A high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating and a preparation method thereof
By using carbon nanotube metal oxide composite thermal filler in crosslinked polyethylene pipes, the problems of poor thermal conductivity and insufficient bending resistance of silane crosslinked polyethylene pipes are solved, and high thermal conductivity, high heat resistance and good static resistance are achieved. Preparation of polyethylene pipes with hydraulic performance.
Patent Information
- Application Number
- CN202410797311.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The thermal conductivity of existing silane crosslinked polyethylene pipes is poor, resulting in cracks and leakage easily in bending places, and the slow crack growth resistance becomes poor after adding thermal filler.
The carbon nanotube metal oxide composite thermal conductivity filler is mixed with raw material A and raw material B for extrusion and crosslinking to prepare high thermal conductivity and high heat resistance crosslinking polyethylene pipes. By controlling the extrusion temperature and crosslinking time, Improve the thermal conductivity and bending resistance of the pipe.
It significantly improves the thermal conductivity and hydrostatic resistance of the pipe, reduces the risk of leakage and rupture at bending, and remains stable in a long-term high-temperature and high-pressure environment, and has good vacuum retention.
Abstract
Description
Technical Field
[0001] The invention relates to a high-thermal-conductivity and high-heat-resistance cross-linked polyethylene pipe for water heating and a preparation method thereof, belonging to the field of polymer compositions. Background Art
[0002] Polyethylene is the world's most produced and consumed plastic, and is widely used in industry, agriculture and daily life. Due to the linear structure of its molecular chain, its high-temperature resistance is poor. Polyethylene cross-linking technology can change the spatial structure of polyethylene, giving it a network structure. The performance of cross-linked polyethylene is improved, and its heat resistance temperature is greatly increased. Combined with its excellent physical and hygienic properties, it can be used as water heating and floor heating pipes, and has broad market potential.
[0003] There are currently two main methods for producing cross-linked polyethylene pipes, namely silane cross-linking and peroxide cross-linking. The two methods are different in reaction mechanism and production method. Silane cross-linking first produces molded pipes and then cross-links them, while peroxide cross-linking is to cross-link the material in a molten state and then cool it to form the pipe. Among them, peroxide cross-linking has high requirements on the quality of the cross-linking raw material resin. This method greatly destroys the crystallinity of the material, and the mechanical properties of the produced pipes are poor, which is manifested in the low yield strength and fracture strength of the material. This situation will not occur with silane cross-linking.
[0004] Since the material produced by silane cross-linking has a higher cross-linking density, the thermal conductivity of the pipe prepared by silane cross-linking will deteriorate when the pipe is of the same thickness. If it is used as a floor heating pipe, it is not conducive to the conduction of heat. This requires the addition of thermally conductive fillers, which need to be evenly dispersed in the pipe and form a thermal conductive chain to significantly improve the thermal conductivity. Too much filler will reduce the performance of the material and the material's resistance to slow crack growth will deteriorate, especially at the bends of the pipe, which are prone to cracks and leakage.
[0005] In summary, in the prior art, the mechanical properties of silane cross-linked polyethylene pipes are good, but due to the high cross-linking density caused by this cross-linking method, the thermal conductivity of the pipe will deteriorate. After adding thermally conductive fillers, the pipe's resistance to slow crack growth will deteriorate, and it will be easy to rupture and leak at the bends. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the defects of the prior art by preparing a carbon nanotube metal oxide composite thermal conductive filler, adding it to raw material A component, then mixing and extruding it with raw material B, and finally cross-linking it to prepare a pipe, thereby improving the thermal conductivity of the pipe and reducing the probability of rupture and leakage at the bending part of the pipe.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] The raw materials of the pipe are composed of raw material A and raw material B, wherein the mass ratio of raw material A to raw material B is 20:22-28.
[0009] The following are further improvements to the above technical solution:
[0010] The raw materials of the raw material A include high-density polyethylene, medium-density polyethylene, low-density polyethylene, carbon nanotube metal oxide composite thermal conductive filler, silane crosslinking agent, crosslinking catalyst, and antioxidant, and the mass ratio is 40-50:22-28:31-39:4.5-5.5:0.8-1.2:1-1.5:0.7-1.
[0011] The molecular weight of the high-density polyethylene is 2.5*10 5 , density is 0.937g / cm 3 ;
[0012] The molecular weight of the medium density polyethylene is 1.7*10 5 , density is 0.925g / cm 3 ;
[0013] The molecular weight of the low-density polyethylene is 5.2*10 4 , density is 0.912g / cm 3 ;
[0014] The silane crosslinking agent is vinyl trimethoxy silane;
[0015] The cross-linking catalyst is dibutyltin laurate maleate;
[0016] The antioxidant is antioxidant 1076.
[0017] The raw materials of the raw material B include medium-density polyethylene, low-density polyethylene, antioxidant, and lubricant, and the mass ratio is 50-60:31-38:0.4-0.6:0.8-1.2;
[0018] The molecular weight of the medium density polyethylene is 1.7*10 5 , density is 0.925g / cm 3 ;
[0019] The molecular weight of the low-density polyethylene is 5.2*10 4 , density is 0.912g / cm 3 ;
[0020] The antioxidant is antioxidant 1076;
[0021] The lubricant is low-density oxidized polyethylene wax with a density of 0.905 g / cm 3 .
[0022] The preparation method of the raw material A is:
[0023] The raw materials of raw material A are mixed according to a proportion, and after being mixed evenly, they are fed into an extruder, and the extrusion temperature is controlled to be 230-240° C., and extrusion is performed to obtain raw material A;
[0024] The preparation method of the raw material B is:
[0025] The raw materials of raw material B are mixed according to proportions, and after being mixed evenly, they are sent into an extruder, and the extrusion temperature is controlled to be 220-230° C., and extrusion is performed to obtain raw material B.
[0026] The preparation method of the carbon nanotube metal oxide composite thermal conductive filler is as follows:
[0027] The carbon nanotubes are mixed with deionized water, stirred to be uniformly dispersed, and then sodium lauryl polyether sulfate is added to the carbon nanotube dispersion, stirred until completely dissolved, and then the ultrasonic frequency is controlled to be 32-38kHz, and ultrasonication is performed for 15-20min. After ultrasonication, the surface-treated carbon nanotubes are obtained by filtering, washing, and drying. The surface-treated carbon nanotubes are then added to a zirconium chloride solution, and the ultrasonic frequency is controlled to be 52-57kHz, and ultrasonication is performed for 70-80min. After ultrasonication, the stirring speed is controlled to be 110-130r / min, and stirring is performed for 175-195min. Then, the filter residue is dried at 82-89°C for 290-320min, and then the dried filter residue is heat-treated at 412-422°C in a nitrogen atmosphere for 290-320min. After cooling, a carbon nanotube metal oxide composite thermal conductive filler is obtained.
[0028] The mass ratio of the carbon nanotubes to deionized water is 2:14-16;
[0029] The carbon nanotubes have a length of 250-300 nm and a diameter of 30-40 nm;
[0030] The mass ratio of the carbon nanotube dispersion to sodium laureth sulfate is 50-60:3;
[0031] The mass ratio of the surface treated carbon nanotubes to the zirconium chloride solution is 17:42-46;
[0032] The concentration of the zirconium chloride solution is 4.5-5.5wt%.
[0033] The preparation method of the polyethylene pipe is:
[0034] The raw material A and the raw material B are mixed in proportion, and after being mixed evenly, they are fed into an extruder, and the extrusion temperature is controlled to be 235-245°C, and extrusion is performed to obtain a tube blank, and the tube blank is placed in an environment with a temperature of 18-25°C and a relative humidity of 60-70%, and cross-linked at room temperature for 70-80 hours, and after cross-linking, a high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating is obtained;
[0035] The outer diameter of the tube blank is 40 mm and the wall thickness is 4.5 mm.
[0036] Compared with the prior art, the present invention achieves the following beneficial effects:
[0037] The pipe of the present invention has good thermal conductivity. According to the method of GB / T3399-1982, the thermal conductivity of the pipe is tested, and the thermal conductivity is 1.74-1.77 W / m·K.
[0038] The pipe of the present invention has good hydrostatic pressure resistance. According to the method of GB / T18992.2-2003, the hydrostatic pressure resistance of the pipe is tested under different hydrostatic pressure stresses. There is no leakage or rupture under the conditions of 12MPa, 20°C, and 1h; there is no leakage or rupture under the conditions of 4.8MPa, 95°C, and 1h; there is no leakage or rupture under the conditions of 4.7MPa, 95°C, and 22h; there is no leakage or rupture under the conditions of 4.6MPa, 95°C, and 165h; there is no leakage or rupture under the conditions of 4.4MPa, 95°C, and 1000h.
[0039] The pipe of the present invention has good heat resistance. According to the method of GB / T18992.2-2003, the thermal stability of the pipe is tested. Under the conditions of 2.5MPa, 110°C and 8760h, there is no leakage and no cracking.
[0040] The pipe of the present invention has good bending resistance, and leakage and rupture are not easy to occur at the bending part. According to the test under the condition of level 5 in the method of GB / T18992.2-2003, the pipe does not leak or rupture;
[0041] The pipe of the present invention has good vacuum retention performance. The test is carried out according to the method of GB / T18992.2-2003, the test temperature is 23°C, the test time is 1 hour, the test pressure is -0.08MPa, and the vacuum pressure change in the pipe is 0.001MPa. DETAILED DESCRIPTION
[0042] Example 1
[0043] A high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating, the raw materials of which are composed of raw material A and raw material B, wherein the mass ratio of raw material A to raw material B is 20:25;
[0044] The raw materials of the raw material A include high-density polyethylene, medium-density polyethylene, low-density polyethylene, carbon nanotube metal oxide composite thermal conductive filler, silane cross-linking agent, cross-linking catalyst, and antioxidant, and the mass ratio is 45:25:35:5:1:1.2:0.8.
[0045] The molecular weight of the high-density polyethylene is 2.5*10 5 , density is 0.937g / cm 3 ;
[0046] The molecular weight of the medium density polyethylene is 1.7*10 5 , density is 0.925g / cm 3 ;
[0047] The molecular weight of the low-density polyethylene is 5.2*10 4 , density is 0.912g / cm 3 ;
[0048] The silane crosslinking agent is vinyl trimethoxy silane;
[0049] The cross-linking catalyst is dibutyltin laurate maleate;
[0050] The antioxidant is antioxidant 1076.
[0051] The raw materials of the raw material B include medium-density polyethylene, low-density polyethylene, antioxidant, and lubricant, and the mass ratio is 55:35:0.5:1;
[0052] The molecular weight of the medium density polyethylene is 1.7*10 5 , density is 0.925g / cm 3 ;
[0053] The molecular weight of the low-density polyethylene is 5.2*10 4 , density is 0.912g / cm 3 ;
[0054] The antioxidant is antioxidant 1076;
[0055] The lubricant is low-density oxidized polyethylene wax with a density of 0.905 g / cm 3 .
[0056] The preparation method of the raw material A is:
[0057] The raw materials of raw material A are mixed according to a proportion, and after being mixed evenly, they are fed into an extruder, and the extrusion temperature is controlled to be 235° C., and extrusion is performed to obtain raw material A;
[0058] The preparation method of the raw material B is:
[0059] The raw materials of raw material B are mixed according to proportions, and after being evenly mixed, they are fed into an extruder, and the extrusion temperature is controlled to be 225° C., and extrusion is performed to obtain raw material B.
[0060] The preparation method of the carbon nanotube metal oxide composite thermal conductive filler is as follows:
[0061] The carbon nanotubes are mixed with deionized water, stirred to be evenly dispersed, and a carbon nanotube dispersion is obtained. Then, sodium lauryl polyether sulfate is added to the carbon nanotube dispersion, stirred until completely dissolved, and then the ultrasonic frequency is controlled to be 35kHz, and ultrasonication is performed for 17 minutes. After ultrasonication, the surface-treated carbon nanotubes are obtained by filtering, washing, and drying. Then, the surface-treated carbon nanotubes are added to a zirconium chloride solution, and the ultrasonic frequency is controlled to be 55kHz, and ultrasonication is performed for 75 minutes. After ultrasonication, the stirring speed is controlled to be 120r / min, and stirring is performed for 180 minutes. Then, the filter residue is dried at 85°C for 300 minutes, and then the dried filter residue is heat-treated at 415°C in a nitrogen atmosphere for 300 minutes. After cooling, a carbon nanotube metal oxide composite thermal conductive filler is obtained.
[0062] The mass ratio of the carbon nanotubes to deionized water is 2:15;
[0063] The carbon nanotubes have a length of 270 nm and a diameter of 35 nm;
[0064] The mass ratio of the carbon nanotube dispersion to sodium laureth sulfate is 55:3;
[0065] The mass ratio of the surface treated carbon nanotubes to the zirconium chloride solution is 17:45;
[0066] The concentration of the zirconium chloride solution is 5wt%.
[0067] The preparation method of the polyethylene pipe is:
[0068] The raw material A and the raw material B are mixed in proportion, and after being mixed evenly, they are fed into an extruder, and the extrusion temperature is controlled to be 240°C, and extrusion is performed to obtain a tube blank, and the tube blank is placed in an environment with a temperature of 20°C and a relative humidity of 65%, and cross-linked at room temperature for 72 hours, and a high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating is obtained after cross-linking;
[0069] The outer diameter of the tube blank is 40 mm and the wall thickness is 4.5 mm.
[0070] Example 2
[0071] A high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating, the raw materials of which are composed of raw material A and raw material B, wherein the mass ratio of raw material A to raw material B is 20:22;
[0072] The raw materials of the raw material A include high-density polyethylene, medium-density polyethylene, low-density polyethylene, carbon nanotube metal oxide composite thermal conductive filler, silane cross-linking agent, cross-linking catalyst, and antioxidant, and the mass ratio is 40:22:31:4.5:0.8:1:0.7.
[0073] The molecular weight of the high-density polyethylene is 2.5*10 5 , density is 0.937g / cm 3 ;
[0074] The molecular weight of the medium density polyethylene is 1.7*10 5 , density is 0.925g / cm 3 ;
[0075] The molecular weight of the low-density polyethylene is 5.2*10 4 , density is 0.912g / cm 3 ;
[0076] The silane crosslinking agent is vinyl trimethoxy silane;
[0077] The cross-linking catalyst is dibutyltin laurate maleate;
[0078] The antioxidant is antioxidant 1076.
[0079] The raw materials of the raw material B include medium-density polyethylene, low-density polyethylene, antioxidant, and lubricant, and the mass ratio is 50:31:0.4:0.8;
[0080] The molecular weight of the medium density polyethylene is 1.7*10 5 , density is 0.925g / cm 3 ;
[0081] The molecular weight of the low-density polyethylene is 5.2*10 4 , density is 0.912g / cm 3 ;
[0082] The antioxidant is antioxidant 1076;
[0083] The lubricant is low-density oxidized polyethylene wax with a density of 0.905 g / cm 3 .
[0084] The preparation method of the raw material A is:
[0085] The raw materials of raw material A are mixed according to a proportion, and after being mixed evenly, they are fed into an extruder, and the extrusion temperature is controlled to be 230° C., and extrusion is performed to obtain raw material A;
[0086] The preparation method of the raw material B is:
[0087] The raw materials of raw material B are mixed according to proportions, and after being mixed evenly, they are sent into an extruder, and the extrusion temperature is controlled to be 220° C., and extrusion is performed to obtain raw material B.
[0088] The preparation method of the carbon nanotube metal oxide composite thermal conductive filler is as follows:
[0089] The carbon nanotubes are mixed with deionized water, stirred to be evenly dispersed, and a carbon nanotube dispersion is obtained. Then, sodium lauryl polyether sulfate is added to the carbon nanotube dispersion, stirred until completely dissolved, and then the ultrasonic frequency is controlled to be 32kHz, and ultrasonication is performed for 15 minutes. After ultrasonication, the surface-treated carbon nanotubes are obtained by filtering, washing, and drying. Then, the surface-treated carbon nanotubes are added to a zirconium chloride solution, and the ultrasonic frequency is controlled to be 52kHz, and ultrasonication is performed for 80 minutes. After ultrasonication, the stirring speed is controlled to be 110r / min, and stirring is performed for 195 minutes. Then, filtering is performed, and the filter residue is dried at 82°C for 320 minutes. Then, the dried filter residue is heat-treated at 412°C in a nitrogen atmosphere for 320 minutes. After cooling, a carbon nanotube metal oxide composite thermal conductive filler is obtained.
[0090] The mass ratio of the carbon nanotubes to deionized water is 2:14;
[0091] The carbon nanotubes have a length of 250 nm and a diameter of 30 nm;
[0092] The mass ratio of the carbon nanotube dispersion to sodium laureth sulfate is 50:3;
[0093] The mass ratio of the surface treated carbon nanotubes to the zirconium chloride solution is 17:42;
[0094] The concentration of the zirconium chloride solution is 4.5 wt %.
[0095] The preparation method of the polyethylene pipe is:
[0096] The raw material A and the raw material B are mixed in proportion, and after being mixed evenly, they are fed into an extruder, and the extrusion temperature is controlled to be 235° C., and extrusion is performed to obtain a tube billet, and the tube billet is placed in an environment with a temperature of 18° C. and a relative humidity of 60%, and cross-linked at room temperature for 70 hours, and a high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating is obtained after cross-linking;
[0097] The outer diameter of the tube blank is 40 mm and the wall thickness is 4.5 mm.
[0098] Example 3
[0099] A high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating, the raw materials of which are composed of raw material A and raw material B, wherein the mass ratio of raw material A to raw material B is 20:28;
[0100] The raw materials of the raw material A include high-density polyethylene, medium-density polyethylene, low-density polyethylene, carbon nanotube metal oxide composite thermal conductive filler, silane cross-linking agent, cross-linking catalyst, and antioxidant, and the mass ratio is 50:28:39:5.5:1.2:1.5:1.
[0101] The molecular weight of the high-density polyethylene is 2.5*10 5 , density is 0.937g / cm 3 ;
[0102] The molecular weight of the medium density polyethylene is 1.7*10 5 , density is 0.925g / cm 3 ;
[0103] The molecular weight of the low-density polyethylene is 5.2*10 4 , density is 0.912g / cm 3 ;
[0104] The silane crosslinking agent is vinyl trimethoxy silane;
[0105] The cross-linking catalyst is dibutyltin laurate maleate;
[0106] The antioxidant is antioxidant 1076.
[0107] The raw materials of the raw material B include medium-density polyethylene, low-density polyethylene, antioxidant, and lubricant, and the mass ratio is 60:38:0.6:1.2;
[0108] The molecular weight of the medium density polyethylene is 1.7*10 5 , density is 0.925g / cm 3 ;
[0109] The molecular weight of the low-density polyethylene is 5.2*10 4 , density is 0.912g / cm 3 ;
[0110] The antioxidant is antioxidant 1076;
[0111] The lubricant is low-density oxidized polyethylene wax with a density of 0.905 g / cm 3 .
[0112] The preparation method of the raw material A is:
[0113] The raw materials of raw material A are mixed according to a proportion, and after being mixed evenly, they are fed into an extruder, and the extrusion temperature is controlled to be 240° C., and extrusion is performed to obtain raw material A;
[0114] The preparation method of the raw material B is:
[0115] The raw materials of raw material B are mixed according to proportions, and after being evenly mixed, they are fed into an extruder, and the extrusion temperature is controlled to be 230° C., and extrusion is performed to obtain raw material B.
[0116] The preparation method of the carbon nanotube metal oxide composite thermal conductive filler is as follows:
[0117] The carbon nanotubes are mixed with deionized water, stirred to be evenly dispersed, and a carbon nanotube dispersion is obtained. Then, sodium lauryl polyether sulfate is added to the carbon nanotube dispersion, stirred until completely dissolved, and then the ultrasonic frequency is controlled to be 38kHz, and ultrasonication is performed for 20 minutes. After ultrasonication, the surface-treated carbon nanotubes are obtained by filtering, washing, and drying. Then, the surface-treated carbon nanotubes are added to a zirconium chloride solution, and the ultrasonic frequency is controlled to be 57kHz, and ultrasonication is performed for 70 minutes. After ultrasonication, the stirring speed is controlled to be 130r / min, and stirring is performed for 175 minutes. Then, filtering is performed, and the filter residue is dried at 89°C for 290 minutes. Then, the dried filter residue is heat-treated at 422°C in a nitrogen atmosphere for 290 minutes. After cooling, a carbon nanotube metal oxide composite thermal conductive filler is obtained.
[0118] The mass ratio of the carbon nanotubes to deionized water is 2:16;
[0119] The carbon nanotube has a length of 300 nm and a diameter of 40 nm;
[0120] The mass ratio of the carbon nanotube dispersion to sodium laureth sulfate is 60:3;
[0121] The mass ratio of the surface treated carbon nanotubes to the zirconium chloride solution is 17:48;
[0122] The concentration of the zirconium chloride solution is 5.5wt%.
[0123] The preparation method of the polyethylene pipe is:
[0124] The raw material A and the raw material B are mixed in proportion, and after being mixed evenly, they are fed into an extruder, and the extrusion temperature is controlled to be 245°C, and extrusion is performed to obtain a tube blank, and the tube blank is placed in an environment with a temperature of 25°C and a relative humidity of 70%, and cross-linked at room temperature for 80 hours, and a high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating is obtained after cross-linking;
[0125] The outer diameter of the tube blank is 40 mm and the wall thickness is 4.5 mm.
[0126] Comparative Example 1
[0127] Different from Example 1, the preparation method of the carbon nanotube metal oxide composite thermal conductive filler is changed to the following operation:
[0128] The carbon nanotubes and nano zirconium oxide are mixed and ground so that the ground particles are no longer than the length of the carbon nanotubes, thereby obtaining a carbon nanotube metal oxide composite thermal conductive filler;
[0129] The mass ratio of the surface treated carbon nanotubes to nano zirconium oxide is 17:2;
[0130] The particle size of the nano zirconium oxide is 50 nm.
[0131] Comparative Example 2
[0132] Different from Example 1, the preparation method of the carbon nanotube metal oxide composite thermal conductive filler is changed to the following operation:
[0133] The carbon nanotubes are mixed with deionized water, stirred to be uniformly dispersed, and then sodium dodecylbenzene sulfonate is added to the carbon nanotube dispersion, stirred until completely dissolved, and then the ultrasonic frequency is controlled to be 35kHz, and ultrasonication is performed for 17 minutes. After ultrasonication, the surface-treated carbon nanotubes are obtained by filtering, washing, and drying. The surface-treated carbon nanotubes are then added to an aluminum chloride solution, and the ultrasonic frequency is controlled to be 55kHz, and ultrasonication is performed for 75 minutes. After ultrasonication, the stirring speed is controlled to be 120r / min, and stirring is performed for 180 minutes. Then, the filter residue is dried at 85°C for 300 minutes, and then the dried filter residue is heat-treated at 415°C in a nitrogen atmosphere for 300 minutes. After cooling, the carbon nanotube metal oxide composite thermal conductive filler is obtained.
[0134] The mass ratio of the carbon nanotubes to deionized water is 2:15;
[0135] The carbon nanotubes have a length of 270 nm and a diameter of 35 nm;
[0136] The mass ratio of the carbon nanotube dispersion to sodium dodecylbenzene sulfonate is 55:3;
[0137] The mass ratio of the surface treated carbon nanotubes to the aluminum chloride solution is 17:45;
[0138] The concentration of the aluminum chloride solution is 5wt%.
[0139] Example 4 Thermal Conductivity Test
[0140] The thermal conductivity of the pipes of Examples 1-3 and Comparative Examples 1-2 was tested according to the method of GB / T3399-1982. The results are shown in Table 1.
[0141] Table 1
[0142] Group Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Thermal conductivity (W / m·K) 1.75 1.74 1.77 1.44 1.53
[0143] In Example 1-3, a carbon nanotube metal oxide composite thermal conductive filler is prepared, added to raw material A component, mixed with raw material B and extruded, and finally cross-linked to prepare a pipe. The pipe has good thermal conductivity and high thermal conductivity coefficient.
[0144] Comparative Example 1: A carbon nanotube metal oxide composite thermal conductive filler is obtained by grinding and mixing carbon nanotubes and nano zirconium oxide, adding the composite filler to raw material A, and then mixing and extruding with raw material B, and finally cross-linking to prepare a pipe. The thermal conductivity of the pipe is slightly improved, and the thermal conductivity coefficient is low;
[0145] Comparative Example 2 used aluminum chloride as the source of metal oxide, and finally prepared a thermally conductive filler composite of carbon nanotubes and aluminum oxide, which had a small improvement on the thermal conductivity of the tube and had a slightly low thermal conductivity coefficient.
[0146] Example 5 Hydrostatic Pressure Resistance Test
[0147] The pipes of Examples 1-3 and Comparative Examples 1-2 were tested for hydrostatic pressure resistance under different hydrostatic pressure stresses according to the method of GB / T18992.2-2003. The results are shown in Table 2.
[0148] Table 2
[0149] Group Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 12MPa / 20℃ / 1h No leakage, no cracking No leakage, no cracking No leakage, no cracking Slight leakage, no rupture Slight leakage, no rupture 4.8MPa / 95℃ / 1h No leakage, no cracking No leakage, no cracking No leakage, no cracking No leakage, no cracking No leakage, no cracking 4.7MPa / 95℃ / 22h No leakage, no cracking No leakage, no cracking No leakage, no cracking No leakage, no cracking No leakage, no cracking 4.6MPa / 95℃ / 165h No leakage, no cracking No leakage, no cracking No leakage, no cracking No leakage, no cracking No leakage, no cracking 4.4MPa / 95℃ / 1000h No leakage, no cracking No leakage, no cracking No leakage, no cracking Slight leakage, no rupture No leakage, no cracking
[0150] In Example 1-3, a carbon nanotube metal oxide composite thermal conductive filler is prepared, added to raw material A component, mixed with raw material B and extruded, and finally cross-linked to prepare a pipe. The pipe has good hydrostatic pressure resistance and does not leak or rupture under different test conditions.
[0151] Comparative Example 1: A carbon nanotube metal oxide composite thermal conductive filler is obtained by grinding and mixing carbon nanotubes and nano zirconium oxide, adding the composite thermal conductive filler to raw material A, and then mixing and extruding with raw material B, and finally cross-linking to prepare a pipe, resulting in poor hydrostatic pressure resistance of the pipe, especially in a short-term high-pressure environment, slight leakage will occur, and slight leakage will also occur in a long-term low-pressure environment;
[0152] Comparative Example 2 used aluminum chloride as the source of metal oxides, and finally prepared a thermally conductive filler composited with carbon nanotubes and aluminum oxide, which resulted in poor hydrostatic pressure resistance of the pipe, especially in a high-pressure environment for a short period of time, resulting in slight leakage.
[0153] Example 6 Heat resistance test
[0154] The thermal stability of the pipes of Examples 1-3 and Comparative Examples 1-2 was tested according to the method of GB / T18992.2-2003. The results are shown in Table 3.
[0155] Table 3
[0156] Group Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Hydrostatic stress / 2.5MPaTest temperature / 110℃Test time / 8760h No leakage, no cracking No leakage, no cracking No leakage, no cracking Slight leakage, no rupture Slight leakage, no rupture
[0157] In Example 1-3, a carbon nanotube metal oxide composite thermal conductive filler is prepared, added to raw material A component, mixed with raw material B and extruded, and finally cross-linked to prepare a pipe. The pipe has good heat resistance and does not leak or rupture in a long-term high temperature environment.
[0158] Comparative Example 1: A carbon nanotube metal oxide composite thermal conductive filler is obtained by grinding and mixing carbon nanotubes and nano zirconium oxide, adding the composite filler to raw material A, and then mixing and extruding with raw material B, and finally cross-linking to prepare a pipe, resulting in poor heat resistance of the pipe. In a high temperature environment for a long time, slight leakage may occur;
[0159] Comparative Example 2 used aluminum chloride as the source of metal oxide, and finally prepared a thermal conductive filler composite of carbon nanotubes and aluminum oxide, which resulted in poor heat resistance of the tube. In a high-temperature environment for a long time, slight leakage would occur.
[0160] Example 7 Bending Test
[0161] The pipes of Examples 1-3 and Comparative Examples 1-2 were tested according to the conditions of Level 5 in the method of GB / T18992.2-2003, and the bending parts of the pipes were observed for leakage and rupture. The test results are shown in Table 4.
[0162] Table 4
[0163] Group Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 20℃ / 1h No leakage, no cracking No leakage, no cracking No leakage, no cracking Slight leakage, no rupture No leakage, no cracking
[0164] In Example 1-3, a carbon nanotube metal oxide composite thermal conductive filler is prepared, added to raw material A component, mixed with raw material B and extruded, and finally cross-linked to prepare a pipe. The pipe has good bending resistance and no leakage or rupture occurs at the bend during the test.
[0165] Comparative Example 1: A carbon nanotube-metal oxide composite thermal conductive filler is obtained by grinding and mixing carbon nanotubes and nano zirconium oxide, adding the composite filler to raw material A, and then mixing and extruding with raw material B, and finally cross-linking to prepare a pipe, resulting in poor bending resistance of the pipe, and slight leakage occurred at the bend during the test;
[0166] Comparative Example 2 used aluminum chloride as the source of metal oxide, and finally prepared a thermally conductive filler composite of carbon nanotubes and aluminum oxide, which resulted in poor bending resistance of the tube and slight leakage at the bend during the test.
[0167] Example 8 Vacuum Test
[0168] The pipes of Examples 1-3 and Comparative Examples 1-2 were tested according to the method of GB / T18992.2-2003. The test temperature was 23°C, the test time was 1 hour, the test pressure was -0.08MPa, and the change in vacuum pressure in the pipe was counted after the test. The test results are shown in Table 5.
[0169] Table 5
[0170] Group Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Vacuum pressure change 0.001MPa 0.001MPa 0.001MPa 0.004MPa 0.003MPa
[0171] In Example 1-3, a carbon nanotube metal oxide composite thermal conductive filler is prepared, added to raw material A component, mixed with raw material B and extruded, and finally cross-linked to prepare a pipe. The pipe has good vacuum retention performance and small vacuum pressure change;
[0172] Comparative Example 1: A carbon nanotube-metal oxide composite thermal conductive filler is obtained by grinding and mixing carbon nanotubes and nano zirconium oxide, adding the composite filler to raw material A, and then mixing and extruding with raw material B, and finally cross-linking to prepare a pipe, resulting in poor vacuum holding performance of the pipe and large changes in vacuum pressure;
[0173] Comparative Example 2 used aluminum chloride as the source of metal oxide, and finally prepared a thermally conductive filler composite of carbon nanotubes and aluminum oxide, which resulted in poor vacuum holding performance of the tube and slightly larger vacuum pressure variation.
Claims
1. A high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating, characterized in that: The raw materials of the pipe are composed of raw material A and raw material B, wherein the mass ratio of raw material A to raw material B is 20:22-28; The raw materials of the raw material A include high-density polyethylene, medium-density polyethylene, low-density polyethylene, carbon nanotube metal oxide composite thermal conductive filler, silane crosslinking agent, crosslinking catalyst, and antioxidant, and the mass ratio is 40-50:22-28:31-39:4.5-5.5:0.8-1.2:1-1.5:0.7-1; The raw materials of the raw material B include medium-density polyethylene, low-density polyethylene, antioxidant, and lubricant, and the mass ratio is 50-60:31-38:0.4-0.6:0.8-1.2; The preparation method of the raw material A is: The raw materials of raw material A are mixed according to a proportion, and after being mixed evenly, they are fed into an extruder, and the extrusion temperature is controlled to be 230-240° C., and extrusion is performed to obtain raw material A; The preparation method of the raw material B is: The raw materials of raw material B are mixed according to the proportion, and after being mixed evenly, they are fed into an extruder, and the extrusion temperature is controlled to be 220-230° C., and extrusion is performed to obtain raw material B; The preparation method of the carbon nanotube metal oxide composite thermal conductive filler is as follows: The carbon nanotubes are mixed with deionized water, stirred to be evenly dispersed, and a carbon nanotube dispersion is obtained. Then, sodium lauryl polyether sulfate is added to the carbon nanotube dispersion, stirred until completely dissolved, and then the ultrasonic frequency is controlled to be 32-38kHz, and ultrasonication is performed for 15-20min. After ultrasonication, the surface-treated carbon nanotubes are obtained by filtering, washing, and drying. Then, the surface-treated carbon nanotubes are added to a zirconium chloride solution, and the ultrasonic frequency is controlled to be 52-57kHz, and ultrasonication is performed for 70-80min. After ultrasonication, stirring is performed, and then filtering is performed. The filter residue is dried at 82-89°C for 290-320min, and then the dried filter residue is heat-treated at 412-422°C in a nitrogen atmosphere for 290-320min. After cooling, the carbon nanotube metal oxide composite thermal conductive filler is obtained. The mass ratio of the carbon nanotubes to deionized water is 2:14-16; The mass ratio of the carbon nanotube dispersion to sodium laureth sulfate is 50-60:3; The mass ratio of the surface treated carbon nanotubes to the zirconium chloride solution is 17:42-46; The concentration of the zirconium chloride solution is 4.5-5.5wt%.
2. A high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating according to claim 1, characterized in that: In the raw material of raw material A, the molecular weight of high-density polyethylene is 2.5×10 5 , density is 0.937g / cm 3 ; The molecular weight of medium density polyethylene is 1.7×10 5 , density is 0.925g / cm 3 ; The molecular weight of low-density polyethylene is 5.2×10 4 , density is 0.912g / cm 3 ; The silane crosslinker is vinyltrimethoxysilane; The cross-linking catalyst is dibutyltin laurate maleate; The antioxidant is antioxidant 1076.
3. The high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating according to claim 1, characterized in that: In the raw material of the raw material B, the molecular weight of the medium density polyethylene is 1.7×10 5 , density is 0.925g / cm 3 ; The molecular weight of low-density polyethylene is 5.2×10 4 , density is 0.912g / cm 3 ; The antioxidant is antioxidant 1076; The lubricant is low-density oxidized polyethylene wax with a density of 0.905g / cm 3 .
4. The high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating according to claim 1, characterized in that: In the preparation method of the carbon nanotube-metal oxide composite thermal conductive filler, the length of the carbon nanotube is 250-300nm and the diameter is 30-40nm.
5. The high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating according to claim 1, characterized in that: In the preparation method of the carbon nanotube metal oxide composite thermal conductive filler, in the stirring step after ultrasonication, the stirring method is to control the stirring speed to 110-130 r / min, and stir for 175-195 min.
6. The method for preparing a high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating according to claim 1, characterized in that: The preparation method is: Raw material A and raw material B are mixed in proportion, and after being evenly mixed, they are fed into an extruder, and the extrusion temperature is controlled to be 235-245°C for extrusion to obtain a tube billet, and the tube billet is placed in an environment with a temperature of 18-25°C and a relative humidity of 60-70%, and cross-linked at room temperature for 70-80 hours. After cross-linking, a high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating is obtained.
7. The method for preparing a high thermal conductivity and high heat resistance cross-linked polyethylene pipe for water heating according to claim 6, characterized in that: The outer diameter of the tube blank is 40 mm and the wall thickness is 4.5 mm.