Light emitting diode and method for preparing light emitting diode
By designing the pad overlaps with the edge of the reflective layer, the gap is eliminated, and the miniaturization of the micro-light emitting diode is achieved, which solves the problem of larger size in the prior art and improves electrical performance.
Patent Information
- Application Number
- CN202410735946.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-06-07
AI Technical Summary
The existing micro-light emitting diodes have a large size due to the gap between the pad and the reflective layer, making it difficult to achieve a miniaturized design.
By designing the pad overlaps with the edges of the reflective layer, the gap is eliminated, and the pad design in rectangular or other shapes is used to facilitate the graphic processing, forming a step structure and covering the passivation layer to reduce size.
The light emitting diode is smaller in size and is suitable for miniaturization design. The overlap between the pad and the edge of the reflective layer eliminates gaps and improves electrical performance.
Smart Images

Figure CN118335877B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of light-emitting devices, and in particular to a light-emitting diode and a method for preparing the light-emitting diode. Background Art
[0002] Light-emitting diodes can cover the wavelength range from ultraviolet to infrared. At present, the low-resolution display market is still dominated by liquid crystal displays (LCD), and micro light-emitting diodes (Micro LED) are gradually gaining attention in the low-resolution display market due to their own advantages.
[0003] The micro light emitting diode provided by the related technology generally includes an epitaxial structure, an electrode, a reflective layer, a pad, and the like.
[0004] However, the micro light emitting diodes provided by the related art still have the problem of being large in size. Summary of the invention
[0005] The embodiments of the present disclosure provide a light emitting diode and a method for manufacturing the light emitting diode, which is conducive to the miniaturization design of the light emitting diode. The technical solution is as follows:
[0006] In one aspect, a light emitting diode is provided, the light emitting diode comprising: an epitaxial structure, a first electrode, a second electrode, a reflective layer, a first electrode pad, and a second electrode pad;
[0007] The epitaxial structure comprises a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence, wherein the first semiconductor layer, the active layer, and the second semiconductor layer form a step structure, the first electrode is located on a step surface of the step structure, the second electrode is located on a surface of the second semiconductor layer, the reflective layer covers the step structure and the first electrode and the second electrode, the first electrode pad penetrates the reflective layer and is connected to the first electrode, and the second electrode pad penetrates the reflective layer and is connected to the second electrode;
[0008] A projection of the reflective layer on the first semiconductor layer coincides with the first semiconductor layer, and edges of projections of the first electrode pad and the second electrode pad on the first semiconductor layer coincide with edges of a projection of the reflective layer on the first semiconductor layer.
[0009] Optionally, the projection of the reflective layer on the first semiconductor layer is a first rectangle, the projections of the first electrode pad and the second electrode pad on the first semiconductor layer are second rectangles, and three sides of each of the second rectangles coincide with three sides of the first rectangle.
[0010] Optionally, the length of the second rectangle is 20-30 μm, and the width of the second rectangle is 10-15 μm.
[0011] Optionally, the light emitting diode further includes: a passivation layer, the passivation layer covers the epitaxial structure, the reflective layer and the side walls of the first electrode pad and the second electrode pad, and the passivation layer also covers the spacing area between the first electrode pad and the second electrode pad.
[0012] Optionally, the light emitting diode further comprises: a substrate and a bonding layer;
[0013] The first semiconductor layer is bonded to the substrate via the bonding layer.
[0014] In another aspect, a method for preparing a light emitting diode is provided, the method comprising:
[0015] forming a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence, wherein the second semiconductor layer, the active layer, and the first semiconductor layer constitute an epitaxial structure;
[0016] Performing a patterning process on the epitaxial structure to form a step structure;
[0017] Manufacturing a first electrode and a second electrode, wherein the first electrode is located on a step surface of the step structure, and the second electrode is located on a surface of the second semiconductor layer;
[0018] Manufacturing a reflective layer, wherein the reflective layer covers the step structure and the first electrode and the second electrode;
[0019] A first electrode pad and a second electrode pad are manufactured, wherein the first electrode pad passes through the reflective layer and is connected to the first electrode, and the second electrode pad passes through the reflective layer and is connected to the second electrode; a projection of the reflective layer on the first semiconductor layer overlaps with the first semiconductor layer, and edges of the projections of the first electrode pad and the second electrode pad on the first semiconductor layer overlap with edges of the projection of the reflective layer on the first semiconductor layer.
[0020] Optionally, the manufacturing of the first electrode pad and the second electrode pad includes:
[0021] depositing a metal stack;
[0022] forming a first photoresist mask layer on the metal stack;
[0023] Under the shielding of the first photoresist mask layer, patterning the metal stack, the reflective layer and the epitaxial structure so that the projections of the metal stack and the reflective layer on the first semiconductor layer overlap with the first semiconductor layer;
[0024] removing the first photoresist mask layer;
[0025] Making a second photoresist mask layer on the metal stack, wherein the middle portion of the second photoresist mask layer is hollowed out;
[0026] Under the shielding of the second photoresist mask layer, patterning the metal stack so that the metal stack is separated from the middle to obtain the first electrode pad and the second electrode pad;
[0027] The second photoresist mask layer is removed.
[0028] Optionally, the projection of the reflective layer on the first semiconductor layer is a first rectangle, the projections of the first electrode pad and the second electrode pad on the first semiconductor layer are second rectangles, and three sides of each of the second rectangles coincide with three sides of the first rectangle.
[0029] Optionally, the length of the second rectangle is 20-30 μm, and the width of the second rectangle is 10-15 μm.
[0030] Optionally, the light emitting diode preparation method further includes:
[0031] A passivation layer is manufactured, wherein the passivation layer covers the epitaxial structure, the reflective layer, and the side walls of the first electrode pad and the second electrode pad, and the passivation layer also covers the spacing area between the first electrode pad and the second electrode pad.
[0032] The technical solution provided by the embodiments of the present disclosure has the following beneficial effects:
[0033] In the embodiment of the present disclosure, the edges of the first electrode pad and the second electrode pad of the light-emitting diode coincide with the edges of the reflective layer, eliminating the gap between the edges of the first electrode pad and the second electrode pad and the edges of the reflective layer in the related art, thereby making the size of the light-emitting diode smaller and facilitating miniaturized design. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0035] Figure 1 It is a structural schematic diagram of a light emitting diode provided by the related technology;
[0036] Figure 2It is a top view of a light emitting diode provided by the related technology;
[0037] Figure 3 is a structural schematic diagram of a light emitting diode provided by an embodiment of the present disclosure;
[0038] Figure 4 is a top view of a light emitting diode provided by an embodiment of the present disclosure;
[0039] Figure 5 is a flow chart of a method for preparing a light emitting diode provided by an embodiment of the present disclosure;
[0040] Figure 6 This is a flow chart of another method for preparing a light emitting diode provided in an embodiment of the present disclosure.
[0041] The reference numerals are as follows:
[0042] 10: electrode structure; 100: substrate; 101: first semiconductor layer; 102: active layer; 103: second semiconductor layer; 104: bonding layer; 105: first electrode; 106: second electrode; 107: reflective layer; 108: first electrode pad; 109: second electrode pad; 110: passivation layer; 111: first through hole; 112: second through hole; 120: step surface of step structure; 1000: epitaxial structure. DETAILED DESCRIPTION
[0043] In order to make the objectives, technical solutions and advantages of the present disclosure more clear, the embodiments of the present disclosure will be further described in detail below with reference to the accompanying drawings.
[0044] Figure 1 A schematic diagram of the structure of a light emitting diode provided for related technology. Figure 1 The light emitting diode comprises: a substrate 100 , an epitaxial structure 1000 , a bonding layer 104 , a reflective layer 107 , a passivation layer 110 and an electrode structure 10 .
[0045] The epitaxial structure 1000 includes a first semiconductor layer 101 , an active layer 102 , and a second semiconductor layer 103 . The electrode structure 10 includes a first electrode 105 , a second electrode 106 , a first electrode pad 108 , and a second electrode pad 109 .
[0046] The substrate 100 is bonded to the epitaxial structure 1000 via a bonding layer 104 , the reflective layer 107 covers the surface of the epitaxial structure 1000 , the electrode structure 10 penetrates the reflective layer 107 and is connected to the epitaxial structure 1000 , and the passivation layer 110 covers the surface of the reflective layer 107 .
[0047] Figure 2 This is a top view of a light emitting diode provided by the related art, see Figure 2It can be seen that there is a certain gap between the edge of the first electrode pad 108 (the second electrode pad 109 ) and the edge of the reflective layer 107 . This gap causes the overall size of the light-emitting diode to be large, which is not conducive to miniaturization.
[0048] An embodiment of the present disclosure provides a light emitting diode, which includes: an epitaxial structure, a first electrode, a second electrode, a reflective layer, a first electrode pad, and a second electrode pad.
[0049] The epitaxial structure includes a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence, wherein the first semiconductor layer, the active layer, and the second semiconductor layer form a step structure, the first electrode is located on the step surface of the step structure, the second electrode is located on the surface of the second semiconductor layer, the reflective layer covers the step structure and the first electrode and the second electrode, the first electrode pad penetrates the reflective layer and is connected to the first electrode, and the second electrode pad penetrates the reflective layer and is connected to the second electrode.
[0050] A projection of the reflective layer on the first semiconductor layer coincides with the first semiconductor layer, and edges of projections of the first electrode pad and the second electrode pad on the first semiconductor layer coincide with edges of a projection of the reflective layer on the first semiconductor layer.
[0051] In the embodiment of the present disclosure, the edges of the first electrode pad and the second electrode pad of the light-emitting diode coincide with the edges of the reflective layer, eliminating the gap between the edges of the first electrode pad and the second electrode pad and the edges of the reflective layer in the related art, thereby making the size of the light-emitting diode smaller and facilitating miniaturized design.
[0052] Figure 3 A schematic diagram of the structure of a light emitting diode provided by an embodiment of the present disclosure. Figure 3 The light emitting diode comprises: a substrate 100 , an epitaxial structure 1000 , a bonding layer 104 , a reflective layer 107 and an electrode structure 10 .
[0053] The substrate 100 is bonded to the epitaxial structure 1000 via a bonding layer 104 , and the electrode structure 10 penetrates the reflective layer 107 and is connected to the epitaxial structure 1000 .
[0054] In the embodiment of the present disclosure, the epitaxial structure 1000 includes a first semiconductor layer 101, an active layer 102, and a second semiconductor layer 103 stacked in sequence, and the first semiconductor layer 101, the active layer 102, and the second semiconductor layer 103 form a step structure; the first electrode 105 is located on the step surface 120 of the step structure, and the second electrode 106 is located on the surface of the second semiconductor layer 103, the reflective layer 107 covers the step structure and the first electrode 105 and the second electrode 106, the first electrode pad 108 penetrates the reflective layer 107 and is connected to the first electrode 105, and the second electrode pad 109 penetrates the reflective layer 107 and is connected to the second electrode 106.
[0055] Figure 4 is a top view of a light emitting diode provided by an embodiment of the present disclosure. Figure 3 and Figure 4 It can be seen that the reflective layer 107 is on the first semiconductor layer 101 ( Figure 4 The projection of the first electrode pad 108 and the second electrode pad 109 on the first semiconductor layer 101 coincides with the edge of the projection of the reflective layer 107 on the first semiconductor layer 101.
[0056] In the embodiment of the present disclosure, the edges of the first electrode pad and the second electrode pad of the light-emitting diode coincide with the edges of the reflective layer, so that the size of the light-emitting diode can be designed to be smaller, which is conducive to the miniaturized design of the light-emitting diode.
[0057] like Figure 4 As shown, the projection of the reflective layer 107 on the first semiconductor layer 101 is a first rectangle, and the projections of the first electrode pad 108 and the second electrode pad 109 on the first semiconductor layer 101 are a second rectangle, and the three sides of each of the second rectangles coincide with the three sides of the first rectangle. In this implementation, the pads are designed in a rectangular shape so that the sides of the pads coincide with the sides of the reflective layer, which is convenient for patterning and mask design.
[0058] In this implementation, the length of the second rectangle is 20-30 μm, and the width of the second rectangle is 10-15 μm. The pad of this size can meet the electrical performance of the light-emitting diode and is conducive to miniaturization.
[0059] Exemplarily, the length of the second rectangle is 30 μm, and the width of the second rectangle is 15 μm.
[0060] In other implementations, the projection of the reflective layer 107 on the first semiconductor layer 101 is a first rectangle, and the projections of the first electrode pad 108 and the second electrode pad 109 on the first semiconductor layer 101 may not be rectangles, for example, a figure with three sides being rectangles and the other side being an arc.
[0061] Alternatively, in other implementations, the projection of the reflective layer 107 on the first semiconductor layer 101 is not a rectangle, and the projections of the first electrode pad 108 and the second electrode pad 109 on the first semiconductor layer 101 correspond to the projection shape of the reflective layer 107 on the first semiconductor layer 101, that is, the edges overlap.
[0062] In the embodiment of the present disclosure, the substrate 100 may be any one of a sapphire substrate, a Si substrate, a SiC substrate, etc., and the present disclosure does not limit the material of the substrate.
[0063] Exemplarily, the substrate 100 is a sapphire substrate.
[0064] In the embodiment of the present disclosure, the first semiconductor layer 101 may be an N-type semiconductor layer, and the second semiconductor layer 103 may be a P-type semiconductor layer.
[0065] For example, the first semiconductor layer 101 may include a stacked N-type AlGaInP current spreading layer and an N-type AlInP carrier confinement layer, and the second semiconductor layer 103 may include a stacked P-type AlInP carrier confinement layer and a P-type GaP window layer.
[0066] The thickness of the P-type GaP window layer is 2.8-3.2 μm, for example, 3 μm.
[0067] In another example, the first semiconductor layer 101 may be a P-type semiconductor layer, and the second semiconductor layer 103 may be an N-type semiconductor layer.
[0068] In the embodiment of the present disclosure, the active layer 102 may be a multi-quantum well layer. For example, the multi-quantum well layer may include a plurality of periodically alternately stacked AlGaInP quantum well layers and AlGaInP quantum barrier layers.
[0069] Optionally, a corrosion stop layer may be provided between the bonding layer 104 and the first semiconductor layer 101 , and the corrosion stop layer may be a solidified phosphoric acid mixture.
[0070] In the embodiment of the present disclosure, the material of the bonding layer 104 may be any one of photoresist, benzocyclobutene, and silica gel.
[0071] Exemplarily, the material of the bonding layer 104 is silica gel.
[0072] In the embodiment of the present disclosure, the first semiconductor layer 101 , the active layer 102 , and the second semiconductor layer 103 stacked in sequence form a step structure, and the reflective layer 107 covers the step structure.
[0073] In the embodiment of the present disclosure, the reflective layer 107 is a distributed Bragg reflector (DBR) layer.
[0074] In the embodiment of the present disclosure, both the first electrode 105 and the second electrode 106 may include AuGe or AuBe electrodes.
[0075] In the embodiment of the present disclosure, the first electrode pad 108 and the second electrode pad 109 may each include a Cr layer, an Al layer, a Ti layer, a Ni layer, and an Au alloy layer stacked in sequence.
[0076] In one example, the thickness of the Cr layer is 80-120 nm, the thickness of the Al layer is 2500-3500 nm, the thickness of the Ti layer is 450-550 nm, the thickness of the Ni layer is 1800-2200 nm, and the thickness of the Au alloy layer is 18000-22000 nm.
[0077] Exemplarily, the thickness of the Cr layer is 100 nm, the thickness of the Al layer is 3000 nm, the thickness of the Ti layer is 500 nm, the thickness of the Ni layer is 2000 nm, and the thickness of the Au alloy layer is 20000 nm.
[0078] In one example, the first electrode 105 is an N-electrode, and the first electrode pad 108 is an N-electrode pad; the second electrode 106 is a P-electrode, and the second electrode pad 109 is a P-electrode pad.
[0079] In another example, the first electrode 105 is a P-electrode, and the first electrode pad 108 is a P-electrode pad; the second electrode 106 is an N-electrode, and the second electrode pad 109 is an N-electrode pad.
[0080] Optionally, the light emitting diode may further include a passivation layer 110 , which covers the epitaxial structure 1000 , the reflective layer 107 , and the side walls of the first electrode pad 108 and the second electrode pad 109 , and the passivation layer 110 also covers the spacing area between the first electrode pad 108 and the second electrode pad 109 .
[0081] In the embodiment of the present disclosure, since the edge of the pad coincides with the edge of the reflective layer, the passivation layer only needs to cover the side walls of the epitaxial structure 1000, the reflective layer 107, the first electrode pad 108 and the second electrode pad 109, and the area between the first electrode pad 108 and the second electrode pad 109.
[0082] like Figure 3 As shown, in one example, the height of the passivation layer is the same as the height of the pad. In other examples, the height of the passivation layer can be lower than the height of the pad. The lower the height of the passivation layer, the thinner the thickness of the passivation layer at the side is, thereby achieving miniaturization of the light emitting diode.
[0083] In the embodiment of the present disclosure, the passivation layer 110 may be a film layer formed of materials such as a SiO 2 layer and an Al 2 O 3 layer.
[0084] For example, the passivation layer 110 is a SiO 2 layer.
[0085] In the embodiment of the present disclosure, the length of the portion of the passivation layer 110 located between the two pads is 20~30μm, for example 30μm; the width of the portion of the passivation layer 110 located between the two pads is 10~15μm, for example 12μm, that is, the distance between the two pads is 10~15μm.
[0086] In the disclosed embodiment, the thickness of the passivation layer 110 is 4000-6000 angstroms, for example, 5000 angstroms.
[0087] It is worth noting that in the embodiments of the present disclosure, structures may be selectively increased or decreased based on the structure of the above-mentioned light emitting diode, and the present disclosure does not impose any limitation on this.
[0088] Figure 5 A flow chart of a method for preparing a light emitting diode provided in an embodiment of the present disclosure. Figure 5 The method steps include:
[0089] S11, forming a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence, wherein the second semiconductor layer, the active layer, and the first semiconductor layer constitute an epitaxial structure.
[0090] S12, performing graphic processing on the epitaxial structure to form a step structure.
[0091] S13, manufacturing a first electrode and a second electrode, wherein the first electrode is located on a step surface of the step structure, and the second electrode is located on a surface of the second semiconductor layer.
[0092] S14, manufacturing a reflective layer, wherein the reflective layer covers the step structure and the first electrode and the second electrode.
[0093] S15. Make a first electrode pad and a second electrode pad, the first electrode pad penetrates the reflective layer and is connected to the first electrode, the second electrode pad penetrates the reflective layer and is connected to the second electrode; the projection of the reflective layer on the first semiconductor layer overlaps with the first semiconductor layer, and the edges of the projections of the first electrode pad and the second electrode pad on the first semiconductor layer overlap with the edges of the projection of the reflective layer on the first semiconductor layer.
[0094] In the embodiment of the present disclosure, the edges of the first electrode pad and the second electrode pad of the light-emitting diode coincide with the edges of the reflective layer, eliminating the gap between the edges of the first electrode pad and the second electrode pad and the edges of the reflective layer in the related art, thereby making the size of the light-emitting diode smaller and facilitating miniaturized design.
[0095] Figure 6 Another light emitting diode manufacturing method provided by the present disclosure is a flow chart. Figure 6 The method steps include:
[0096] S21. Bond the epitaxial structure to the substrate via a bonding layer.
[0097] In one example, step S21 includes:
[0098] Step 1: fabricating a first semiconductor layer, an active layer and a second semiconductor layer stacked in sequence on a surface of a first temporary substrate, that is, fabricating an epitaxial structure.
[0099] Wherein, the first temporary substrate is a gallium arsenide substrate.
[0100] In one example, step 1 includes:
[0101] The first step is to make the first semiconductor layer.
[0102] In the embodiment of the present disclosure, the first semiconductor layer includes an N-type AlGaInP current spreading layer and an N-type AlInP carrier confinement layer stacked in sequence.
[0103] Exemplarily, a Metal Organic Chemical Vapor Deposition (MOCVD) device is used to sequentially form an N-type AlGaInP current spreading layer and an N-type AlInP carrier confinement layer on the surface of the first temporary substrate.
[0104] In the disclosed embodiment, the growth of the semiconductor layer can be achieved by using Veeco K465i or C4 or RB MOCVD equipment or AIXTRON metal organic chemical vapor deposition equipment. High purity H2 (hydrogen) or high purity N2 (nitrogen) or a mixture of high purity H2 and high purity N2 is used as a carrier gas, high purity NH3 is used as an N source, trimethyl gallium (TMGa) and triethyl gallium (TEGa) are used as gallium sources, trimethyl indium (TMIn) is used as an indium source, silane (SiH4) is used as an N-type dopant, trimethyl aluminum (TMAl) is used as an aluminum source, and bis(cyclopentadienyl) magnesium (CP2Mg) is used as a P-type dopant.
[0105] Optionally, an etching stop layer may be formed between the first temporary substrate and the first semiconductor layer, and the etching medium layer is a solidified phosphoric acid mixture.
[0106] The second step is to make the active layer.
[0107] In the embodiment of the present disclosure, the active layer is a multi-quantum well layer, including a plurality of periodically alternately stacked AlGaInP quantum well layers and AlGaInP quantum barrier layers.
[0108] Exemplarily, a plurality of AlGaInP quantum well layers and AlGaInP quantum barrier layers are alternately grown on the surface of the first semiconductor layer using MOCVD equipment.
[0109] The third step is to make the second semiconductor layer.
[0110] In the embodiment of the present disclosure, the second semiconductor layer includes a P-type AlInP carrier confinement layer and a P-type GaP window layer.
[0111] Exemplarily, a P-type AlInP carrier confinement layer and a P-type GaP window layer are sequentially fabricated on the surface of the active layer using MOCVD equipment.
[0112] Step 2: bonding a second temporary substrate to the surface of the second semiconductor layer.
[0113] The second temporary substrate may be any one of substrates such as a sapphire substrate and a Si substrate.
[0114] In the embodiment of the present disclosure, the second temporary substrate and the second semiconductor layer can be bonded by any one of photoresist, benzocyclobutene, and silica gel.
[0115] The bonding temperature is 280-320° C. For example, the bonding temperature is 300° C.
[0116] In the embodiment of the present disclosure, if the bonding temperature is too high, the semiconductor layer will be damaged, and if the bonding temperature is too low, it will be detrimental to the bonding effect. Using the above temperature for bonding can ensure a good bonding effect without damaging the semiconductor layer.
[0117] Step 3: removing the first temporary substrate.
[0118] Step 4: forming a bonding layer on the surface of the substrate.
[0119] In the embodiment of the present disclosure, the substrate may be any one of a sapphire substrate, a Si substrate and the like, for example, a sapphire substrate.
[0120] In the disclosed embodiment, the material of the bonding layer is any one of photoresist, benzocyclobutene, and silica gel.
[0121] Step 5: bonding the substrate and the first semiconductor layer via the bonding layer.
[0122] The bonding temperature is 280-320° C. For example, the bonding temperature is 300° C.
[0123] Step 6: removing the second temporary substrate.
[0124] In the embodiment of the present disclosure, when removing the second temporary substrate, a solution may be used for treatment, and the adhesive material used for bonding on the surface is removed while the second temporary substrate is removed.
[0125] S22, performing patterning on the first semiconductor layer, the active layer and the second semiconductor layer to form a step structure.
[0126] In one example, step S22 includes:
[0127] The second semiconductor layer, the active layer and the first semiconductor layer stacked in sequence are patterned by using an etching technology to expose the first semiconductor layer to form a step structure.
[0128] In the embodiment of the present disclosure, the step surface of the step structure is located in the first semiconductor layer.
[0129] In the embodiment of the present disclosure, the second semiconductor layer, the active layer, and the first semiconductor layer stacked in sequence are patterned by using an etching technology to expose the first semiconductor layer to form a step structure, which may include:
[0130] In the first step, a layer of photoresist is coated on the surface of the second semiconductor layer.
[0131] The second step is to use a mask to block and expose the photoresist.
[0132] The third step is to develop the exposed photoresist to form a photoresist mask.
[0133] In the fourth step, the second semiconductor layer, the active layer and the first semiconductor layer are etched based on the photoresist mask to form a step structure.
[0134] Step 5: Use a stripping solution to remove the photoresist.
[0135] S23, manufacturing a first electrode and a second electrode, wherein the first electrode is located on the step surface, and the second electrode is located on the surface of the second semiconductor layer.
[0136] In one example, step S23 includes:
[0137] By adopting electron beam evaporation technology or magnetron sputtering technology, a first electrode is formed on the step surface of the first semiconductor layer, and a second electrode is formed on the surface of the second semiconductor layer.
[0138] S24, manufacturing a reflective layer, wherein the reflective layer covers the step structure.
[0139] In one example, step S24 includes:
[0140] A DBR layer is fabricated on the second semiconductor layer and the surface of the step structure by using a plasma enhanced chemical vapor deposition (PECVD) technique or an atomic layer deposition (ALD) technique to form a reflective layer; the reflective layer is patterned to form a first through hole and a second through hole.
[0141] S25 . Make a first electrode pad and a second electrode pad, wherein the first electrode pad penetrates the reflective layer and is connected to the first electrode, and the second electrode pad penetrates the reflective layer and is connected to the second electrode.
[0142] In one example, step S25 includes:
[0143] In the first step, the metal stack is deposited.
[0144] The metal stack is connected to the first electrode through the first through hole, and is connected to the second electrode through the second through hole.
[0145] In the embodiment of the present disclosure, the metal stack includes a Cr layer, an Al layer, a Ti layer, a Ni layer, and an Au alloy layer stacked in sequence.
[0146] In one example, the thickness of the Cr layer is 80-120 nm, the thickness of the Al layer is 2500-3500 nm, the thickness of the Ti layer is 450-550 nm, the thickness of the Ni layer is 1800-2200 nm, and the thickness of the Au alloy layer is 18000-22000 nm.
[0147] Exemplarily, the thickness of the Cr layer is 100 nm, the thickness of the Al layer is 3000 nm, the thickness of the Ti layer is 500 nm, the thickness of the Ni layer is 2000 nm, and the thickness of the Au alloy layer is 20000 nm.
[0148] The second step is to form a first photoresist mask layer on the metal stack.
[0149] The third step is to pattern the metal stack, the reflective layer and the epitaxial structure under the shielding of the first photoresist mask layer, so that the projections of the metal stack and the reflective layer on the first semiconductor layer overlap with the first semiconductor layer.
[0150] Exemplarily, the metal stack, the reflective layer and the epitaxial structure may be patterned by dry etching, for example, etching gas Cl2+BCl3 is used to etch the metal stack and the epitaxial structure, and etching gas CF4 is used to etch the reflective layer. In the above etching process, the temperature is room temperature, the pressure is 4 mTorr, and the etching rate is 100 angstroms / second.
[0151] This step is also the step of making the etching groove (ISO) of the light emitting diode. The present application completes this step together with the patterning process of the pad.
[0152] The first photoresist mask layer may be a positive photoresist mask layer.
[0153] The fourth step is to remove the first photoresist mask layer.
[0154] The fifth step is to make a second photoresist mask layer on the metal stack, wherein the middle part of the second photoresist mask layer is hollowed out.
[0155] The second photoresist mask layer may be a positive photoresist mask layer.
[0156] The sixth step is to pattern the metal stack under the shielding of the second photoresist mask layer, so as to separate the metal stack from the middle to obtain the first electrode pad and the second electrode pad.
[0157] The metal stack may be patterned by dry etching, and the etching method and conditions are the same as those of etching the metal stack in the third step.
[0158] Step seven, removing the second photoresist mask layer.
[0159] In the embodiment of the present disclosure, the first electrode and the first electrode pad form a first electrode structure, and the second electrode and the second electrode pad form a second electrode structure.
[0160] In the embodiment of the present disclosure, the projection of the reflective layer on the first semiconductor layer is a first rectangle, and the projections of the first electrode pad and the second electrode pad on the first semiconductor layer are second rectangles, and the three sides of each of the second rectangles coincide with the three sides of the first rectangle.
[0161] In the embodiment of the present disclosure, the length of the second rectangle is 20-30 μm, and the width of the second rectangle is 10-15 μm.
[0162] S26, manufacturing a passivation layer, wherein the passivation layer covers the epitaxial structure, the reflective layer, and the side walls of the first electrode pad and the second electrode pad, and the passivation layer also covers the spacing area between the first electrode pad and the second electrode pad.
[0163] In one example, step S26 includes:
[0164] A SiO2 layer is fabricated on the surface of the step structure by using a plasma enhanced chemical vapor deposition (PECVD) technique or an atomic layer deposition (ALD) technique; the SiO2 layer is patterned to obtain a passivation layer.
[0165] In the embodiment of the present disclosure, the passivation layer may also be a transparent insulating material such as Al2O3, and the present disclosure does not limit the material of the passivation layer.
[0166] Optionally, after the above steps, the method may further include: thinning the substrate, wherein the thickness of the substrate after thinning is 400-600 microns, for example, 500 microns. After thinning, subsequent processes of light emitting diodes are performed to obtain light emitting diode chips.
[0167] In the disclosed embodiment, the pad manufacturing method is improved, and the pad patterning and etching groove (ISO) are manufactured in one step, so that the influence of the gap can be eliminated. In addition, the pad is treated with a metal processing procedure after the glue is removed, so that possible metal residues can be improved, the chip size can be further reduced, and the competitiveness of the device can be improved. The size of the light-emitting diode chip manufactured by the method of the embodiment of the application is reduced by 4 microns, accounting for about 10%.
[0168] The above description is only an optional embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure shall be included in the protection scope of the present disclosure.
Claims
1. A light emitting diode, characterized in that: The light-emitting diode comprises: an epitaxial structure (1000), a first electrode (105), a second electrode (106), a reflective layer (107), a first electrode pad (108) and a second electrode pad (109); The epitaxial structure (1000) comprises a first semiconductor layer (101), an active layer (102) and a second semiconductor layer (103) which are stacked in sequence, the first semiconductor layer (101), the active layer (102) and the second semiconductor layer (103) forming a step structure, the first electrode (105) being located on a step surface (120) of the step structure, the second electrode (106) being located on a surface of the second semiconductor layer (103), the reflective layer (107) covering the step structure and the first electrode (105) and the second electrode (106), the first electrode pad (108) penetrating the reflective layer (107) and being connected to the first electrode (105), and the second electrode pad (109) penetrating the reflective layer (107) and being connected to the second electrode (106); The projection of the reflective layer (107) on the first semiconductor layer (101) coincides with the first semiconductor layer (101), and the edges of the projections of the first electrode pad (108) and the second electrode pad (109) on the first semiconductor layer (101) coincide with the edges of the projection of the reflective layer (107) on the first semiconductor layer (101).
2. The light emitting diode according to claim 1, characterized in that: The projection of the reflective layer (107) on the first semiconductor layer (101) is a first rectangle, and the projections of the first electrode pad (108) and the second electrode pad (109) on the first semiconductor layer (101) are second rectangles, and the three sides of each of the second rectangles coincide with the three sides of the first rectangle respectively.
3. The light emitting diode according to claim 2, characterized in that: The length of the second rectangle is 20-30 μm, and the width of the second rectangle is 10-15 μm.
4. The light emitting diode according to any one of claims 1 to 3, characterized in that: The light-emitting diode further comprises: a passivation layer (110), the passivation layer (110) covering the epitaxial structure (1000), the reflective layer (107), and the side walls of the first electrode pad (108) and the second electrode pad (109), and the passivation layer (110) also covers the spacing area between the first electrode pad (108) and the second electrode pad (109).
5. The light emitting diode according to any one of claims 1 to 3, characterized in that: The light-emitting diode further comprises: a substrate (100) and a bonding layer (104); The first semiconductor layer (101) and the substrate (100) are bonded via the bonding layer (104).
6. A method for preparing a light emitting diode, characterized in that: The method comprises: forming a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence, wherein the second semiconductor layer, the active layer, and the first semiconductor layer constitute an epitaxial structure; Performing a patterning process on the epitaxial structure to form a step structure; Manufacturing a first electrode and a second electrode, wherein the first electrode is located on a step surface of the step structure, and the second electrode is located on a surface of the second semiconductor layer; Manufacturing a reflective layer, wherein the reflective layer covers the step structure and the first electrode and the second electrode; A first electrode pad and a second electrode pad are manufactured, wherein the first electrode pad passes through the reflective layer and is connected to the first electrode, and the second electrode pad passes through the reflective layer and is connected to the second electrode; a projection of the reflective layer on the first semiconductor layer overlaps with the first semiconductor layer, and edges of the projections of the first electrode pad and the second electrode pad on the first semiconductor layer overlap with edges of the projection of the reflective layer on the first semiconductor layer.
7. The method for preparing a light emitting diode according to claim 6, characterized in that: The method of manufacturing the first electrode pad and the second electrode pad comprises: depositing a metal stack; forming a first photoresist mask layer on the metal stack; Under the shielding of the first photoresist mask layer, patterning the metal stack, the reflective layer and the epitaxial structure so that the projections of the metal stack and the reflective layer on the first semiconductor layer overlap with the first semiconductor layer; removing the first photoresist mask layer; Making a second photoresist mask layer on the metal stack, wherein the middle portion of the second photoresist mask layer is hollowed out; Under the shielding of the second photoresist mask layer, patterning the metal stack so that the metal stack is separated from the middle to obtain the first electrode pad and the second electrode pad; The second photoresist mask layer is removed.
8. The method for preparing a light emitting diode according to claim 6, characterized in that: The projection of the reflective layer on the first semiconductor layer is a first rectangle, and the projections of the first electrode pad and the second electrode pad on the first semiconductor layer are second rectangles, and three sides of each of the second rectangles coincide with three sides of the first rectangle respectively.
9. The method for preparing a light emitting diode according to claim 8, characterized in that: The length of the second rectangle is 20-30 μm, and the width of the second rectangle is 10-15 μm.
10. The method for preparing a light emitting diode according to any one of claims 6 to 9, characterized in that: The light emitting diode preparation method further comprises: A passivation layer is manufactured, wherein the passivation layer covers the epitaxial structure, the reflective layer, and the side walls of the first electrode pad and the second electrode pad, and the passivation layer also covers the spacing area between the first electrode pad and the second electrode pad.