A MXene / graphene composite and its preparation method and application

By mixing MXene and graphene oxide in an aqueous solution, mechanical stirring under heating conditions, reducing with hydrazine hydrate and ammonia water, the preparation of MXene/graphene composite is simplified, and the problem of high preparation cost in the prior art is solved. , improves its electrochemical performance and application value.

CN118335951BActive Publication Date: 2024-11-05BEIFANG UNIV OF NATITIES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410525400.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-29
Publication Date
2024-11-05
Estimated Expiration
2044-04-29

AI Technical Summary

Technical Problem

The existing MXene/graphene composite preparation method is expensive and not suitable for large-scale production, which limits its widespread application in energy storage device electrodes.

Method used

By mixing MXene and graphene oxide in aqueous solution, mechanical stirring under heating conditions, reducing with hydrazine hydrate and ammonia water, the MXene/graphene composite was obtained, which simplified the preparation process and reduced the cost.

Benefits of technology

It improves the electrochemical performance of the composite, improves the specific capacitance, rate performance and energy density, and is suitable for supercapacitors, lithium-ion batteries and other fields, with a wide range of application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118335951B_ABST
    Figure CN118335951B_ABST
Patent Text Reader

Abstract

The invention discloses a MXene / graphene composite and a preparation method and application thereof, wherein the preparation method comprises the following steps: 1. MXene and graphene oxide aqueous solutions are separately prepared, the MXene aqueous solution and the graphene oxide aqueous solution are mixed, and the MXene and graphene oxide are fully mixed in water by mechanical stirring or ultrasonic treatment to form a MXene / graphene oxide mixed aqueous solution; 2. a reducing agent is added to the MXene / graphene oxide mixed aqueous solution, mechanical stirring is performed, and heating is performed, and mechanical stirring is maintained during the heating process to reduce the graphene oxide in the mixed aqueous solution to graphene to obtain a MXene / graphene mixed aqueous solution; 3. the reduced MXene / graphene mixed aqueous solution is filtered, washed, and dried to obtain a MXene / graphene composite. The method can significantly improve the electrochemical performance of the MXene / graphene composite by optimizing the preparation conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrode material for an energy storage device, and in particular to a MXene / graphene composite and a preparation method and application thereof. Background Art

[0002] As people's awareness of environmental protection and climate change increases, the development and utilization of new energy sources are increasingly valued. Energy storage technology is an important component of new energy and is widely used in electric vehicles, home energy storage, grid energy storage and other fields. Among them, the electrodes of energy storage devices are key components, and improving their electrochemical performance is of great significance to improving energy storage efficiency and cycle life.

[0003] As a new type of material, MXene has good electrical conductivity and electrochemical properties, so it has broad application prospects in the fields of energy storage device electrodes, etc. Graphene, as another excellent carbon-based material, has high electrical conductivity and thermal stability, and can improve the structure and electrochemical properties of MXene, so it has become a common method for preparing MXene composites.

[0004] However, the existing preparation methods of MXene / graphene composites usually adopt expensive chemical synthesis methods, such as chemical precipitation, high temperature thermal reduction, wet chemical method, etc., which are not only costly but also have certain limitations for large-scale production. Therefore, it is necessary to explore a simple, economical and effective method for preparing MXene / graphene composites. Summary of the invention

[0005] The purpose of the present invention is to provide a MXene / graphene composite and a preparation method and application thereof, which has the advantages of being simple, economical and efficient, and can greatly improve the electrochemical performance of the composite by optimizing the preparation conditions.

[0006] In order to solve the problems existing in the prior art, the technical solution adopted by the present invention is as follows:

[0007] In a first aspect, the present invention provides a method for preparing a MXene / graphene composite, comprising the following steps:

[0008] ① Prepare aqueous solutions of MXene and graphene oxide respectively, mix the MXene aqueous solution and the graphene oxide aqueous solution, and fully mix the MXene and graphene oxide in water by mechanical stirring or ultrasonic treatment to form a MXene / graphene oxide mixed aqueous solution;

[0009] ② Add a reducing agent to the MXene / graphene oxide mixed aqueous solution, perform mechanical stirring, and heat. During the heating process, maintain mechanical stirring to reduce the graphene oxide in the mixed aqueous solution to graphene, thereby obtaining a MXene / graphene mixed aqueous solution;

[0010] ③ Filter, wash and dry the reduced MXene / graphene mixed aqueous solution to obtain a MXene / graphene composite.

[0011] Furthermore, the method for preparing the MXene aqueous solution comprises the following steps: ultrasonically dispersing MXene nanosheets in deionized water under a protective atmosphere to obtain a MXene aqueous solution, wherein the concentration of the MXene aqueous solution is 0.5-10 g / L, preferably 2 g / L.

[0012] Furthermore, the method for preparing the graphene oxide aqueous solution comprises the following steps: ultrasonically dispersing graphene oxide in deionized water to obtain a graphene oxide aqueous solution, wherein the concentration of the graphene oxide aqueous solution is 0.2-10 g / L, preferably 1 g / L.

[0013] Furthermore, the mass ratio of the MXene nanosheets to graphene oxide is 1-9:1, preferably 4:1.

[0014] Furthermore, the heating temperature in step ② is 50-99° C., and the heating time is 0.5-3 hours.

[0015] Furthermore, the reducing agent in step ② is hydrazine hydrate and ammonia water.

[0016] Furthermore, the mass ratio of the hydrazine hydrate to the graphene oxide is 1:2-20, preferably 1:12; the mass ratio of the ammonia water to the graphene oxide is 1:1-20, preferably 1:6.

[0017] In a second aspect, the present invention provides a MXene / graphene composite prepared by the preparation method described in the first aspect.

[0018] In a third aspect, the present invention provides the use of the MXene / graphene composite described in the second aspect in preparing electrode materials for energy storage devices.

[0019] The advantages and beneficial effects of the present invention are:

[0020] The present invention adds graphene oxide to MXene and adopts optimized preparation conditions to improve the structure and electrochemical properties of MXene, improve the electrochemical properties of the composite, and greatly improve the performance in terms of specific capacitance, rate performance and energy density, thereby improving its practical application value in application scenarios such as energy storage device electrodes.

[0021] The preparation method of the present invention is simple and economical, does not require expensive chemical synthesis methods, and can be prepared by physical mixing and heat treatment methods, has low cost, and is suitable for large-scale production. It has the advantages of being simple, economical and efficient.

[0022] The MXene / graphene composite prepared by the method of the present invention has a wide range of applications, and is suitable for use in the fields of supercapacitors, lithium-ion batteries, electromagnetic shielding, etc., and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a scanning electron microscope image of the MXene / graphene composite prepared in Example 1;

[0024] Figure 2 The constant current charge-discharge curve of the zinc ion hybrid supercapacitor with the MXene / graphene composite prepared in Example 1 as the cathode at 0.5-10 A / g;

[0025] Figure 3 is the specific capacitance of the MXene / graphene composite cathode prepared in Example 1 at 0.5-10 A / g;

[0026] Figure 4 It is a comparison chart of the specific capacitance of MXene / graphene composite cathodes prepared in different embodiments and comparative examples at 0.5-10 A / g. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present application to clearly describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments in the present application belong to the scope of protection of this application.

[0028] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.

[0029] The chemical formula of the MXene material described in this application is M n+1 X n T x , wherein M is a transition metal (such as Ti, Mo, Cr, Nb, V, Sc, Zr, Hf or Ta), X is carbon and / or nitrogen, and T represents a surface functional group (such as O, F, OH, Cl), n = 1, 2, 3 or 4. The MXene nanosheets described in this application can be purchased or prepared by oneself.3 AlC 2 、V 2 CT x 、Ti 3 C 2 T x or Nb 2 CT x As a raw material, MXene fragments are prepared by etching and peeling according to known methods. The graphene oxide described in this application can be purchased or prepared by itself, for example, by the Hummers method or the Brodie method. Example 1

[0030] The MXene nanosheets used in this example were purchased from Foshan Xinxin Technology Co., Ltd. 3 C 2 T x (Purity ≥99.9%).

[0031] The present embodiment provides a method for preparing a MXene / graphene composite, comprising the following steps:

[0032] ① The preparation method of MXene aqueous solution is as follows: ultrasonically disperse MXene nanosheets in deionized water under nitrogen protection atmosphere to obtain MXene aqueous solution, and the concentration of MXene aqueous solution is 2 g / L;

[0033] ② Prepare graphene oxide aqueous solution: The graphene oxide used in this embodiment was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. The graphene oxide was ultrasonically dispersed in deionized water to obtain a graphene oxide aqueous solution. The mass concentration of the graphene oxide aqueous solution was 1 g / L.

[0034] ③ Mix the MXene aqueous solution and the graphene oxide aqueous solution, and stir them mechanically to mix them thoroughly to obtain a MXene / graphene oxide mixed aqueous solution, wherein the mass ratio of MXene nanosheets to graphene oxide is 4:1.

[0035] ④ Add hydrazine hydrate and ammonia water to the MXene / graphene oxide mixed aqueous solution and perform mechanical stirring. The mass ratio of hydrazine hydrate to graphene oxide is 1:12, and the mass ratio of ammonia water to graphene oxide is 1:6. Then heat at 85°C for 1 hour. Maintain mechanical stirring during the heating process to reduce the graphene oxide in the mixed aqueous solution to graphene to obtain a MXene / graphene mixed aqueous solution.

[0036] ⑤ Filter, wash and dry the reduced MXene / graphene mixed aqueous solution to obtain the final MXene / graphene composite.

[0037] Figure 1This is a scanning electron microscope image of the MXene / graphene composite prepared in this example, which has both the flaky structure of MXene and the wrinkled structure of graphene, indicating the successful composite of MXene and graphene. Example 2

[0038] The MXene nanosheets used in this example were prepared by the following method:

[0039] 1g Nb 2 The AlC powder was immersed in 10 mL of 50 wt% HF solution and stirred continuously at room temperature for 90 h. The resulting MXene suspension was repeatedly washed with deionized water six to eight times and centrifuged at 1500 rpm for 15 min until the pH of the supernatant reached about 6.

[0040] The present embodiment provides a method for preparing a MXene / graphene composite, comprising the following steps:

[0041] ① Preparation of MXene aqueous solution: MXene nanosheets were ultrasonically dispersed in deionized water under nitrogen protection atmosphere to obtain MXene aqueous solution; the concentration of MXene aqueous solution was 3 g / L;

[0042] ② Prepare a graphene oxide aqueous solution. The graphene oxide used in this embodiment is prepared by the commonly used Hummers method. The graphene oxide is ultrasonically dispersed in deionized water to obtain a graphene oxide aqueous solution. The mass concentration of the graphene oxide aqueous solution is 1.5 g / L.

[0043] ③ Mix the MXene aqueous solution and the graphene oxide aqueous solution, perform ultrasonic treatment to fully mix them, and obtain a MXene / graphene oxide mixed aqueous solution. The mass ratio of MXene nanosheets to graphene oxide is 9:1.

[0044] ④ Add hydrazine hydrate and ammonia water to the MXene / graphene oxide mixed aqueous solution and perform mechanical stirring. The mass ratio of hydrazine hydrate to graphene oxide is 1:10, and the mass ratio of ammonia water to graphene oxide is 1:10. Then heat at 90°C for 1 hour. Maintain mechanical stirring during the heating process to reduce the graphene oxide in the mixed aqueous solution to graphene to obtain a MXene / graphene mixed aqueous solution.

[0045] ⑤ Filter, wash and dry the reduced MXene / graphene mixed aqueous solution to obtain the final MXene / graphene composite. Example 3

[0046] The MXene nanosheets used in this example were prepared by the following method:

[0047] In an ice bath, 2 g V 2 AlC powder was slowly added to 60 mL of HF solution with a concentration of 6 M. After stirring at room temperature for about 10 days, the resulting mixture solution was washed with deionized water by centrifugation several times.

[0048] The present embodiment provides a method for preparing a MXene / graphene composite, comprising the following steps:

[0049] ① Preparation of MXene aqueous solution: Ultrasonic dispersion of MXene nanosheets in deionized water under argon protective atmosphere to obtain MXene aqueous solution; the concentration of MXene aqueous solution is 1 g / L;

[0050] ② Prepare an aqueous solution of graphene oxide. The preparation method of the aqueous solution of graphene oxide used in this embodiment is to prepare graphene oxide by the commonly used Brodie method, ultrasonically disperse graphene oxide in deionized water to obtain an aqueous solution of graphene oxide. The mass concentration of the aqueous solution of graphene oxide is 2 g / L.

[0051] ③ Mix the MXene aqueous solution and the graphene oxide aqueous solution, and stir them mechanically to mix them thoroughly to obtain a MXene / graphene oxide mixed aqueous solution. The mass ratio of MXene nanosheets to graphene oxide is 1:1.

[0052] ④ Add hydrazine hydrate and ammonia water to the MXene / graphene oxide mixed aqueous solution and perform mechanical stirring. The mass ratio of hydrazine hydrate to graphene oxide is 1:5, and the mass ratio of ammonia water to graphene oxide is 1:4. Then heat at 85°C for 1 hour. Maintain mechanical stirring during the heating process to reduce the graphene oxide in the mixed aqueous solution to graphene to obtain a MXene / graphene mixed aqueous solution.

[0053] ⑤ Filter, wash and dry the reduced MXene / graphene mixed aqueous solution to obtain the final MXene / graphene composite. Example 4

[0054] The MXene nanosheets used in this example were prepared by the following method:

[0055] 2 g of LiF was mixed with 40 ml of 9 M HCl and stirred at room temperature for 30 minutes. Subsequently, 2 g of Ti 3 AlC 2 The powder was slowly added to the above mixture. After etching at 35°C for 24 hours, it was repeatedly washed with ultrapure water until the pH reached 6.

[0056] The present embodiment provides a method for preparing a MXene / graphene composite, comprising the following steps:

[0057] ① The preparation method of MXene aqueous solution is: ultrasonically disperse MXene nanosheets in deionized water under argon protective atmosphere to obtain MXene aqueous solution, and the concentration of MXene aqueous solution is 5g / L;

[0058] ② Prepare a graphene oxide aqueous solution. The graphene oxide used in this embodiment is prepared by the commonly used Brodie method. The graphene oxide is ultrasonically dispersed in deionized water to obtain a graphene oxide aqueous solution. The mass concentration of the graphene oxide aqueous solution is 0.5 g / L, and the remaining steps are the same as in Example 1. Comparative Example 1

[0059] This comparative example provides a method for preparing a MXene / graphene composite. The difference between this comparative example and Example 1 is only that steps ④ and ⑤ are different.

[0060] Step ④ of this comparative example is to subject the MXene / graphene oxide mixed aqueous solution obtained in step ③ of Example 1 to a self-assembly reaction for 2 hours, and then freeze-dry for 20 hours to obtain a MXene / graphene oxide composite;

[0061] In step ⑤ of this comparative example, the MXene / graphene oxide composite is placed in a sealed container, and 1.5 mL of a hydrazine hydrate-ammonia aqueous solution is dripped around the MXene / graphene oxide composite (the hydrazine hydrate-ammonia aqueous solution is composed of hydrazine hydrate with a mass concentration of 85% and ammonia aqueous solution with a mass concentration of 25% in a volume ratio of 2:1), and then the sealed container is placed in an oven and heated at 60° C. for 24 h for steam reduction to obtain a MXene / graphene composite. The rest is the same as in Example 1. Comparative Example 2

[0062] This comparative example provides a method for preparing a MXene / graphene composite. The difference between this comparative example and Example 1 is only that:

[0063] In step ④ of this comparative example, the MXene / graphene oxide mixed aqueous solution obtained in step ③ is subjected to self-assembly reaction for 2 hours, and then freeze-dried for 20 hours to obtain a MXene / graphene oxide composite, and the MXene / graphene oxide composite is evenly spread in a corundum crucible, and the crucible is placed in a tube furnace, and under argon protection, the temperature is raised to 400° C. at a rate of 5° C. / min, and then reduced for 2 hours, and cooled to room temperature to obtain a MXene / graphene composite. This comparative example does not have step ⑤, and the rest is the same as Example 1. Comparative Example 3

[0064] This comparative example provides a method for preparing a MXene / graphene composite. The difference between this comparative example and Example 1 is only that: in step ④, the mass ratio of hydrazine hydrate to graphene oxide is 1:22, and the rest is the same as Example 1. Comparative Example 4

[0065] This comparative example provides a method for preparing a MXene / graphene composite. The difference between this comparative example and Example 1 is only that the mass ratio of ammonia water to graphene oxide in step ④ is 1:0.5, and the rest is the same as Example 1.

[0066] Application Examples

[0067] The MXene / graphene composites prepared in Examples 1-4 and Comparative Examples 1-4 were used as cathodes, zinc foil was used as anodes, and 2M ZnSO 4 Assembling zinc-ion hybrid supercapacitors with electrolytes.

[0068] Figure 2 The constant current charge-discharge curves of the zinc ion hybrid supercapacitor containing the MXene / graphene composite prepared in Example 1 at different current densities of 0.5A / g, 1A / g, 2A / g, 5A / g and 10A / g. Figure 2 It can be seen that an obvious charging platform appears only at a current density of 0.5 A / g, and there is no obvious voltage drop at all current densities, indicating the small internal resistance of the zinc ion hybrid supercapacitor.

[0069] like Figure 3 As shown, the MXene / graphene composite cathode prepared in Example 1 has specific capacitances of 660F / g, 446F / g, 398F / g, 281F / g and 209F / g at current densities of 0.5A / g, 1A / g, 2A / g, 5A / g and 10A / g, respectively, showing excellent specific capacitance.

[0070] Figure 4 The comparison diagram of the specific capacitance of the MXene / graphene composite cathode prepared in Examples 1-4 and Comparative Examples 1-4 as a function of current density is shown in FIG. Figure 4 It can be seen that when the current density increases from 0.5A / g to 10A / g, the specific capacitance of Example 1 decreases from 660F / g to 209F / g, the specific capacitance of Example 2 decreases from 532F / g to 126F / g, the specific capacitance of Example 3 decreases from 455F / g to 146F / g, the specific capacitance of Example 4 decreases from 600F / g to 201F / g, the specific capacitance of Comparative Example 1 decreases from 390F / g to 125F / g, the specific capacitance of Comparative Example 2 decreases from 420F / g to 72F / g, the specific capacitance of Comparative Example 3 decreases from 250F / g to 78F / g, and the specific capacitance of Comparative Example 4 decreases from 160F / g to 50F / g, which indicates that the MXene / graphene composite cathode prepared in Example 1 has the best energy storage performance.

[0071] The embodiments of the present application are described above in conjunction with the accompanying drawings, but the present application is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the guidance of the present application, ordinary technicians in this field can also make many forms without departing from the purpose of the present application and the scope of protection of the claims, all of which are within the protection of the present application.

Claims

1. A method for preparing a MXene / graphene composite, characterized in that: The following steps are involved: ① Prepare aqueous solutions of MXene and graphene oxide respectively, mix the MXene aqueous solution and the graphene oxide aqueous solution, and fully mix the MXene and graphene oxide in water by mechanical stirring or ultrasonic treatment to form a MXene / graphene oxide mixed aqueous solution; ② Add a reducing agent to the MXene / graphene oxide mixed aqueous solution, perform mechanical stirring, and heat. During the heating process, maintain mechanical stirring to reduce the graphene oxide in the mixed aqueous solution to graphene, thereby obtaining a MXene / graphene mixed aqueous solution; ③ Filtering, washing and drying the reduced MXene / graphene mixed aqueous solution to obtain a MXene / graphene composite; The preparation method of the MXene aqueous solution comprises the following steps: ultrasonically dispersing MXene nanosheets in deionized water under a protective atmosphere to obtain a MXene aqueous solution, wherein the concentration of the MXene aqueous solution is 0.5-10 g / L; The mass ratio of the MXene nanosheets to graphene oxide is 1-9:1; The reducing agent in step ② is hydrazine hydrate and ammonia water; The mass ratio of the hydrazine hydrate to the graphene oxide is 1:2-20, and the mass ratio of the ammonia water to the graphene oxide is 1:1-20.

2. The method for preparing the MXene / graphene composite according to claim 1, characterized in that: The method for preparing the graphene oxide aqueous solution comprises the following steps: ultrasonically dispersing graphene oxide in deionized water to obtain a graphene oxide aqueous solution, wherein the concentration of the graphene oxide aqueous solution is 0.2-10 g / L.

3. The method for preparing the MXene / graphene composite according to claim 1, characterized in that: The heating temperature in step ② is 50-99° C., and the heating time is 0.5-3 hours.

4. The method for preparing a MXene / graphene composite according to claim 1, characterized in that: The mass ratio of the hydrazine hydrate to the graphene oxide is 1:12, and the mass ratio of the ammonia water to the graphene oxide is 1:

6.

5. A MXene / graphene composite prepared by the preparation method according to any one of claims 1 to 4.

6. Use of the MXene / graphene composite according to claim 5 in preparing electrode materials for energy storage devices.