A method for preparing mineral fiber cotton using waste incineration fly ash and iron tailings

By reducing and melting waste incineration fly ash and iron tailings in an electric furnace, combined with flue gas purification, the problems of resource waste and low heavy metal recovery efficiency in the existing technology are solved, and efficient resource utilization and environmentally friendly minerals are achieved Fiber cotton preparation.

CN118344014BActive Publication Date: 2024-10-22NORTH CHINA UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410687459.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2024-10-22
Estimated Expiration
2044-05-30

AI Technical Summary

Technical Problem

Existing technology makes it difficult to effectively utilize waste incineration fly ash and iron tailings, resulting in resource waste and environmental pollution. Moreover, plasma melting technology is costly and energy-intensive, and fails to achieve effective recovery of heavy metals.

Method used

By mixing waste incineration fly ash and finely ground iron tailings with a binder, pelletizing is performed and then reduced and melted in an electric furnace. The carbon in the fly ash is used as a reducing agent to generate iron alloy liquid and glass liquid. , separated by centrifuge and flue gas purification device respectively, to prepare mineral fiber wool and secondary fly ash.

Benefits of technology

It achieves efficient resource utilization of waste incineration fly ash and iron tailings, reduces energy consumption, increases iron recovery rate, avoids heavy metals entering the glass structure, achieves detoxification of fly ash and efficient recovery of valuable metals, and prepares The mineral fiber wool has excellent mechanical properties and is suitable for thermal insulation and sound insulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118344014B_ABST
    Figure CN118344014B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of solid waste resource utilization, and in particular to a method for preparing mineral fiber cotton using fly ash from garbage incineration and iron tailings. A method for preparing mineral fiber cotton using fly ash from garbage incineration and iron tailings comprises the following steps: fully mixing fly ash from garbage incineration, finely ground iron tailings and a binder, adding water to continue mixing and then pelletizing; reducing and melting the pellets to obtain ferroalloy liquid and glass liquid; letting the glass liquid flow out from the slag-making port of an electric furnace, and centrifuging to obtain mineral fiber cotton; taking out the ferroalloy after standing; and collecting the flue gas using a flue gas purification device during the melting process to obtain secondary fly ash. The present invention makes full use of carbon, calcium, chlorine and metal oxides in fly ash and silicon and iron oxides in iron tailings, and prepares ferroalloy, mineral fiber cotton and secondary fly ash through melting reduction. The present invention not only realizes the detoxification of fly ash, but also simultaneously realizes the high-value resource utilization of fly ash from garbage incineration and iron tailings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste resource utilization, and in particular to a method for preparing mineral fiber cotton by utilizing waste incineration fly ash and iron tailings. Background Art

[0002] Waste incineration power generation has achieved the reduction of waste, and the harmlessness, energy and resource utilization of waste is a goal of environmental protection projects. However, in the process of waste incineration, secondary pollutants from waste incineration fly ash will be generated. my country has included fly ash from the incineration of domestic waste in the "National List of Hazardous Wastes", and has classified fly ash from the incineration of domestic waste as hazardous waste, requiring proper disposal. Fly ash also contains metals such as iron, copper, nickel and chromium, as well as inorganic substances such as calcium, sodium and potassium. Therefore, it is urgent to carry out relevant research work on the resource utilization of fly ash from the incineration of domestic waste.

[0003] Iron tailings are waste after ore dressing and are also the main component of industrial solid waste. Since most of the valuable iron has been extracted, the utilization rate of the remaining materials is low, and most of them are stored in tailings ponds. The storage not only occupies a large amount of land; but also the tailings pond is a dangerous source and poses a safety risk. Therefore, it is very important to develop a method for utilizing iron tailings to achieve the inherent safety of tailings ponds.

[0004] Mineral wool and its products have the advantages of being light, durable, non-flammable, non-corrosive, and not susceptible to insect infestation, and are excellent heat-insulating, heat-preserving, and sound-absorbing materials. CN112661402B discloses a method for preparing mineral fibers by plasma melting of garbage fly ash, thermal insulation mineral wool, and uses. This method prepares mineral wool from fly ash from garbage incineration by plasma melting. However, the plasma technology is expensive and not as mature as the electric furnace technology; and the plasma melting temperature is between 1400-1600°C, which consumes a lot of energy; during the process of preparing fibers from fly ash, most of the heavy metals remain in the rock wool fibers, and the recovery of heavy metals in the fly ash is not achieved. At the same time, this method uses waste glass as a silicon-increasing agent. The technology for preparing mineral wool and glass fibers using waste glass is relatively mature in China, but the mineral fibers prepared by adding fly ash have lower performance than those prepared by using waste glass alone, which reduces the utilization efficiency of waste glass.

[0005] CN107159678A discloses a dioxin control method in the process of iron ore sintering and coordinated treatment of garbage fly ash. In this method, four components, namely, garbage fly ash, lime milk, flammable solid fuel and sludge, are mixed, granulated and dried to obtain small balls containing garbage fly ash; the iron ore sintering raw material is granulated and mixed with the small balls containing garbage fly ash, and the mixture is ignited and sintered after distribution. However, this method only solidifies the fly ash and does not realize the product utilization of the fly ash well.

[0006] In summary, waste incineration fly ash and iron tailings are two types of solid wastes that urgently need to be treated, and there is an urgent need to develop methods to fully utilize fly ash and iron tailings and convert them into products. Summary of the invention

[0007] The object of the present invention is to provide a method for preparing mineral fiber cotton by utilizing waste incineration fly ash and iron tailings, so as to solve or alleviate the problems existing in the above-mentioned prior art.

[0008] In order to achieve the above-mentioned object, the present invention provides a method for preparing mineral fiber cotton using waste incineration fly ash and iron tailings, which adopts the following technical scheme:

[0009] A method for preparing mineral fiber cotton using waste incineration fly ash and iron tailings comprises the following steps:

[0010] (1) The waste incineration fly ash, finely ground iron tailings and binder are fully mixed, and water is added to continue mixing before pelletizing. Then, the pellets are placed in an electric furnace for reduction and melting to obtain ferroalloy liquid and glass liquid. Since the density of ferroalloy is greater than that of glass liquid, the ferroalloy liquid is precipitated at the bottom of the electric furnace.

[0011] (2) The glass liquid flows out from the slag-making port of the electric furnace and is introduced into a centrifuge through a drainage trough for centrifugation to obtain mineral fiber wool; the ferroalloy is taken out after being left to stand in the electric furnace;

[0012] (3) During the reduction and melting process, the flue gas is captured by a flue gas purification device to obtain secondary fly ash.

[0013] Preferably, in step (1), the finely ground iron tailings are obtained by the following steps: grinding the iron tailings for 5 to 25 minutes at a grinding concentration of 55 to 70%, and finely grinding to -150 μm with a proportion of not less than 80%.

[0014] Preferably, in step (1), the mass fraction of the waste incineration fly ash is 20-50%, and the mass fraction of the iron tailings is 50-80%; the binder is at least one of water glass, carboxymethyl cellulose, starch and sludge, and the amount of the binder is 1-8% of the total mass of the waste incineration fly ash and the iron tailings; the amount of water is 3-8% of the total mass of the waste incineration fly ash and the iron tailings.

[0015] Further preferably, in step (1), the pelletizing is performed using a disc pelletizing machine or a pelletizing machine, the rotation speed of the disc pelletizing machine is 20 to 45 r / min, the inclination angle is 40 to 55°, and the pelletizing time is 5 to 15 min; the pressure of the pelletizing machine is 10 to 30 MPa; and the diameter of the pellets is 0.5 to 5 cm.

[0016] More preferably, in step (1), the temperature of the reduction melting is 1200-1400° C., and the melting time is 30-180 min; the acidity coefficient of the glass liquid is 1.6-2.5, the surface tension coefficient of the glass liquid is 0.2-0.5 N / m, and the viscosity of the glass liquid is 1-3 Pa.s.

[0017] Preferably, the mass percentages of the main elements in the waste incineration fly ash are as follows: Ca 10-60%, C 5-20%, Si 0.1-10%, Al 0.1-8%, Cl 10-30%, Fe 0.1-8%, Na 0.1-6%, K 0.1-6%, S 0.1-3%, Zn 0-1%, Pb 0-1%, Cr 0-1%, Cu 0-1%, Ni 0-1%, and Cd 0-1%.

[0018] Further preferably, the mass percentages of the main components of the iron tailings are as follows: Fe2O35-25%, SiO240-80%, Al2O35-25%, CaO 1-20%, and MgO 1-10%.

[0019] Further preferably, in step (2), the centrifuge is a four-roller centrifuge or a two-roller centrifuge, the rotational speeds of the four rollers of the four-roller centrifuge are 2000-4000, 3000-5000, 3000-6000 and 3000-7000 r / min respectively; the rotational speeds of the two rollers of the two-roller centrifuge are 3000-8000 and 3000-8000 r / min; the diameter of the mineral fiber wool is 5-4 μm, and the tensile strength is 500-1500 MPa.

[0020] More preferably, in step (2), the ferroalloy is taken out from the bottom of the electric furnace after 3 to 15 days, and the iron content in the ferroalloy is ≥ 80%, and the total content of copper, nickel and chromium metals is ≤ 5%.

[0021] Still further preferably, in step (3), the secondary fly ash is a mixture of 10-80% NaCl, 10-80% KCl, 1-10% PbCl2, 1-10% ZnCl2 and 0-10% CdCl2.

[0022] Beneficial effects:

[0023] (1) Waste incineration fly ash is a system with high calcium, high chlorine and high carbon, and also contains trace heavy metals in the form of oxides or sulfides. Iron tailings are mainly composed of quartz, pyroxene and magnetite, and are a system with high iron, high silicon and a certain amount of aluminum. The present invention treats the two together at high temperature, and the carbon in the waste incineration fly ash reacts with CO2 under high temperature conditions to generate CO, providing a reducing agent for the reduction reaction; at the same time, carbon can also directly participate in the reduction reaction. The heavy metal oxides (such as Cu, Ni, Cr, etc.) in the waste incineration fly ash, the magnetite in the iron tailings and the iron oxides in the pyroxene are respectively reduced to metallic iron and other metals under a high-temperature reducing atmosphere, thereby achieving the reduction of metal-containing minerals in the system. Compared with the reduction process of iron tailings using coal, coke, etc. as a reducing agent, the present invention uses carbon in fly ash as a reducing agent, saves carbon resources, has a lower temperature for high-temperature molten reduction reaction, and consumes less energy, thereby achieving energy conservation and emission reduction.

[0024] (2) The SiO2 content in iron tailings is very high. SiO2 can regulate the melting point of the SiO2-Al2O3-CaO system. Due to the presence of Fuji body (FeO) and iron, the melting point of the system can also be reduced. The melting point of the system is reduced to below 1400°C, and the system is completely liquid. This method has a lower melting temperature than the direct melting of waste incineration fly ash. Compared with the direct reduction process of iron tailings and iron ore, there is no need to add additives such as sodium carbonate and fluorite, which can save resources.

[0025] (3) A high content of Si can also reduce the viscosity of the system, because it is an amorphous glass structure after cooling, so it is called glass liquid. In a low-viscosity liquid phase system, iron particles can quickly aggregate into a ferroalloy liquid and gather in the lower part of the liquid phase system, while the glass liquid with a smaller specific gravity gathers in the upper part, so that the iron liquid and the glass liquid are separated into layers due to different specific gravities. At the same time, the iron liquid forms an alloy with iron-loving heavy metals (such as copper, nickel and chromium, etc.), and the iron grade in the ferroalloy can reach more than 85%, and the iron recovery rate can reach more than 80%, realizing the recovery of iron-loving heavy metals in waste incineration fly ash and iron in iron tailings, and reducing the ratio of heavy metals in fly ash entering the glass liquid. At the same time, compared with the metallic iron obtained by direct reduction of iron tailings and refractory iron ore, the iron grade in the ferroalloy obtained by the invention is higher, and contains metals such as Cu, Ni, Cr, etc., with higher added value.

[0026] (4) During the reduction melting process, due to the high SiO2 in the iron tailings and the reduction stratification of the iron minerals, the acidity coefficient of the glass liquid is further increased, the acidity coefficient of the glass liquid is 1.6-2.5, the surface tension coefficient of the glass liquid is 0.2-0.5N / m, the viscosity of the glass liquid is 1-3Pa.s, the diameter of the mineral fiber wool is 5-14μm, the tensile strength is 500-1500MPa, and the heavy metal leaching of the mineral fiber wool meets the requirements of relevant standards. The mineral fiber wool of the present invention has good quality and can be used to prepare thermal insulation mineral wool, fire-resistant and sound-proof materials, etc., and is used as thermal insulation and fire-resistant materials for walls, roofs, ceilings, etc. of buildings, cold storage and thermal insulation materials for heat pipes, etc., with high added value and broad application prospects.

[0027] (5) Dioxins in fly ash from garbage incineration are decomposed at 750°C to generate inorganic substances such as CO2, H2O, and HCl, which lose their toxicity. The melting temperature of the present invention is 1100°C, which completely decomposes dioxins. The present invention uses a flue gas capture system to capture secondary fly ash. Heavy metals such as Zn, Pb, and Cd react with chloride ions in the fly ash to form chlorides that volatilize into the secondary fly ash, obtaining secondary fly ash whose main components are NaCl, KCl, PbCl2, ZnCl2, and CdCl2. The grade of Pb and Zn reaches more than 4%, which can be used as raw materials for industrial Pb and Zn; iron-loving heavy metals such as Cu, Ni, Cr, etc. can be recovered by forming alloys with metallic iron. Unlike fly ash melting to fix heavy metals in the glass structure, the present invention further recovers valuable metals in the fly ash to prevent them from entering the glass structure and causing potential environmental risks. The present invention achieves fly ash detoxification and also achieves efficient recovery of valuable metals therein. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. Among them:

[0029] Figure 1 is a flow chart of the present invention;

[0030] Figure 2 This is a microscopic structure diagram of the mineral fiber cotton in Example 1 of the present invention;

[0031] Figure 3 This is the XRD diagram of the mineral fiber cotton in Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments. Each example is provided by way of explanation of the present invention and does not limit the present invention. In fact, it will be clear to those skilled in the art that modifications and variations can be made in the present invention without departing from the scope or spirit of the present invention. For example, a feature shown or described as a part of one embodiment can be used in another embodiment to produce yet another embodiment. All other embodiments obtained by those of ordinary skill in the art based on the embodiments in the embodiments of the present invention should belong to the scope of protection of the embodiments of the present invention.

[0033] Example 1

[0034] A method for preparing mineral fiber cotton using waste incineration fly ash and iron tailings comprises the following steps:

[0035] (1) The iron tailings were ball milled for 10 min at a grinding concentration of 60% and finely ground to -150 μm, accounting for 91%. 25% of domestic waste incineration fly ash was mixed with 75% of finely ground iron tailings, and 3% of the total mass of domestic waste incineration fly ash and iron tailings. Then, 4% of the total mass of fly ash and iron tailings was added to continue mixing. After mixing, the disc ball making machine was added for pelletizing. The speed of the disc ball making machine was 25 r / min, the inclination angle was 45°, the ball making time was 8 min, and the pellet diameter was 1 cm.

[0036] (2) After the balling is completed, the pellets are poured into an electric furnace for reduction melting to form glass liquid. The melting temperature is 1200°C and the melting time is 180 minutes. During the reduction melting process, the acidity coefficient of the glass liquid is 2.43, the surface tension coefficient of the glass liquid is 0.24N / m, and the viscosity of the glass liquid is 1.58Pa.s. The glass liquid is introduced into a four-roller centrifuge through a drainage trough. The four roller speeds of the four-roller centrifuge are 2980, 3100, 4520 and 5239r / min respectively. After centrifugation, mineral fiber wool is obtained. The diameter of the mineral fiber wool is 8μm and the tensile strength is 813MPa.

[0037] The heavy metal leaching of the obtained mineral fiber wool was carried out using the methods in the standards "Horizontal Oscillation Method for Toxicity Leaching of Solid Waste" (HJ557-2010) and "Acetate Buffer Solution Method for Toxicity Leaching of Solid Waste" (HJ / T300-2007). The results showed that the heavy metal leaching of the obtained mineral fiber wool met the requirements of relevant standards.

[0038] (3) During the reduction and melting process, the secondary fly ash is collected by the flue gas capture system to obtain a mixed secondary fly ash consisting of 45.13% NaCl, 33.45% KCl, 6.42% PbCl2, 5.13% ZnCl2 and 1.08% CdCl2.

[0039] (4) After the electric furnace has been running for 3 days, the ferroalloy at the bottom of the electric furnace is taken out. The iron content of the ferroalloy is 86.18%, and the total content of copper, nickel and chromium is 2.34%. Figure 1 shown.

[0040] In this embodiment, the mass percentages of the main elements in the waste incineration fly ash are as follows: Ca 50.25%, C 10.89%, Si 1.83%, Al 2.11%, Cl 14.14%, Fe 1.14%, Na 2.21%, K 4.09%, and S 1.56%.

[0041] Waste incineration fly ash also includes the following mass percentages of heavy metal elements: Zn 0.48%, Pb 0.12%, Cu 0.08%, Ni 0.02%, Cr 0.12%, and Cd 0.01%.

[0042] The percentages of the main chemical components of iron tailings are as follows: Fe2O3 12.15%, SiO2 48.50%, Al2O3 16.43%, CaO 8.92% and MgO 5.44%.

[0043] Depend on Figure 2 It can be seen that the surface of mineral fiber cotton is smooth and the fineness is about 10μm.

[0044] Depend on Figure 3 It can be seen that the obtained mineral fiber wool is mainly composed of amorphous diffraction peaks, indicating that it is mainly composed of a non-crystalline glass structure.

[0045] Example 2

[0046] A method for preparing mineral fiber cotton using waste incineration fly ash and iron tailings comprises the following steps:

[0047] The iron tailings were ball-milled in a ball mill with a grinding concentration of 55% for 5 minutes, and the fine grinding to -150μm accounted for 83%. 40% of the fly ash from the incineration of domestic waste was mixed with 60% of the finely ground iron tailings and 4% of the total mass of the fly ash and iron tailings. Water of 5% of the total mass of the fly ash and iron tailings was added to continue mixing. After mixing, the pellets were added to the ball press for pellet pressing. The pressure of the ball press was 28MPa and the diameter of the pellets was 5cm. After the ball making was completed, the pellets were poured into an electric furnace for reduction melting to form glass liquid. The melting temperature was 1300°C and the melting time was 90min. During the reduction melting process, the acidity coefficient of the glass liquid was 1.96, the surface tension coefficient of the glass liquid was 0.31N / m, and the viscosity of the glass liquid was 2.13 Pa.s. The glass liquid is introduced into a four-roll centrifuge through a drainage trough. The four roller speeds of the four-roll centrifuge are 3980, 4215, 5120 and 5890 r / min, respectively. After centrifugation, mineral fiber wool is obtained. The diameter of the mineral fiber wool is 5 μm and the tensile strength is 1435 MPa. The heavy metal leaching of the obtained mineral fiber wool is carried out by the methods in the standards of "Solid Waste Leaching Toxicity Leaching Method Horizontal Oscillation Method" (HJ557-2010) and "Solid Waste Leaching Toxicity Leaching Method Acetate Buffer Solution Method" (HJ / T300-2007). The results show that the heavy metal leaching of the obtained mineral fiber wool meets the requirements of relevant standards.

[0048] (3) During the reduction and melting process, the secondary fly ash is collected by the flue gas capture system to obtain a mixed secondary fly ash consisting of 42.33% NaCl, 38.27% KCl, 4.85% PbCl2, 4.31% ZnCl2 and 1.08% CdCl2.

[0049] (4) After the electric furnace was operated for 5 days, the ferroalloy at the bottom of the furnace was taken out. The iron content of the ferroalloy was 90.15%, and the total content of copper, nickel and chromium was 3.18%.

[0050] In this embodiment, the mass percentages of the main elements in the waste incineration fly ash are as follows: Ca 33.58%, C 15.89%, Si 2.98%, Al 2.58%, Cl 22.35%, Fe 2.01%, Na 3.21%, K 3.05%, and S 1.03%.

[0051] Waste incineration fly ash also includes the following mass percentages of heavy metal elements: Zn 0.36%, Pb 0.21%, Cu 0.08%, Ni 0.11%, Cr 0.08%, and Cd 0.06%.

[0052] The percentage mass contents of the main chemical components of the iron tailings are as follows: Fe2O3 18.54%, SiO2 62.58%, Al2O3 5.32%, CaO 3.16% and MgO 1.57%.

[0053] Example 3

[0054] A method for preparing mineral fiber cotton using waste incineration fly ash and iron tailings comprises the following steps:

[0055] (1) The iron tailings were ball-milled in a ball mill with a grinding concentration of 70% for 25 minutes, and finely ground to -150μm with a proportion of 96%. 50% of the fly ash from the incineration of domestic waste was mixed with 50% of the finely ground iron tailings, and 8% of the total mass of starch from the fly ash from the incineration of domestic waste and the iron tailings, and then 8% of the total mass of water from the fly ash and the iron tailings was added to continue mixing. After mixing, the mixture was added to the ball press for pelletizing, wherein the pressure of the ball press was 16MPa and the diameter of the pellets was 3cm.

[0056] (2) After the balling is completed, the pellets are poured into an electric furnace for reduction melting to form glass liquid. The melting temperature is 1400°C and the melting time is 30 minutes. During the reduction melting process, the acidity coefficient of the glass liquid is 1.75, the surface tension coefficient of the glass liquid is 0.46N / m, and the viscosity of the glass liquid is 2.89 Pa.s. The glass liquid is introduced into a two-roller centrifuge through a drainage trough. The two roller speeds of the two-roller centrifuge are 5120 and 7890r / min respectively. After centrifugation, mineral fiber cotton is obtained. The diameter of the mineral fiber is 14μm and the tensile strength is 535MPa.

[0057] The heavy metal leaching of the obtained mineral fiber wool was carried out using the methods in the standards "Horizontal Oscillation Method for Toxicity Leaching of Solid Waste" (HJ557-2010) and "Acetate Buffer Solution Method for Toxicity Leaching of Solid Waste" (HJ / T300-2007). The results showed that the heavy metal leaching of the obtained mineral fiber wool met the requirements of relevant standards.

[0058] (3) During the reduction and melting process, the secondary fly ash is collected by the flue gas capture system to obtain a mixed secondary fly ash consisting of 53.58% NaCl, 31.41% KCl, 4.98% PbCl2, 5.53% ZnCl2 and 2.01% CdCl2.

[0059] (4) After the electric furnace was in operation for 15 days, the ferroalloy at the bottom of the furnace was taken out. The iron content of the ferroalloy was 82.56%, and the total content of copper, nickel and chromium was 2.89%.

[0060] In this embodiment, the mass percentages of the main elements in the waste incineration fly ash are as follows: Ca 19.85%, C 6.89%, Si 9.58%, Al 7.56%, Cl 28.59%, Fe 8.58%, Na 4.08%, K 1.59%, and S 1.20%.

[0061] Waste incineration fly ash also includes the following mass percentages of heavy metal elements: Zn 0.41%, Pb 0.32%, Cu 0.05%, Ni 0.01%, Cr 0.05%, and Cd 0.06%.

[0062] The percentage mass contents of the main chemical components of the iron tailings are as follows: Fe2O3 6.35%, SiO2 76.89%, Al2O3 5.81%, CaO 2.33% and MgO 0.77%.

[0063] The present invention makes full use of carbon, calcium, chlorine and metal oxides in fly ash and silicon and iron oxides in iron tailings to prepare ferroalloy, mineral fiber wool and secondary fly ash through smelting reduction. The present invention not only achieves the detoxification of fly ash, but also realizes the high-value resource utilization of waste incineration fly ash and iron tailings.

[0064] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" mean that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing mineral fiber cotton using waste incineration fly ash and iron tailings, characterized in that: The following steps are involved: (1) Fully mixing waste incineration fly ash, finely ground iron tailings and a binder, adding water and continuing to mix, and then pelletizing; then, placing the pellets in an electric furnace for reduction melting to obtain ferroalloy liquid and glass liquid. Since the density of the ferroalloy is greater than that of the glass liquid, the ferroalloy liquid is precipitated at the bottom of the electric furnace; the reduction melting temperature is 1200-1400°C, and the melting time is 30-180 minutes; the acidity coefficient of the glass liquid is 1.6-2.5, the surface tension coefficient of the glass liquid is 0.2-0.5N / m, and the viscosity of the glass liquid is 1-3Pa.s; (2) The glass liquid flows out from the slag-making port of the electric furnace and is introduced into a centrifuge through a drainage trough for centrifugation to obtain mineral fiber wool; the ferroalloy is taken out after being left to stand in the electric furnace; (3) During the reduction and melting process, the flue gas is captured by a flue gas purification device to obtain secondary fly ash.

2. The method for preparing mineral fiber wool using waste incineration fly ash and iron tailings according to claim 1, characterized in that: In step (1), the finely ground iron tailings are obtained by the following steps: grinding the iron tailings for 5 to 25 minutes at a grinding concentration of 55 to 70%, and finely grinding to -150 μm with a proportion of not less than 80%.

3. The method for preparing mineral fiber wool using waste incineration fly ash and iron tailings according to claim 1, characterized in that: In step (1), the mass fraction of the waste incineration fly ash is 20-50%, and the mass fraction of the iron tailings is 50-80%; the binder is at least one of water glass, carboxymethyl cellulose, starch and sludge, and the amount of the binder is 1-8% of the total mass of the waste incineration fly ash and the iron tailings; the amount of water is 3-8% of the total mass of the waste incineration fly ash and the iron tailings.

4. The method for preparing mineral fiber wool using waste incineration fly ash and iron tailings according to claim 3, characterized in that: In step (1), the pelletizing is performed by a disc pelletizing machine or a pelletizing machine, the rotation speed of the disc pelletizing machine is 20 to 45 r / min, the inclination angle is 40 to 55°, and the pelletizing time is 5 to 15 min; the pressure of the pelletizing machine is 10 to 30 MPa; and the diameter of the pellets is 0.5 to 5 cm.

5. The method for preparing mineral fiber wool using waste incineration fly ash and iron tailings according to any one of claims 1 to 4, characterized in that: The mass percentages of the main elements in the waste incineration fly ash are as follows: Ca 10-60%, C 5-20%, Si 0.1-10%, Al 0.1-8%, Cl 10-30%, Fe 0.1-8%, Na 0.1-6%, K 0.1-6%, S 0.1-3%, Zn 0-1%, Pb 0-1%, Cr 0-1%, Cu 0-1%, Ni 0-1%, and Cd 0-1%.

6. The method for preparing mineral fiber wool using waste incineration fly ash and iron tailings according to claim 5, characterized in that: The mass percentages of the main components of the iron tailings are as follows: Fe2O3 5-25%, SiO2 40-80%, Al2O3 5-25%, CaO 1-20%, and MgO 1-10%.

7. The method for preparing mineral fiber wool using waste incineration fly ash and iron tailings according to claim 6, characterized in that: In step (2), the centrifuge is a four-roller centrifuge or a two-roller centrifuge, and the rotational speeds of the four rollers of the four-roller centrifuge are 2000-4000, 3000-5000, 3000-6000 and 3000-7000 r / min respectively; the rotational speeds of the two rollers of the two-roller centrifuge are 3000-8000 and 3000-8000 r / min respectively; the diameter of the mineral fiber wool is 5-4 μm, and the tensile strength is 500-1500 MPa.

8. The method for preparing mineral fiber wool using waste incineration fly ash and iron tailings according to claim 7, characterized in that: In step (2), the ferroalloy is taken out from the bottom of the electric furnace after 3 to 15 days, and the iron content in the ferroalloy is ≥80%, and the total content of copper, nickel and chromium metals is ≤5%.

9. The method for preparing mineral fiber wool using waste incineration fly ash and iron tailings according to claim 8, characterized in that: In step (3), the secondary fly ash is a mixture of 10-80% NaCl, 10-80% KCl, 1-10% PbCl2, 1-10% ZnCl2 and 0-10% CdCl2.