A method for recycling environmentally friendly solid waste

By drying, dehydrating, membrane separation and combustion of solid waste, combining the mixing and stirring of mineral impurities and furnace ash, concrete with high strength and good stability is produced, which solves the problem of low resource utilization efficiency of solid waste and achieves the Efficient and environmentally friendly resource utilization.

CN118328400BActive Publication Date: 2024-11-29EDSONBURG NEW MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410507957.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2024-11-29
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

The existing solid waste treatment methods are inefficient in the resource utilization of solid waste, resulting in serious resource waste.

Method used

Emulsified oil mixture was obtained by drying, dehydrating, and membrane separation. Mineral impurities were obtained by sorting, screening and crushing, and they were obtained with furnace ash, emulsified oil mixture, titanium dioxide, water, diatomaceous earth, graphite fiber, glass fiber, cement , quicklime, defoaming agent and water reducing agent are mixed and stirred to produce concrete with high strength and good stability.

Benefits of technology

It improves the resource utilization rate of solid waste, produces concrete with high strength and good stability, and is environmentally friendly and efficient.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention is applicable to the technical field of solid waste treatment, and provides an environmentally friendly solid waste resource utilization method, comprising the following steps: step (1), drying and dehydrating the solid waste, and separating the waste liquid through a membrane to obtain an emulsified oil mixture; step (2), sorting and screening out mineral impurities in the solid waste, crushing, and setting aside; step (3), adding the solid waste to a combustion furnace, burning, collecting the ash generated after the combustion, recovering the heat generated by the combustion, and discharging the combustion tail gas after treatment; step (4), adding the mineral impurities, ash, and emulsified oil mixture to a mixing container in proportion, and then adding titanium dioxide, water, diatomaceous earth, graphite fiber, glass fiber, cement, quicklime, defoamer, and water reducer to mix and stir to obtain concrete. The concrete obtained by the present invention has high strength, good stability, and durability, and greatly improves the resource utilization of solid waste, and is environmentally friendly and efficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste treatment, in particular to an environmentally friendly solid waste resource utilization method. Background Art

[0002] Solid waste refers to solid waste and pollutants generated by life, industry, agriculture and other activities, including but not limited to waste paper, waste plastic, waste metal, waste glass, waste wood, waste food, construction waste, etc. There are many ways to classify solid waste. According to its composition, it can be divided into organic waste and inorganic waste; according to its form, it can be divided into solid waste, semi-solid waste and liquid (gaseous) waste; according to its pollution characteristics, it can be divided into hazardous waste and general waste, etc.; according to its source, it can be divided into mining, industrial, urban life, agricultural and radioactive.

[0003] Most of the existing solid waste is treated through landfill, combustion, gasification and other methods. These treatment methods have low efficiency in resource utilization of solid waste and cause serious waste of resources. Summary of the invention

[0004] The purpose of the present invention is to provide an environmentally friendly solid waste resource utilization method to solve the problem of low resource utilization efficiency of solid waste in existing solid waste treatment methods in the prior art.

[0005] To achieve the above object, the present invention provides the following technical solution: an environmentally friendly solid waste resource utilization method, comprising the following steps:

[0006] Step (1), drying and dehydrating the solid waste, and separating the waste liquid through a membrane to obtain an emulsified oil mixture;

[0007] Step (2), sorting and screening out mineral impurities in the solid waste, crushing and setting aside;

[0008] Step (3), adding solid waste into a combustion furnace, burning, collecting the ash generated after the combustion, recovering the heat generated by the combustion, and treating the exhaust gas from the combustion before discharging;

[0009] Step (4), adding the mineral impurities, furnace ash, and emulsified oil mixture into a mixing container in proportion, and then adding titanium dioxide, water, diatomaceous earth, graphite fiber, glass fiber, cement, quicklime, defoamer, and water reducing agent to mix and stir to obtain concrete.

[0010] Preferably, the membrane material used for the membrane separation is an ultrafiltration membrane, and the temperature of the membrane separation is 35°C to 40°C.

[0011] Preferably, the moisture content of the dehydrated solid waste is ≤3%.

[0012] Preferably, the particle size of the mineral impurities is 3 to 8 mm.

[0013] Preferably, the contents of each component in the concrete are as follows, in parts by mass:

[0014] 5-9 parts of mineral impurities, 8-14 parts of furnace ash, 1.2-1.9 parts of emulsified oil mixture, 1-3 parts of titanium dioxide, 10-15 parts of water, 1-2 parts of diatomaceous earth, 2-6 parts of graphite fiber, 1-3 parts of glass fiber, 32-54 parts of cement, 3-7 parts of quicklime, 0.5-1.4 parts of defoaming agent and 1-1.6 parts of water reducing agent.

[0015] Preferably, the content ratio of the graphite fiber to the glass fiber is 2:1.

[0016] Preferably, the water reducing agent is lignin sulfonate or naphthalene sulfonate, and the defoaming agent is polysiloxane.

[0017] The present invention has at least the following beneficial effects:

[0018] The present invention provides an environmentally friendly solid waste resource utilization method, which obtains an emulsified oil mixture through dehydration and membrane separation, obtains mineral impurities through sorting, screening and crushing, obtains furnace ash through burning solid waste, and mixes the mineral impurities, furnace ash and emulsified oil mixture with titanium dioxide, water, diatomaceous earth, graphite fiber, glass fiber, cement, quicklime, defoaming agent and water reducing agent to obtain concrete. The obtained concrete has high strength, good stability and durability, and greatly improves the resource utilization of solid waste, is environmentally friendly and efficient. DETAILED DESCRIPTION

[0019] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] Example 1

[0021] An environmentally friendly solid waste resource utilization method comprises the following steps:

[0022] Step (1), drying and dehydrating the solid waste until the water content of the solid waste is ≤3%, and performing membrane separation on the waste liquid using an ultrafiltration membrane at a temperature of 35° C. to obtain an emulsified oil mixture;

[0023] Step (2), sorting and screening out mineral impurities in the solid waste, and crushing the mineral impurities to a particle size of 3 to 8 mm for later use;

[0024] Step (3), adding solid waste into a combustion furnace, burning, collecting the ash generated after the combustion, recovering the heat generated by the combustion, and treating the exhaust gas from the combustion before discharging;

[0025] Step (4), adding the mixture of mineral impurities, furnace ash and emulsified oil into a mixing container in proportion, and then adding titanium dioxide, water, diatomaceous earth, graphite fiber, glass fiber, cement, quicklime, defoamer and water reducing agent to mix and stir to prepare concrete;

[0026] The contents of each component in concrete are as follows in terms of mass:

[0027] 5 parts of mineral impurities, 8 parts of furnace ash, 1.2 parts of emulsified oil mixture, 1 part of titanium dioxide, 10 parts of water, 1 part of diatomaceous earth, 2 parts of graphite fiber, 1 part of glass fiber, 32 parts of cement, 3 parts of quicklime, 0.5 parts of defoamer and 1 part of water reducer;

[0028] The content ratio of graphite fiber to glass fiber is 2:1; the water reducer is lignin sulfonate, and the defoamer is polysiloxane.

[0029] Example 2

[0030] An environmentally friendly solid waste resource utilization method comprises the following steps:

[0031] Step (1), drying and dehydrating the solid waste until the water content of the solid waste is ≤3%, and performing membrane separation on the waste liquid using an ultrafiltration membrane at a temperature of 38° C. to obtain an emulsified oil mixture;

[0032] Step (2), sorting and screening out mineral impurities in the solid waste, and crushing the mineral impurities to a particle size of 3 to 8 mm for later use;

[0033] Step (3), adding solid waste into a combustion furnace, burning, collecting the ash generated after the combustion, recovering the heat generated by the combustion, and treating the exhaust gas from the combustion before discharging;

[0034] Step (4), adding the mixture of mineral impurities, furnace ash and emulsified oil into a mixing container in proportion, and then adding titanium dioxide, water, diatomaceous earth, graphite fiber, glass fiber, cement, quicklime, defoamer and water reducing agent to mix and stir to prepare concrete;

[0035] The contents of each component in concrete are as follows in terms of mass:

[0036] 8 parts of mineral impurities, 12 parts of furnace ash, 1.7 parts of emulsified oil mixture, 2.1 parts of titanium dioxide, 12 parts of water, 1.6 parts of diatomaceous earth, 5 parts of graphite fiber, 2.5 parts of glass fiber, 46 parts of cement, 5 parts of quicklime, 1.2 parts of defoamer and 1.5 parts of water reducer;

[0037] The content ratio of graphite fiber to glass fiber is 2:1; the water reducer is naphthalenesulfonate, and the defoamer is polysiloxane.

[0038] Example 3

[0039] An environmentally friendly solid waste resource utilization method comprises the following steps:

[0040] Step (1), drying and dehydrating the solid waste until the water content of the solid waste is ≤3%, and performing membrane separation on the waste liquid using an ultrafiltration membrane at a temperature of 40° C. to obtain an emulsified oil mixture;

[0041] Step (2), sorting and screening out mineral impurities in the solid waste, and crushing the mineral impurities to a particle size of 3 to 8 mm for later use;

[0042] Step (3), adding solid waste into a combustion furnace, burning, collecting the ash generated after the combustion, recovering the heat generated by the combustion, and treating the exhaust gas from the combustion before discharging;

[0043] Step (4), adding the mixture of mineral impurities, furnace ash and emulsified oil into a mixing container in proportion, and then adding titanium dioxide, water, diatomaceous earth, graphite fiber, glass fiber, cement, quicklime, defoamer and water reducing agent to mix and stir to prepare concrete;

[0044] The contents of each component in concrete are as follows in terms of mass:

[0045] 9 parts of mineral impurities, 14 parts of furnace ash, 1.9 parts of emulsified oil mixture, 3 parts of titanium dioxide, 15 parts of water, 2 parts of diatomaceous earth, 6 parts of graphite fiber, 3 parts of glass fiber, 54 parts of cement, 7 parts of quicklime, 1.4 parts of defoamer and 1.6 parts of water reducer;

[0046] The content ratio of graphite fiber to glass fiber is 2:1; the water reducer is lignin sulfonate, and the defoamer is polysiloxane.

[0047] The present invention processes solid waste to obtain a mixture of mineral impurities, furnace ash and emulsified oil in proportion, and mixes the mixture with titanium dioxide, water, diatomaceous earth, graphite fiber, glass fiber, cement, quicklime, defoamer and water reducer to obtain concrete with high strength, good stability and durability.

[0048] The above shows and describes the basic principles, main features and advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and that the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.

[0049] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for recycling environmentally friendly solid waste, characterized in that: The following steps are involved: Step (1), drying and dehydrating the solid waste, and separating the waste liquid through a membrane to obtain an emulsified oil mixture; Step (2), sorting and screening out mineral impurities in the solid waste, crushing and setting aside; Step (3), adding solid waste into a combustion furnace, burning, collecting the ash generated after the combustion, recovering the heat generated by the combustion, and treating the exhaust gas from the combustion before discharging; Step (4), adding the mixture of mineral impurities, furnace ash and emulsified oil into a mixing container in proportion, and then adding titanium dioxide, water, diatomaceous earth, graphite fiber, glass fiber, cement, quicklime, defoamer and water reducing agent to mix and stir to prepare concrete; The contents of each component in concrete are as follows in terms of mass: 5-9 parts of mineral impurities, 8-14 parts of furnace ash, 1.2-1.9 parts of emulsified oil mixture, 1-3 parts of titanium dioxide, 10-15 parts of water, 1-2 parts of diatomaceous earth, 2-6 parts of graphite fiber, 1-3 parts of glass fiber, 32-54 parts of cement, 3-7 parts of quicklime, 0.5-1.4 parts of defoaming agent and 1-1.6 parts of water reducing agent.

2. The method for recycling environmentally friendly solid waste according to claim 1, characterized in that: The membrane material used for the membrane separation is an ultrafiltration membrane, and the temperature of the membrane separation is 35°C to 40°C.

3. The method for recycling environmentally friendly solid waste according to claim 1, characterized in that: The moisture content of the dehydrated solid waste is ≤3%.

4. The method for recycling environmentally friendly solid waste according to claim 1, characterized in that: The particle size of the mineral impurities is 3 to 8 mm.

5. The method for recycling environmentally friendly solid waste according to claim 1, characterized in that: The content ratio of the graphite fiber to the glass fiber is 2:

1.

6. The method for recycling environmentally friendly solid waste according to claim 1, characterized in that: The water reducing agent is lignin sulfonate or naphthalene sulfonate, and the defoaming agent is polysiloxane.

Citation Information

Patent Citations

  • Ecological hollow building block and preparation method

    CN111892366A

  • Process for producing cement by comprehensively utilizing solid wastes and preparation device thereof

    CN116003003A