxyalkylamide into 50 kg of ethyl acetate and mix evenly to obtain a premixed liquid c; spray the premixed liquid c onto one side of the sheet blank with a high-pressure spray gun to a thickness of 20 μm, air-dry naturally to constant weight, and then cure with a microwave heater, wherein the microwave power is 320 W and the microwave time is 1 h, and then cool to room temperature.
[0039] Example 2
[0040] A recyclable polyvinyl alcohol resin packaging material comprises a polyvinyl alcohol sheet blank and a polyester layer coated on one side of the polyvinyl alcohol sheet blank.
[0041] The raw materials of the polyvinyl alcohol sheet blank include: 150kg of polyvinyl alcohol, 50kg of nano-white carbon black, 6kg of graphene oxide, 2kg of amino-terminated polyamide-amine, 2kg of sodium alginate, 0.1kg of N-hydroxysuccinimide and 2kg of calcium chloride.
[0042] The raw materials of the polyester layer include: 15kg of polylactic acid, 5kg of polybutylene succinate, 15kg of thermosetting carboxyl-terminated polyester resin, 5kg of polyacrylic acid, 10kg of nano silicon carbide powder and 1kg of hydroxyalkylamide.
[0043] The method for preparing the above-mentioned recyclable polyvinyl alcohol resin packaging material comprises the following steps:
[0044] S1. Add graphene oxide to 40 kg of water, and ultrasonically disperse for 15 min at a frequency of 20 kHz. Add amino-terminated polyamide-amine and sodium alginate and continue ultrasonicating for 5 min. Add N-hydroxysuccinimide and stir at a speed of 500 r / min for 5 min to obtain preform a.
[0045] S2, adding calcium chloride to 40 kg of deionized water and stirring evenly to obtain a premixed solution b;
[0046] S3, adding polyvinyl alcohol to 500 kg of deionized water, stirring at 70° C. for 30 min to obtain pre-dispersed polyvinyl alcohol; adding premixed liquid a, premixed liquid b, and nano-white carbon black to the pre-dispersed polyvinyl alcohol in a stirring state, stirring at 80° C. for 40 min, rolling into a sheet, and drying at 70° C. for 20 h to obtain a sheet blank;
[0047] S4. Add polylactic acid, polybutylene succinate, thermosetting end-carboxyl polyester resin, polyacrylic acid, nano-silicon carbide powder, and hydroxyalkylamide into 100 kg of dimethylacetamide and mix evenly to obtain a premixed liquid c; spray the premixed liquid c onto one side of the sheet blank with a high-pressure spray gun to a thickness of 50 μm, air-dry naturally to constant weight, and then cure with a microwave heater, wherein the microwave power is 360 W and the microwave time is 5 h, and then cool to room temperature.
[0048] Example 3
[0049] A recyclable polyvinyl alcohol resin packaging material comprises a polyvinyl alcohol sheet blank and a polyester layer coated on one side of the polyvinyl alcohol sheet blank.
[0050] The raw materials of the polyvinyl alcohol sheet blank include: 80kg of polyvinyl alcohol, 30kg of nano calcium carbonate, 10kg of nano white carbon black, 3kg of graphene oxide, 1.7kg of amino-terminated polyamide-amine, 1.2kg of sodium alginate, 0.08kg of N-hydroxysuccinimide and 1.4kg of calcium chloride.
[0051] The raw materials of the polyester layer include: 18 kg of polyhydroxyalkanoate, 8 kg of thermosetting carboxyl-terminated polyester resin, 4 kg of polyacrylic acid, 4 kg of nano silicon carbide powder, and 0.8 kg of hydroxyalkylamide.
[0052] The method for preparing the above-mentioned recyclable polyvinyl alcohol resin packaging material comprises the following steps:
[0053] S1. Add graphene oxide to 25 kg of water, and ultrasonically disperse for 12 min at a frequency of 12 kHz. Add amino-terminated polyamide-amine and sodium alginate and continue ultrasonicating for 4 min. Add N-hydroxysuccinimide and stir at a speed of 200 r / min for 4 min to obtain preform a.
[0054] S2, adding calcium chloride to 25 kg of deionized water and stirring evenly to obtain a premixed solution b;
[0055] S3, adding polyvinyl alcohol to 400 kg of deionized water, stirring at a temperature of 62 ° C for 25 minutes to obtain pre-dispersed polyvinyl alcohol; adding premixed liquid a, premixed liquid b, nano calcium carbonate, and nano white carbon black to the pre-dispersed polyvinyl alcohol in a stirring state, stirring at a temperature of 73 ° C for 30 minutes, rolling into a sheet, and drying at 55 ° C for 18 hours to obtain a sheet blank;
[0056] S4. Add polyhydroxyalkanoic acid ester, thermosetting end carboxyl polyester resin, polyacrylic acid, nano silicon carbide powder and hydroxyalkylamide into 70 kg of dimethylacetamide and mix evenly to obtain premixed liquid c; spray the premixed liquid c onto one side of the sheet blank with a high-pressure spray gun to a thickness of 40 μm, air-dry naturally to constant weight, and then cure with a microwave heater, wherein the microwave power is 330 W and the microwave time is 4 h, and then cool to room temperature.
[0057] Example 4
[0058] A recyclable polyvinyl alcohol resin packaging material comprises a polyvinyl alcohol sheet blank and a polyester layer coated on one side of the polyvinyl alcohol sheet blank.
[0059] The raw materials of the polyvinyl alcohol sheet blank include: 120kg of polyvinyl alcohol, 20kg of nano calcium carbonate, 5kg of graphene oxide, 1.3kg of amino-terminated polyamide-amine, 1.8kg of sodium alginate, 0.02kg of N-hydroxysuccinimide and 1.8kg of calcium chloride.
[0060] The raw materials of the polyester layer include: 12kg of polybutylene succinate, 12kg of thermosetting carboxyl-terminated polyester resin, 2kg of polyacrylic acid, 8kg of nano silicon carbide powder, and 0.2kg of hydroxyalkylamide.
[0061] The method for preparing the above-mentioned recyclable polyvinyl alcohol resin packaging material comprises the following steps:
[0062] S1. Add graphene oxide to 35 kg of water, and ultrasonically disperse for 8 min at a frequency of 18 kHz. Add amino-terminated polyamide-amine and sodium alginate and continue ultrasonicating for 2 min. Add N-hydroxysuccinimide and stir at a speed of 400 r / min for 2 min to obtain preform a.
[0063] S2, adding calcium chloride to 35 kg of deionized water and stirring evenly to obtain a premixed solution b;
[0064] S3, adding polyvinyl alcohol to 300 kg of deionized water, stirring at a temperature of 68 ° C for 15 minutes to obtain pre-dispersed polyvinyl alcohol; adding premixed liquid a, premixed liquid b, and nano-calcium carbonate to the pre-dispersed polyvinyl alcohol in a stirring state, stirring at a temperature of 77 ° C for 20 minutes, rolling into a sheet, and drying at 65 ° C for 12 hours to obtain a sheet blank;
[0065] S4. Add polybutylene succinate, thermosetting end-carboxyl polyester resin, polyacrylic acid, nano-silicon carbide powder and hydroxyalkylamide into 90 kg of dimethylformamide and mix evenly to obtain a premixed liquid c; spray the premixed liquid c onto one side of the sheet blank with a high-pressure spray gun to a thickness of 30 μm, air-dry naturally to constant weight, and then cure with a microwave heater, wherein the microwave power is 350 W and the microwave time is 2 h, and then cool to room temperature.
[0066] Example 5
[0067] A recyclable polyvinyl alcohol resin packaging material comprises a polyvinyl alcohol sheet blank and a polyester layer coated on one side of the polyvinyl alcohol sheet blank.
[0068] The raw materials of the polyvinyl alcohol sheet blank include: 100 kg of polyvinyl alcohol, 30 kg of nano-bentonite, 4 kg of graphene oxide, 1.5 kg of amino-terminated polyamide-amine, 1.5 kg of sodium alginate, 0.05 kg of N-hydroxysuccinimide, and 1.6 kg of calcium chloride.
[0069] The raw materials of the polyester layer include: 15kg of polylactic acid, 10kg of thermosetting carboxyl-terminated polyester resin, 3kg of polyacrylic acid, 6kg of nano silicon carbide powder, and 0.5kg of hydroxyalkylamide.
[0070] The method for preparing the above-mentioned recyclable polyvinyl alcohol resin packaging material comprises the following steps:
[0071] S1. Add graphene oxide to 30 kg of water, and ultrasonically disperse for 10 min at a frequency of 15 kHz. Add amino-terminated polyamide-amine and sodium alginate and continue ultrasonicating for 3 min. Add N-hydroxysuccinimide and stir at a speed of 300 r / min for 3 min to obtain preform a.
[0072] S2. Add calcium chloride into 30 kg of deionized water and stir evenly to obtain a premixed solution b;
[0073] S3, adding polyvinyl alcohol to 350 kg of deionized water, stirring at a temperature of 65 ° C for 20 minutes to obtain pre-dispersed polyvinyl alcohol; adding premixed liquid a, premixed liquid b, and nano-bentonite to the pre-dispersed polyvinyl alcohol in a stirring state, stirring at a temperature of 75 ° C for 25 minutes, rolling into a sheet, and drying at 60 ° C for 15 hours to obtain a sheet blank;
[0074] S4. Add polylactic acid, thermosetting end-carboxyl polyester resin, polyacrylic acid, nano-silicon carbide powder and hydroxyalkylamide into 80 kg of dimethylformamide and mix evenly to obtain a premixed liquid c; spray the premixed liquid c onto one side of the sheet blank with a high-pressure spray gun to a thickness of 35 μm, air-dry naturally to constant weight, and then cure with a microwave heater, wherein the microwave power is 340 W and the microwave time is 3 h, and then cool to room temperature.
[0075] Comparative Example 1
[0076] A recyclable polyvinyl alcohol resin packaging material comprises a polyvinyl alcohol sheet blank and a polyester layer coated on one side of the polyvinyl alcohol sheet blank.
[0077] The raw materials of the polyvinyl alcohol sheet blank include: 100 kg of polyvinyl alcohol, 30 kg of nano-bentonite, 4 kg of graphene oxide, 1.5 kg of sodium alginate, 0.05 kg of N-hydroxysuccinimide, and 1.6 kg of calcium chloride.
[0078] The raw materials of the polyester layer include: 15kg of polylactic acid, 10kg of thermosetting carboxyl-terminated polyester resin, 3kg of polyacrylic acid, 6kg of nano silicon carbide powder, and 0.5kg of hydroxyalkylamide.
[0079] The method for preparing the above-mentioned recyclable polyvinyl alcohol resin packaging material comprises the following steps:
[0080] S1. Add graphene oxide to 30 kg of water, and ultrasonically disperse for 10 min at a frequency of 15 kHz. Add sodium alginate and continue ultrasonicating for 3 min. Add N-hydroxysuccinimide and stir at a speed of 300 r / min for 3 min to obtain preform a.
[0081] S2. Add calcium chloride into 30 kg of deionized water and stir evenly to obtain a premixed solution b;
[0082] S3, adding polyvinyl alcohol to 350 kg of deionized water, stirring at a temperature of 65 ° C for 20 minutes to obtain pre-dispersed polyvinyl alcohol; adding premixed liquid a, premixed liquid b, and nano-bentonite to the pre-dispersed polyvinyl alcohol in a stirring state, stirring at a temperature of 75 ° C for 25 minutes, rolling into a sheet, and drying at 60 ° C for 15 hours to obtain a sheet blank;
[0083] S4. Add polylactic acid, thermosetting end-carboxyl polyester resin, polyacrylic acid, nano-silicon carbide powder and hydroxyalkylamide into 80 kg of dimethylformamide and mix evenly to obtain a premixed liquid c; spray the premixed liquid c onto one side of the sheet blank with a high-pressure spray gun to a thickness of 35 μm, air-dry naturally to constant weight, and then cure with a microwave heater, wherein the microwave power is 340 W and the microwave time is 3 h, and then cool to room temperature.
[0084] Comparative Example 2
[0085] A recyclable polyvinyl alcohol resin packaging material comprises a polyvinyl alcohol sheet blank and a polyester layer coated on one side of the polyvinyl alcohol sheet blank.
[0086] The raw materials of the polyvinyl alcohol sheet blank include: 100 kg of polyvinyl alcohol, 30 kg of nano-bentonite, 4 kg of graphene oxide, 1.5 kg of amino-terminated polyamide-amine, 1.5 kg of sodium alginate, 0.05 kg of N-hydroxysuccinimide, and 1.6 kg of calcium chloride.
[0087] The raw materials of the polyester layer include: 15kg of polylactic acid, 10kg of thermosetting carboxyl-terminated polyester resin, 3kg of polyacrylic acid, 6kg of calcium carbonate powder with a particle size of 0.1-0.5μm, and 0.5kg of hydroxyalkylamide.
[0088] The method for preparing the above-mentioned recyclable polyvinyl alcohol resin packaging material comprises the following steps:
[0089] S1. Add graphene oxide to 30 kg of water, and ultrasonically disperse for 10 min at a frequency of 15 kHz. Add amino-terminated polyamide-amine and sodium alginate and continue ultrasonicating for 3 min. Add N-hydroxysuccinimide and stir at a speed of 300 r / min for 3 min to obtain preform a.
[0090] S2. Add calcium chloride into 30 kg of deionized water and stir evenly to obtain a premixed solution b;
[0091] S3, adding polyvinyl alcohol to 350 kg of deionized water, stirring at a temperature of 65 ° C for 20 minutes to obtain pre-dispersed polyvinyl alcohol; adding premixed liquid a, premixed liquid b, and nano-bentonite to the pre-dispersed polyvinyl alcohol in a stirring state, stirring at a temperature of 75 ° C for 25 minutes, rolling into a sheet, and drying at 60 ° C for 15 hours to obtain a sheet blank;
[0092] S4. Add polylactic acid, thermosetting end-carboxyl polyester resin, polyacrylic acid, calcium carbonate powder and hydroxyalkylamide into 80 kg of dimethylformamide and mix evenly to obtain a premixed liquid c; spray the premixed liquid c onto one side of the sheet blank using a high-pressure spray gun with a thickness of 35 μm, air-dry naturally to constant weight, and then cure using a microwave heater with a microwave power of 340 W and a microwave time of 3 h, and then cool to room temperature.
[0093] The thickness of the packaging materials obtained in Example 5 and Comparative Examples 1-2 was tested, and the thickness was within the range of 285.7±5.39μm. The tensile properties were tested with reference to GB / T 1040.2-2022 "Determination of tensile properties of plastics Part 2: Test conditions for molded and extruded plastics". Figure 1 As shown, the tensile strength and elongation at break of the packaging material obtained in Example 5 are both the highest, which proves that the packaging material obtained in the present invention has excellent mechanical properties.
[0094] The applicant believes that this is because the present invention grafts dendritic polyamide-amine onto the graphene oxide sheet structure, and then compounds it with sodium alginate and combines it in polyvinyl alcohol to form a network structure similar to a reinforcing rib structure. At the same time, the polyamide-amine surface has a large number of active amino groups, which can form hydrogen bonds with sodium alginate, which can significantly enhance the good dispersion of fillers in the system. After curing, it not only significantly enhances the cross-linking density of the blank, but also enhances the mechanical strength. The bio-based polyester is compounded with a thermosetting carboxyl-terminated polyester resin and polyacrylic acid, and under the action of hydroxyalkylamide, the micro-nano filler can be uniformly attached to one side of the sheet blank. With microwave curing, the polyacrylic acid and the polyvinyl alcohol sheet blank are cross-linked and bonded, and the bonding strength is extremely high, which further promotes the improvement of mechanical strength.
[0095] The polyester layer of the packaging materials obtained in Example 5 and Comparative Examples 1-2 was tested for static water contact angle using a contact angle tester. Then, the polyester layer of each group of samples was subjected to a tensile wear test, as follows:
[0096] A 250g iron block was placed on each group of composite materials, and then 400-grit sandpaper was used to keep close contact with each group of composite materials. Then, each group of composite materials was dragged in the same direction with a wear length of 20cm. After 20 scraping cycles, the static water contact angle of each group of samples was tested.
[0097] like Figure 2 As shown, the static water contact angle of the polyester layer of the packaging material obtained in Example 5 before and after abrasion is ≥150°, showing a super hydrophobic effect. The static water contact angle of the polyester layer of the packaging material obtained in Comparative Example 1 after abrasion is >150°, showing a super hydrophobic effect, but it decreases rapidly after abrasion, while the static water contact angle of the polyester layer of the packaging material obtained in Comparative Example 2 is always <150°.
[0098] The applicant believes that this is because comparative example 2 uses calcium carbonate powder with a particle size of 0.1-0.5 μm as the raw material for the polyester layer, which cannot form a micro-nano structure and is difficult to achieve a super-hydrophobic effect; while comparative example 1 does not use amino-terminated polyamide-amine, so the bonding strength between its polyester layer and the polyvinyl alcohol sheet blank is not as good as that in Example 5, resulting in the destruction of the polyester layer after wear, thereby losing the super-hydrophobic effect.
[0099] Referring to GB / T 1038.1-2022 "Test method for gas permeability of plastic film and sheet - Part 1: Differential pressure method", a gas permeometer was used to test the oxygen barrier properties of the packaging materials obtained in Example 5 and Comparative Examples 1-2. The test temperature was 23°C, the relative humidity was 50%, the sample diameter was 97 mm, and the test area was 38.46 cm 2 Referring to GB / T 1037-2021 "Determination of water vapor permeability of plastic films and sheets - Cup weight gain and weight loss method" and GB / T16928-1997 "Test method for water vapor permeability of packaging materials", the water vapor barrier properties of each group of samples were tested using a water vapor permeability tester. The test temperature was 38°C, the relative humidity was 90%, the sample diameter was 74mm, and the test area was 33cm 2 .
[0100] like Figure 3 As shown, the gas permeability and moisture permeability of the packaging material obtained in Example 5 are both lower than those of the comparative example, indicating that the barrier effect of the packaging material obtained in Example 5 is better than that of the comparative example.
[0101] The applicant believes that this is because the present invention grafts dendritic polyamide-amine onto the graphene oxide sheet structure, then compounds it with sodium alginate and combines it in polyvinyl alcohol to form a network structure similar to a reinforcing rib structure, which has excellent water and oxygen barrier properties; at the same time, the polyamide-amine surface has a large number of active amino groups, which can form hydrogen bonds with sodium alginate, which can significantly enhance the good dispersion of fillers in the system, and can further enhance its barrier properties after curing. The bio-based polyester is compounded with thermosetting end carboxyl polyester resin and polyacrylic acid, which can promote the uniform attachment of micro-nano fillers to one side of the sheet blank under the action of hydroxyalkylamide, and with microwave curing, the polyacrylic acid and the polyvinyl alcohol sheet blank are cross-linked and bonded, and the bonding strength is extremely high, which further blocks the diffusion of water and gas.
[0102] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A recyclable polyvinyl alcohol resin packaging material, characterized in that: include: A polyvinyl alcohol sheet body, and a polyester layer coated on one side of the polyvinyl alcohol sheet body; The raw materials of the polyvinyl alcohol sheet blank include: 50-150 parts of polyvinyl alcohol, 10-50 parts of filler, 2-6 parts of graphene oxide, 1-2 parts of amino-terminated polyamide-amine, 1-2 parts of sodium alginate, 0.01-0.1 parts of N-hydroxysuccinimide, and 1-2 parts of calcium chloride; The polyester layer raw materials include: 10-20 parts of bio-based polyester, 5-15 parts of thermosetting carboxyl-terminated polyester resin, 1-5 parts of polyacrylic acid, 2-10 parts of nano silicon carbide powder and 0.1-1 part of hydroxyalkylamide.
2. The recyclable polyvinyl alcohol resin packaging material according to claim 1, characterized in that: Polyvinyl alcohol is Nichigo G-Polymer TM .
3. The recyclable polyvinyl alcohol resin packaging material according to claim 1, characterized in that: The bio-based polyester is at least one of polylactic acid, polyhydroxyalkanoate, and polybutylene succinate.
4. The recyclable polyvinyl alcohol resin packaging material according to claim 1, characterized in that: The filler is at least one of nano bentonite, nano calcium carbonate and nano white carbon black.
5. A method for preparing the recyclable polyvinyl alcohol resin packaging material according to any one of claims 1 to 4, characterized in that: The steps include: S1, adding graphene oxide to water and ultrasonically dispersing for 5-15 minutes, adding amino-terminated polyamide-amine and sodium alginate thereto and continuing ultrasonication for 1-5 minutes, adding N-hydroxysuccinimide and stirring for 1-5 minutes to obtain preform a; S2, adding calcium chloride into deionized water and stirring evenly to obtain a premixed solution b; S3, adding polyvinyl alcohol to deionized water, stirring at 60-70° C. for 10-30 min to obtain pre-dispersed polyvinyl alcohol; adding premixed liquid a, premixed liquid b, and filler to the pre-dispersed polyvinyl alcohol in sequence under stirring, stirring at 70-80° C. for 10-40 min, rolling into a sheet, and drying to obtain a sheet blank; S4. Add bio-based polyester, thermosetting end-carboxyl polyester resin, polyacrylic acid, nano-silicon carbide powder and hydroxyalkylamide into the organic solution and mix evenly to obtain a premixed liquid c; spray the premixed liquid c onto one surface of the sheet blank under high pressure, air-dry naturally to constant weight, cure by microwave heating for 1-5 hours, and cool to room temperature.
6. The method for preparing the recyclable polyvinyl alcohol resin packaging material according to claim 5, characterized in that: In S1, the ultrasonic dispersion frequency is 10-20 kHz.
7. The method for preparing the recyclable polyvinyl alcohol resin packaging material according to claim 5, characterized in that: In S1, after adding N-hydroxysuccinimide, stir at a speed of 100-500 r / min for 1-5 min.
8. The method for preparing the recyclable polyvinyl alcohol resin packaging material according to claim 5, characterized in that: In S3, the drying temperature is 50-70°C and the drying time is 10-20h.
9. The method for preparing the recyclable polyvinyl alcohol resin packaging material according to claim 5, characterized in that: In S4, the organic solvent is at least one of ethyl acetate, dimethylformamide, and dimethylacetamide.
10. The method for preparing the recyclable polyvinyl alcohol resin packaging material according to claim 5, characterized in that: In S4, the microwave power is 320-360W.