A slow-release repair agent for paddy field soil contaminated by cadmium and arsenic as well as its preparation process and application

Through the combined technology of modified diatomite and biochar, the problems of limited passivation effect and long remediation time of cadmium and arsenic composite contaminated soil are solved, achieving simultaneous passivation and stable reduction of cadmium and arsenic, ensuring safe utilization of soil .

CN118325619BActive Publication Date: 2024-10-01HUNAN LVERKANG BIOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410433348.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-11
Publication Date
2024-10-01
Estimated Expiration
2044-04-11

AI Technical Summary

Technical Problem

The existing technology has problems of limited passivation effect and long remediation time when treating soil contaminated by cadmium and arsenic. In particular, the simultaneous passivation effect of cadmium and arsenic is not good, and may affect the soil biological community structure, resulting in inconsistent changes in subsequent physical and chemical properties. clear.

Method used

Modified diatomite and calcium peroxide are used for mixing and granulation, and modified biochar is used as a coating material to coat the calcium peroxide composite particles. Through the modification functions of modified diatomite and biochar Improve the adsorption and passivation effect of cadmium and arsenic, form a porous structure and phosphate groups to enhance the stability of cadmium and arsenic.

Benefits of technology

It achieves simultaneous passivation control of cadmium and arsenic during the entire growth period of rice, significantly reduces the cadmium and arsenic content in rice and soil, and ensures the safe use of cadmium and arsenic composite contaminated soil. The remediation agent is used in a small amount and has a stable effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118325619B_ABST
    Figure CN118325619B_ABST
Patent Text Reader

Abstract

The present invention discloses a slow-release repair agent for paddy field soil contaminated by cadmium and arsenic, and its preparation process and application, comprising the following steps: S1, preparation of modified diatomaceous earth; S2, mixed granulation; S3, preparation of modified biochar; S4, coating. The slow-release repair agent for paddy field soil contaminated by cadmium and arsenic provided by the present invention is prepared by mixing and granulating modified diatomaceous earth with calcium peroxide, so that the inside of the calcium peroxide composite particles has a porous structure, the internal structure of the particles is complicated, and the release rate of oxygen in the repair agent is delayed. Subsequently, the calcium peroxide composite particles are coated with modified biochar to extend the adsorption and passivation effect, so that the adsorption and passivation effect of the composite particles can be carried out to implement cadmium and arsenic synchronous passivation and control on rice throughout the growth period. The repair agent can effectively reduce the cadmium and arsenic content in rice, realize the safe utilization of paddy field soil contaminated by cadmium and arsenic, and has a small dosage, significant effect and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of soil pollution remediation, and specifically relates to a slow-release remediation agent for paddy field soil contaminated with cadmium and arsenic as well as a preparation process and application thereof. Background Art

[0002] In recent years, with the rapid development of industry and agriculture in my country, the problem of heavy metal pollution in soil has become increasingly serious, and the resulting economic losses have restricted the sustainable development of agriculture. Heavy metal pollution has always been an environmental issue related to the balance of natural ecology and human health and safety. In particular, cadmium (Cd) and arsenic (As), which are considered carcinogens, have become environmental pollutants of global concern. Heavy metal pollution in soil can lead to a decrease in soil productivity, cause groundwater pollution, and endanger human health risks through the food chain.

[0003] Cadmium and arsenic are both first-level carcinogens. Areas of cadmium-arsenic combined pollution often overlap with rice-growing areas. In addition, rice, as a major food crop, is prone to accumulate cadmium and arsenic. Rice production under the combined influence of multiple factors has posed a serious threat to my country's food security and people's lives and health. Therefore, it is urgent to control the combined pollution of cadmium and arsenic in rice fields.

[0004] For heavy metal contaminated soil, researchers have developed a series of in-situ and ex-situ remediation technologies. Taking into account factors such as remediation cost, technical difficulty, remediation time and public acceptability, in-situ remediation technology is currently the most respected remediation technology for heavy metal contaminated soil, among which in-situ passivation remediation technology is the most widely used. The main principle of passivation remediation is to control the effectiveness of heavy metals in the soil by adding chemical agents or materials. However, since cadmium and arsenic have opposite biological characteristics, it is difficult to remediate cadmium and arsenic compound contaminated soil. Cadmium and arsenic compound pollution has become a difficulty and hot spot in soil pollution remediation.

[0005] Chinese patent CN113136214A discloses a cadmium-arsenic passivated soil slow-release repair agent and its preparation method and application. The invention provides a cadmium-arsenic passivated soil slow-release repair agent, which contains the following components by mass: 80-99 parts of calcium peroxide powder; 0.01-2 parts of organosilicon; 1-10 parts of ethyl cellulose. The invention also provides a method for preparing a soil slow-release repair agent and its application. The invention granulates and encapsulates calcium peroxide powder and organosilicon repair materials with different passivation principles to prepare slow-release repair agent particles, which can implement cadmium-arsenic synchronous passivation control during the entire growth period of rice, effectively reduce the cadmium-arsenic content in rice and soil, reduce the cadmium content of rice by more than 70%, reduce the arsenic content of rice by more than 80%, reduce the effective cadmium content of soil by more than 24%, reduce the effective arsenic content of soil by more than 34%, and reduce the trivalent arsenic content of soil by more than 76%, thus realizing the safe utilization of paddy field soil contaminated by cadmium-arsenic compound. However, the patent uses organosilicon and ethyl cellulose to coat calcium peroxide, and these two materials have limited passivation effects on arsenic isolation, and the repair effect still has room for further improvement. Chinese patent CN113652238A discloses a repair agent for cadmium and arsenic in contaminated soil for synchronous passivation and its application, and its preparation method comprises the following steps: preparing Delftia sp. B9 into a bacterial suspension, mixing it evenly with iron salt, and adjusting the pH value to obtain a composite suspension. The repair agent for cadmium and arsenic in the synchronous passivation contaminated soil has low raw material cost and is not easy to cause secondary pollution, and has broad application prospects in the field of Cd and As composite contaminated soil. However, the time required for the repair agent in the patent to produce a significant effect on the passivation of contaminated soil is relatively long, and other strains (Delftia sp.) added to the soil are easy to change the original biological community structure in the soil, and it is not clear what kind of impact it has on the subsequent physical and chemical properties of the soil, which is not conducive to widespread use.

[0006] Therefore, in view of the difficulty in simultaneous remediation and treatment of cadmium-arsenic co-contaminated soil, the field has developed a remediation agent that can achieve simultaneous passivation of cadmium and arsenic, which has important practical value and realistic significance. Summary of the invention

[0007] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a slow-release repair agent for paddy field soil contaminated with cadmium and arsenic, and its preparation process and application. The soil slow-release repair agent can effectively reduce the cadmium and arsenic content in rice, realize the safe utilization of paddy field soil contaminated with cadmium and arsenic, and has good application prospects.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] A preparation process of a slow-release repair agent for paddy field soil contaminated by cadmium and arsenic, comprising the following steps:

[0010] S1. Preparation of modified diatomite: adding pretreated diatomite to an ethanol aqueous solution, then adding vinyl triethoxysilane, stirring to react, filtering, washing, and drying after the reaction is completed to obtain diatomite containing double bonds; adding diatomite containing double bonds to dimethylformamide, then adding polyethylene glycol methacrylate phosphate and azobisisobutyronitrile, reacting at a constant temperature, filtering, washing, and drying after the reaction is completed to obtain modified diatomite;

[0011] S2, mixing and granulating: by weight, 70-80 parts of calcium peroxide powder and 20-30 parts of the modified diatomaceous earth in step S1 are mixed evenly, and then granulated to obtain calcium peroxide composite particles;

[0012] S3, preparation of modified biochar: adding the pretreated biochar to an ethanol aqueous solution, then adding γ-aminopropyltriethoxysilane, heating reaction, filtering, washing, and drying after the reaction is completed to obtain amination biochar; then adding the amination biochar to dimethylformamide, then adding 2-mercaptonicotinic acid and triethylamine, stirring reaction, filtering, washing, and drying after the reaction is completed to obtain modified biochar;

[0013] S4, coating: using the modified biochar in step S3 as a coating material, coating the calcium peroxide composite particles in step S2, and obtaining a soil slow-release repair agent after drying.

[0014] Preferably, the specific method for pretreating diatomite in step S1 is as follows: by weight, 100 parts of diatomite are added to 1000-1200 parts of a 5-8% sodium hydroxide solution, and immersed at 70-80° C. for 1-2 hours. After the immersion is completed, 150-200 parts of a 10-15% manganese chloride solution are added, stirred for 1-2 hours, and then filtered, washed, dried, and calcined at 350-450° C. for 2-3 hours to obtain pretreated diatomite.

[0015] In the present invention, diatomaceous earth is used as the substrate, which has unique properties such as high permeability, high porosity, small particle size, large surface area, low thermal conductivity and chemical inertness. By modifying it, its adsorption performance and stabilization ability for Cd and As ions in the soil can be improved.

[0016] Preferably, the volume ratio of ethanol to water in the ethanol aqueous solution in step S1 is 3:1, the mass ratio of the pretreated diatomaceous earth and vinyl triethoxysilane is 100:10-15, the temperature of the stirring reaction is 50-60°C, and the time is 4-5h; the mass ratio of the double bond-containing diatomaceous earth, polyethylene glycol methacrylate phosphate, and azobisisobutyronitrile is 100:12-17:0.5-1, and the temperature of the isothermal reaction is 90-100°C, and the time is 2-3h.

[0017] In the present invention, the added polyethylene glycol methacrylate phosphate contains a phosphoric acid group and an oxygen-containing group, and the phosphorus group can form a coordination bond with the cadmium ion, thereby achieving the passivation of the cadmium ion.

[0018] Preferably, the specific method of granulation in step S2 is: adjusting the inclination angle of the disc of the disc granulator to 50-65°, and adjusting the heating device to 40-55°C; mixing the calcium peroxide powder and the modified diatomaceous earth evenly to obtain a mixed powder, putting it into the disc of the disc granulator, adjusting the speed of the disc granulator to 20-40r / min, and according to the granulation situation, using a water mist spray gun to continuously spray water mist at the rising point of the powder, and continuously screening out particles with a diameter of 3-5mm and smooth surface, and continuously adding the mixed powder until the granulation is completed.

[0019] In the present invention, calcium peroxide is an oxidant that is soluble in water and is alkaline and releases oxygen. It can reduce the effectiveness of cadmium in the soil by increasing the soil pH and can also oxidize the more toxic As 3+ Converted to less toxic As 5+ , to reduce As activity.

[0020] Preferably, the specific preparation method of the pretreated biochar described in step S3 is as follows: by weight, 100-150 parts of corn cobs are crushed and added to 800-1000 parts of a sodium hydroxide solution with a mass fraction of 5-8%, stirred and immersed for 3-5 hours at room temperature, and then 200-300 parts of a 10-15% ferric nitrate solution are added, and aged at 40-50°C for 12-16 hours. After aging, it is filtered and dried, calcined at 350-450°C for 2-4 hours, and ground to obtain pretreated biochar.

[0021] In the present invention, corn cobs are used as biomass to prepare biochar, which has the characteristics of porous structure, rich surface functional groups, high specific surface area, etc. Due to the strong electronegativity and rich porous structure of the biochar surface, it has strong adsorption and stabilization capabilities for most cationic heavy metals, but has limited efficiency for anions such as metalloid arsenic. By modifying it, its adsorption of arsenic ions can be improved.

[0022] Preferably, the volume ratio of ethanol to water in the ethanol aqueous solution in step S3 is 3:1, the mass ratio of the pretreated biochar and γ-aminopropyltriethoxysilane is 100:10-15, the temperature of the heating reaction is 55-65°C, and the time is 3-4h.

[0023] Preferably, in step S3, the mass ratio of the amination biochar, 2-mercaptonicotinic acid and triethylamine is 100:10-15:40-50, the stirring reaction temperature is 75-85°C, and the reaction time is 2-3h.

[0024] In the present invention, the added 2-mercaptonicotinic acid, the mercapto groups contained in it can coordinate with arsenic ions, so as to achieve the adsorption and fixation of arsenic ions, thereby improving the synchronous passivation effect of the soil slow-release repair agent on cadmium and arsenic.

[0025] Preferably, the specific steps of the coating treatment in step S4 are as follows: adjust the inclination angle of the disc of the drum granulator to 55-60°, adjust the heating device to 45-50°C, place 100 parts of calcium peroxide composite particles in the drum granulator, place 10-20 parts of modified biochar as coating materials in a vibrating feeder, add them at a uniform speed, and use a water mist spray gun to continuously spray water mist at the rising part of the particles until the coating is completed, and dry them at 80-100°C for 3-5h.

[0026] The present invention also protects a slow-release repair agent for paddy field soil contaminated with cadmium and arsenic prepared by the process as described above.

[0027] The present invention also protects the use of the above-mentioned slow-release repair agent for paddy field soil contaminated by cadmium and arsenic, wherein the slow-release repair agent for paddy field soil contaminated by cadmium and arsenic is added to the contaminated soil at 0.1-1% of the soil mass.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) The slow-release repair agent for paddy field soil contaminated with cadmium and arsenic provided by the present invention is prepared by mixing modified diatomaceous earth and calcium peroxide to form granules, so that the calcium peroxide composite particles have a porous structure, complicate the internal structure of the particles, and slow down the release rate of oxygen in the repair agent. The calcium peroxide composite particles are then coated with modified biochar to extend the adsorption and passivation effect, so that the adsorption and passivation effect can be extended to implement simultaneous passivation and control of cadmium and arsenic during the entire growth period of rice. The present invention prepares a soil slow-release repair agent by using modified diatomaceous earth, calcium peroxide, and modified biochar through a specific method. The repair agent can effectively reduce the cadmium and arsenic content in rice, realize the safe utilization of paddy field soil contaminated with cadmium and arsenic, and has a small dosage, significant effect and stability.

[0030] (2) The modified diatomite added to the cadmium-arsenic composite contaminated paddy soil slow-release repair agent provided by the present invention is first subjected to alkali treatment to enlarge its internal pores and increase its specific surface area, thereby increasing its adsorption performance. At the same time, manganese ions are doped after the treatment to precipitate manganese oxide on the surface of the diatomite. Manganese oxide has a high adsorption capacity for heavy metals and has relatively complete pore characteristics, which increases the surface area and surface negative charge of the diatomite, thereby improving the adsorption passivation effect of the repair agent on cadmium ions; then the pretreated diatomite is vinylized, and then It is reacted with polyethylene glycol methacrylate phosphate to introduce phosphate groups on the surface of diatomite, which can form insoluble metal orthophosphates with Cd through complexation, coordination, precipitation and other reactions. The phosphorus-containing groups can reduce the adsorption of As by rice through site competition. At the same time, it can also synergistically passivate Cd and As with the iron oxides in the modified biochar, thereby improving the passivation effect of the soil slow-release remediation agent. The phosphorus-containing groups are introduced into the surface of diatomite by chemical grafting, making it difficult for the passivated Cd and As to fall off, thereby avoiding secondary pollution.

[0031] (3) The slow-release repair agent for paddy field soil contaminated by cadmium and arsenic provided by the present invention, the modified biochar added, is used as a coating material, and due to its loose and porous characteristics, the slow-release performance of the repair agent can be further improved; the biomass is first treated with alkali, and ferric nitrate is added. The alkali treatment can destroy part of the non-crystalline cellulose in the biomass, expose the crystalline cellulose on the surface, improve its adsorption performance, and increase the adsorption amount of iron ions. At the same time, it can also cause the pore structure of the biomass to change, so that the prepared biochar has a larger porosity and specific surface area; then the pretreated biochar is amino-modified, and then it is reacted with 2-mercaptonicotinic acid. Through the reaction of the amino group on the biochar with the carboxyl group in the 2-mercaptonicotinic acid, thiol and nitrogen heterocyclic groups are introduced into the surface of the biochar. The thiol group can coordinate with the arsenic ions to achieve the adsorption and fixation of the arsenic ions to form a stable complex. The present invention introduces 2-mercaptonicotinic acid into the surface of the biochar by a chemical grafting method, thereby significantly improving the adsorption passivation effect and stability of the repair agent for Cd and As ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The graph showing the changes in active oxygen content in each group of extracts;

[0033] Figure 2 This is a graph showing the effects of each group of soil slow-release remediation agents on the cadmium content in rice;

[0034] Figure 3 This is a graph showing the effect of each group of soil slow-release remediation agents on the arsenic content in rice;

[0035] Figure 4 This is the effect of each group of soil slow-release remediation agents on the effective cadmium content in the soil;

[0036] Figure 5 This is a graph showing the effect of each group of soil slow-release remediation agents on the effective arsenic content in the soil. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] The diatomaceous earth was purchased from Shijiazhuang Yitian Mineral Products Co., Ltd., with a mesh size of 325; the calcium peroxide was purchased from Henan Huize Bioengineering Co., Ltd., with a composition of 70% calcium peroxide and 30% calcium hydroxide; the rice was late rice variety Jinyou 59.

[0039] Example 1

[0040] A preparation process of a slow-release repair agent for paddy field soil contaminated by cadmium and arsenic, comprising the following steps:

[0041] S1. Preparation of modified diatomite: 100 g of diatomite was added to 1100 g of 7% sodium hydroxide solution, and immersed at 75° C. for 1.5 h. After the immersion, 180 g of 10% manganese chloride solution was added, and stirred for 1.5 h. The mixture was then filtered, washed, dried, and calcined at 400° C. for 2.5 h to obtain pretreated diatomite. 100 g of pretreated diatomite was added to 1500 mL of ethanol aqueous solution (the volume ratio of ethanol to water was 3:1), then add 13g of vinyl triethoxysilane, stir and react at 55°C for 4.5h, filter, wash and dry after the reaction is completed to obtain diatomaceous earth containing double bonds; add 100g of diatomaceous earth containing double bonds to 1000mL of dimethylformamide, then add 15g of polyethylene glycol methacrylate phosphate and 0.8g of azobisisobutyronitrile, and react at a constant temperature of 55°C for 4.5h. After the reaction is completed, filter, wash and dry to obtain modified diatomaceous earth;

[0042] S2, mixed granulation: the disc inclination angle of the disc granulator is adjusted to 60°, and the heating device is adjusted to 50°C; 750g of calcium peroxide powder and 250g of modified diatomaceous earth are mixed evenly to obtain a mixed powder, which is put into the disc of the disc granulator, and the speed of the disc granulator is adjusted to 30r / min. According to the granulation situation, a water mist spray gun is used to continuously spray water mist at the rising part of the powder, and particles with a diameter of 3-5mm and smooth surface are continuously screened out, and the mixed powder is continuously added until the granulation is completed to obtain calcium peroxide composite particles;

[0043] S3. Preparation of modified biochar: 130 g corn cob was crushed and added to 900 g sodium hydroxide solution with a mass fraction of 7%, stirred and immersed at room temperature for 4 h, then 250 g ferric nitrate solution with a mass fraction of 10% was added, and aged at 45 ° C for 14 h. After aging, it was filtered and dried, calcined at 400 ° C for 3 h, and then ground through a 150 mesh sieve to obtain pretreated biochar; 100 g pretreated biochar was added to 1000 mL ethanol aqueous solution (the volume ratio of ethanol to water was 3:1), and then 13 g γ-aminopropyltriethoxysilane was added, and the reaction was carried out at 60 ° C for 3.5 h. After the reaction was completed, it was filtered, washed and dried to obtain amino biochar; then 100 g amino biochar was added to 1000 mL dimethylformamide, and then 13 g 2-mercaptonicotinic acid and 45 g triethylamine were added, and the reaction was carried out at 80 ° C for 2.5 h. After the reaction was completed, it was filtered, washed and dried to obtain modified biochar;

[0044] S4. Coating: adjust the inclination angle of the drum granulator disc to 55°, adjust the heating device to 45°C, place 1000g of calcium peroxide composite particles in the drum granulator, place 150g of modified biochar as the coating material in the vibrating feeder, feed them at a uniform speed, and use a water mist spray gun to continuously spray water mist on the rising part of the particles until the coating is completed. Dry at 90°C for 4h to obtain the soil slow-release repair agent.

[0045] Example 2

[0046] A preparation process of a slow-release repair agent for paddy field soil contaminated by cadmium and arsenic, comprising the following steps:

[0047] S1. Preparation of modified diatomite: 100 g of diatomite was added to 1000 g of 8% sodium hydroxide solution, and immersed at 70° C. for 2 h. After the immersion, 150 g of 15% manganese chloride solution was added, and stirred for 2 h. Then, the mixture was filtered, washed, dried, and calcined at 350° C. for 3 h to obtain pretreated diatomite; 100 g of pretreated diatomite was added to 1500 mL of ethanol aqueous solution (the volume ratio of ethanol to water was 3:1), and then 10 g of vinyl triethoxysilane was added, and the mixture was stirred and reacted at 50° C. for 5 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain diatomite containing double bonds; 100 g of diatomite containing double bonds was added to 1000 mL of dimethylformamide, and then 12 g of polyethylene glycol methacrylate phosphate and 0.5 g of azobisisobutyronitrile were added, and the mixture was kept at 50° C. for 5 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain modified diatomite;

[0048] S2, mixed granulation: the disc inclination angle of the disc granulator is adjusted to 50°, and the heating device is adjusted to 40°C; 700g of calcium peroxide powder and 300g of modified diatomaceous earth are mixed evenly to obtain a mixed powder, which is put into the disc of the disc granulator, and the speed of the disc granulator is adjusted to 20r / min. According to the granulation situation, a water mist spray gun is used to continuously spray water mist at the rising part of the powder, and particles with a diameter of 3-5mm and smooth surface are continuously screened out, and the mixed powder is continuously added until the granulation is completed to obtain calcium peroxide composite particles;

[0049] S3. Preparation of modified biochar: 100 g corn cob was crushed and added to 800 g sodium hydroxide solution with a mass fraction of 8%, stirred and immersed at room temperature for 5 h, then 200 g ferric nitrate solution with a mass fraction of 15% was added, aged at 40 ° C for 16 h, filtered and dried after aging, calcined at 350 ° C for 4 h, and then ground through a 150 mesh sieve to obtain pretreated biochar; 100 g pretreated biochar was added to 1000 mL ethanol aqueous solution (the volume ratio of ethanol to water was 3:1), and then 10 g γ-aminopropyltriethoxysilane was added, reacted at 55 ° C for 4 h, filtered, washed and dried after the reaction was completed to obtain amino biochar; then 100 g amino biochar was added to 1000 mL dimethylformamide, and then 10 g 2-mercaptonicotinic acid and 40 g triethylamine were added, reacted at 75 ° C for 3 h, filtered, washed and dried after the reaction was completed to obtain modified biochar;

[0050] S4. Coating: adjust the inclination angle of the drum granulator disc to 55°, adjust the heating device to 45°C, place 1000g of calcium peroxide composite particles in the drum granulator, place 100g of modified biochar as the coating material in the vibrating feeder, feed them at a uniform speed, and use a water mist spray gun to continuously spray water mist on the rising part of the particles until the coating is completed. Dry at 80°C for 5h to obtain the soil slow-release repair agent.

[0051] Example 3

[0052] A preparation process of a slow-release repair agent for paddy field soil contaminated by cadmium and arsenic, comprising the following steps:

[0053] S1. Preparation of modified diatomite: 100 g of diatomite was added to 1200 g of 5% sodium hydroxide solution, immersed at 80° C. for 1 h, and after the immersion, 200 g of 10% manganese chloride solution was added, stirred for 1 h, and then filtered, washed, dried, and calcined at 450° C. for 2 h to obtain pretreated diatomite; 100 g of pretreated diatomite was added to 1500 mL of ethanol aqueous solution (the volume ratio of ethanol to water was 3:1), and then 15 g of vinyl triethoxysilane was added, stirred and reacted at 60° C. for 4 h, and after the reaction was completed, filtered, washed, and dried to obtain diatomite containing double bonds; 100 g of diatomite containing double bonds was added to 1000 mL of dimethylformamide, and then 17 g of polyethylene glycol methacrylate phosphate and 1 g of azobisisobutyronitrile were added, and the mixture was kept at 60° C. for 4 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain modified diatomite;

[0054] S2, mixed granulation: the disc inclination angle of the disc granulator is adjusted to 65°, and the heating device is adjusted to 55°C; 800g of calcium peroxide powder and 200g of modified diatomaceous earth are mixed evenly to obtain a mixed powder, which is put into the disc of the disc granulator, and the speed of the disc granulator is adjusted to 40r / min. According to the granulation situation, a water mist spray gun is used to continuously spray water mist at the rising part of the powder, and particles with a diameter of 3-5mm and smooth surface are continuously screened out, and the mixed powder is continuously added until the granulation is completed to obtain calcium peroxide composite particles;

[0055] S3. Preparation of modified biochar: 150 g corn cob was crushed and added to 1000 g sodium hydroxide solution with a mass fraction of 5%, stirred and immersed at room temperature for 3 h, then 300 g ferric nitrate solution with a mass fraction of 15% was added, and aged at 50°C for 12 h. After aging, it was filtered and dried, calcined at 450°C for 2 h, and then ground through a 150-mesh sieve to obtain pretreated biochar; 100 g pretreated biochar was added to 1000 mL ethanol aqueous solution (the volume ratio of ethanol to water was 3:1), and then 15 g γ-aminopropyltriethoxysilane was added, and the reaction was carried out at 65°C for 3 h. After the reaction was completed, it was filtered, washed and dried to obtain amino biochar; then 100 g amino biochar was added to 1000 mL dimethylformamide, and then 15 g 2-mercaptonicotinic acid and 50 g triethylamine were added, and the reaction was carried out at 85°C for 2 h. After the reaction was completed, it was filtered, washed and dried to obtain modified biochar;

[0056] S4. Coating: adjust the inclination angle of the drum granulator disc to 60°, adjust the heating device to 50°C, place 1000g of calcium peroxide composite particles in the drum granulator, place 200g of modified biochar as coating material in the vibrating feeder, feed them at a uniform speed, and use a water mist spray gun to continuously spray water mist on the rising part of the particles until the coating is completed. Dry at 100°C for 3h to obtain the soil slow-release repair agent.

[0057] Comparative Example 1

[0058] A preparation process of a slow-release repair agent for paddy field soil contaminated by cadmium and arsenic, comprising the following steps:

[0059] S1. Preparation of modified diatomite: 100 g of diatomite was added to 1100 g of a 7% sodium hydroxide solution, and immersed at 75° C. for 1.5 h. After the immersion, the mixture was filtered, washed, and dried, and calcined at 400° C. for 2.5 h to obtain modified diatomite.

[0060] S2, mixed granulation: the disc inclination angle of the disc granulator is adjusted to 60°, and the heating device is adjusted to 50°C; 750g of calcium peroxide powder and 250g of modified diatomaceous earth are mixed evenly to obtain a mixed powder, which is put into the disc of the disc granulator, and the speed of the disc granulator is adjusted to 30r / min. According to the granulation situation, a water mist spray gun is used to continuously spray water mist at the rising part of the powder, and particles with a diameter of 3-5mm and smooth surface are continuously screened out, and the mixed powder is continuously added until the granulation is completed to obtain calcium peroxide composite particles;

[0061] S3. Preparation of modified biochar: 130 g corn cob was crushed and added to 900 g sodium hydroxide solution with a mass fraction of 7%, stirred and immersed at room temperature for 4 h, then 250 g ferric nitrate solution with a mass fraction of 10% was added, and aged at 45 ° C for 14 h. After aging, it was filtered and dried, calcined at 400 ° C for 3 h, and then ground through a 150 mesh sieve to obtain pretreated biochar; 100 g pretreated biochar was added to 1000 mL ethanol aqueous solution (the volume ratio of ethanol to water was 3:1), and then 13 g γ-aminopropyltriethoxysilane was added, and the reaction was carried out at 60 ° C for 3.5 h. After the reaction was completed, it was filtered, washed and dried to obtain amino biochar; then 100 g amino biochar was added to 1000 mL dimethylformamide, and then 13 g 2-mercaptonicotinic acid and 45 g triethylamine were added, and the reaction was carried out at 85 ° C for 2.5 h. After the reaction was completed, it was filtered, washed and dried to obtain modified biochar;

[0062] S4. Coating: adjust the inclination angle of the drum granulator disc to 55°, adjust the heating device to 45°C, place 1000g of calcium peroxide composite particles in the drum granulator, place 150g of modified biochar as the coating material in the vibrating feeder, feed them at a uniform speed, and use a water mist spray gun to continuously spray water mist on the rising part of the particles until the coating is completed. Dry at 90°C for 4h to obtain the soil slow-release repair agent.

[0063] Comparative Example 2

[0064] A preparation process of a slow-release repair agent for paddy field soil contaminated by cadmium and arsenic, comprising the following steps:

[0065] S1. Preparation of modified diatomite: 100 g of diatomite was added to 1100 g of 7% sodium hydroxide solution, and immersed at 75° C. for 1.5 h. After the immersion, 180 g of 10% manganese chloride solution was added, and stirred for 1.5 h. The mixture was then filtered, washed, dried, and calcined at 400° C. for 2.5 h to obtain pretreated diatomite. 100 g of pretreated diatomite was added to 1500 mL of ethanol aqueous solution (the volume ratio of ethanol to water was 3:1), then add 13g of vinyl triethoxysilane, stir and react at 55°C for 4.5h, filter, wash and dry after the reaction is completed to obtain diatomaceous earth containing double bonds; add 100g of diatomaceous earth containing double bonds to 1000mL of dimethylformamide, then add 15g of polyethylene glycol methacrylate phosphate and 0.8g of azobisisobutyronitrile, and react at a constant temperature of 55°C for 4.5h. After the reaction is completed, filter, wash and dry to obtain modified diatomaceous earth;

[0066] S2, mixed granulation: the disc inclination angle of the disc granulator is adjusted to 60°, and the heating device is adjusted to 50°C; 750g of calcium peroxide powder and 250g of modified diatomaceous earth are mixed evenly to obtain a mixed powder, which is put into the disc of the disc granulator, and the speed of the disc granulator is adjusted to 30r / min. According to the granulation situation, a water mist spray gun is used to continuously spray water mist at the rising part of the powder, and particles with a diameter of 3-5mm and smooth surface are continuously screened out, and the mixed powder is continuously added until the granulation is completed to obtain calcium peroxide composite particles;

[0067] S3. Preparation of modified biochar: 130 g corn cobs were crushed and added into 900 g of 7% sodium hydroxide solution, stirred and immersed at room temperature for 4 h, filtered and dried after immersion, calcined at 400 °C for 3 h, and then ground through a 150 mesh sieve to obtain modified biochar;

[0068] S4. Coating: adjust the inclination angle of the drum granulator disc to 55°, adjust the heating device to 45°C, place 1000g of calcium peroxide composite particles in the drum granulator, place 150g of modified biochar as the coating material in the vibrating feeder, feed them at a uniform speed, and use a water mist spray gun to continuously spray water mist on the rising part of the particles until the coating is completed. Dry at 90°C for 4h to obtain the soil slow-release repair agent.

[0069] The soil slow-release repair agent prepared by Example 1-3 and Comparative Example 1-2 was tested, and the slow-release performance of the slow-release repair agent was evaluated by the water dissolution method, that is, about 3g of the slow-release repair agent particles were weighed, placed in a homemade 300-mesh filter bag, the filter bag was placed in a 250mL ground-mouth conical flask, 250mL of distilled water was added, and the conical flask was placed in a 25°C constant temperature incubator for cultivation. The entire extract was extracted on the 1st, 2nd, 3rd, 4th, 7th, 10th, 14th, 21st day of cultivation, and every 7 days thereafter until 140d. After the extract was extracted, 250mL of distilled water was added to the conical flask, and the cultivation and extraction were continued. After the extract was fully mixed and allowed to stand, the content of dissolved active oxygen in the filtrate was determined, and a curve of the relationship between the amount of active oxygen dissolved and the immersion time was drawn. Each group of experiments was repeated 3 times for parallel determination. Strictly follow the HQ30d portable dissolved oxygen meter operating specifications. It should be noted that the content of active oxygen in water is negatively correlated with temperature. Temperature has a great influence on the content of active oxygen in water. Therefore, cultivation and measurement must be carried out at 25°C. Test results are as follows Figure 1 .

[0070] Depend on Figure 1 It can be seen that the sustained-release repair agent prepared by the present invention has a long release time and a low amplitude of active oxygen, the effective oxygen release time is as long as 130 days, and the changes during the entire extraction period are very stable, and it can play a role in the entire growth period of rice.

[0071] The sustained-release repair agents prepared in Examples 1-3 and Comparative Examples 1-2 were subjected to an effect verification experiment using a rice pot experiment. The pot soil samples were collected from a paddy field in Xiangtan County that was contaminated with cadmium and arsenic. The basic physical and chemical properties of the soil are shown in Table 1.

[0072] Table 1 Physical and chemical properties of potting soil samples

[0073]

[0074] The experiment set up 6 treatments: 1) Blank group: conventional fertilizer + no slow-release repair agent; 2) Example 1 group: conventional fertilizer + slow-release repair agent in Example 1; 3) Example 2 group: conventional fertilizer + slow-release repair agent in Example 2; 4) Example 3 group: conventional fertilizer + slow-release repair agent in Example 3; 5) Comparative Example 1 group: conventional fertilizer + slow-release repair agent in Comparative Example 1; 6) Comparative Example 2 group: conventional fertilizer + slow-release repair agent in Comparative Example 2. Each treatment was repeated 6 times, randomly arranged, and the position was changed from time to time. Three seedlings were planted in each pot, and protective rows were placed around the test area. The culture soil should not be dried and crushed, but directly mixed and put into a plastic bucket, and each pot was placed with 7kg of wet soil. The rice season is late rice, and the rice variety is late rice Jinyou 59 variety. The test pots use plastic buckets of the same size, with a bottom diameter of 25cm, a height of 30cm, and a barrel mouth diameter of 35cm. The fertilizer for potted plant test is calculated as N-P2O5-K2O=0.25-0.15-0.25g / kg soil, and the fertilizer is applied once. According to the results of the previous cultivation test, the slow-release repair agent is mixed with the soil for potted plant test at 0.3% of the soil mass.

[0075] During the rice harvest period, three pots of rice with similar growth and yield were selected from each treatment for soil and plant sampling. The effective cadmium and effective arsenic contents in the soil were determined, and the cadmium and arsenic contents in the rice were determined.

[0076] Depend on Figure 2 , Figure 3 It can be seen that the sustained-release repair agent prepared by the present invention is applied to cadmium-arsenic composite contaminated soil, and the cadmium content in rice is reduced to 0.092 mg / kg, and the arsenic content is reduced to 0.042 mg / kg, which significantly reduces the cadmium and arsenic contents in rice.

[0077] Depend on Figure 4 , Figure 5 It can be seen that after applying the slow-release repair agent prepared by the present invention, the effective cadmium content in the soil dropped to 0.173 mg / kg, and the effective arsenic content dropped to 0.182 mg / kg, which significantly reduced the effective cadmium and effective arsenic contents in the soil.

[0078] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A preparation process for a slow-release repair agent for paddy field soil contaminated by cadmium and arsenic, characterized in that: The following steps are involved: S1. Preparation of modified diatomite: adding pretreated diatomite to an ethanol aqueous solution, then adding vinyl triethoxysilane, stirring to react, filtering, washing, and drying after the reaction is completed to obtain diatomite containing double bonds; adding diatomite containing double bonds to dimethylformamide, then adding polyethylene glycol methacrylate phosphate and azobisisobutyronitrile, reacting at a constant temperature, filtering, washing, and drying after the reaction is completed to obtain modified diatomite; S2, mixing and granulating: by weight, 70-80 parts of calcium peroxide powder and 20-30 parts of the modified diatomaceous earth in step S1 are mixed evenly, and then granulated to obtain calcium peroxide composite particles; S3, preparation of modified biochar: adding the pretreated biochar to an ethanol aqueous solution, then adding γ-aminopropyltriethoxysilane, heating reaction, filtering, washing, and drying after the reaction is completed to obtain amination biochar; then adding the amination biochar to dimethylformamide, then adding 2-mercaptonicotinic acid and triethylamine, stirring reaction, filtering, washing, and drying after the reaction is completed to obtain modified biochar; S4, coating: using the modified biochar in step S3 as a coating material, coating the calcium peroxide composite particles in step S2, and obtaining a soil slow-release repair agent after drying; The specific method for pretreating diatomite in step S1 is as follows: by weight, 100 parts of diatomite are added to 1000-1200 parts of a 5-8% sodium hydroxide solution, and immersed at 70-80° C. for 1-2 hours. After the immersion is completed, 150-200 parts of a 10-15% manganese chloride solution are added, stirred for 1-2 hours, and then filtered, washed, dried, and calcined at 350-450° C. for 2-3 hours to obtain pretreated diatomite; The specific preparation method of the pretreated biochar described in step S3 is as follows: by weight, 100-150 parts of corn cobs are crushed and added to 800-1000 parts of a sodium hydroxide solution with a mass fraction of 5-8%, stirred and immersed for 3-5 hours at room temperature, and then 200-300 parts of a 10-15% ferric nitrate solution are added, and aged at 40-50°C for 12-16 hours. After aging, it is filtered and dried, calcined at 350-450°C for 2-4 hours, and ground to obtain pretreated biochar.

2. The preparation process according to claim 1, characterized in that: In step S1, the volume ratio of ethanol to water in the ethanol aqueous solution is 3:1, the mass ratio of the pretreated diatomaceous earth and vinyl triethoxysilane is 100:10-15, the temperature of the stirring reaction is 50-60°C, and the time is 4-5h; the mass ratio of the double-bond-containing diatomaceous earth, polyethylene glycol methacrylate phosphate, and azobisisobutyronitrile is 100:12-17:0.5-1, the temperature of the isothermal reaction is 90-100°C, and the time is 2-3h.

3. The preparation process according to claim 1, characterized in that: The specific method of granulation in step S2 is: adjusting the inclination angle of the disc of the disc granulator to 50-65°, and adjusting the heating device to 40-55°C; mixing the calcium peroxide powder and the modified diatomaceous earth evenly to obtain a mixed powder, putting it into the disc of the disc granulator, adjusting the speed of the disc granulator to 20-40r / min, and according to the granulation situation, using a water mist spray gun to continuously spray water mist at the rising part of the powder, and continuously screening out particles with a diameter of 3-5mm and smooth surface, and continuously adding the mixed powder until the granulation is completed.

4. The preparation process according to claim 1, characterized in that: The volume ratio of ethanol to water in the ethanol aqueous solution in step S3 is 3:1, the mass ratio of the pretreated biochar and γ-aminopropyltriethoxysilane is 100:10-15, the temperature of the heating reaction is 55-65°C, and the time is 3-4h.

5. The preparation process according to claim 1, characterized in that: In step S3, the mass ratio of the aminated biochar, 2-mercaptonicotinic acid, and triethylamine is 100:10-15:40-50, the stirring reaction temperature is 75-85° C., and the reaction time is 2-3 h.

6. The preparation process according to claim 1, characterized in that: The specific steps of the coating treatment in step S4 are as follows: adjust the inclination angle of the disc of the disc granulator to 55-60°, adjust the heating device to 45-50°C, place 100 parts of calcium peroxide composite particles in the disc granulator, place 10-20 parts of modified biochar as a coating material in a vibrating feeder, add them at a uniform speed, and use a water mist spray gun to continuously spray water mist at the rising part of the particles until the coating is completed, and dry them at 80-100°C for 3-5h.

7. A slow-release repair agent for paddy field soil contaminated with cadmium and arsenic prepared by the process described in any one of claims 1 to 6.

8. An application of the slow-release repair agent for paddy field soil contaminated by cadmium and arsenic as claimed in claim 7, characterized in that: The cadmium-arsenic composite contaminated paddy field soil slow-release repair agent is added to the contaminated soil at 0.1-1% of the soil mass.