A TOPCon solar cell metallization method using silver-coated nickel paste and solar cell

By using silver-clad nickel powder and laser-enhanced sintering process, combined with nickel diffusion regulator, the line resistance problem caused by nickel powder oxidation in TOPCon solar cells is solved, reducing costs and improving conversion efficiency, and achieving higher battery performance.

CN118367063BActive Publication Date: 2024-11-22JINGLAN ADVANCED MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410619598.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-20
Publication Date
2024-11-22
Estimated Expiration
2044-05-20

AI Technical Summary

Technical Problem

During the high-temperature sintering process of TOPCon solar cells, nickel powder is easily oxidized to nickel oxide, resulting in an increase in line resistance, limiting the improvement of battery conversion efficiency. At the same time, silver paste is costly, making it difficult to reduce costs and improve efficiency at the same time.

Method used

Silver-clad nickel powder is used to replace silver powder, and nickel is formed into a nano-nickel tunneling layer through laser-enhanced sintering process, and the free nickel content is adjusted with nickel diffusion regulator, reducing line resistance and improving contact performance.

Benefits of technology

The production cost of TOPCon solar cells is reduced and the conversion efficiency is improved. The conductivity and oxidation resistance of silver-clad nickel powder are better than those of pure silver powder. The nano-nickel tunneling layer formed by the laser-enhanced sintering process reduces the contact resistance of the electrode, realizing the Higher conversion efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of solar cells, and specifically relates to a TOPCon solar cell metallization method and a solar cell using silver-coated nickel paste. A TOPCon solar cell metallization method using silver-coated nickel paste comprises the following steps: screen printing silver-coated nickel conductive paste on the surface of a TOPCon solar cell sheet, drying, sintering in air at 500-750°C to obtain a first sintered cell sheet; performing laser enhanced sintering on the first sintered cell sheet, and applying a reverse deflection voltage to complete the metallization of the TOPCon solar cell sheet. The present invention uses low-cost silver-coated nickel powder to replace silver powder, thereby reducing production costs. The conductivity and oxidation resistance of the silver-coated nickel powder are better than those of nickel powder, and the contact performance of the silver-coated nickel powder is better than that of pure silver powder. The present invention can simultaneously meet the needs of cost reduction and efficiency improvement of TOPCon solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solar cells, and in particular relates to a TOPCon solar cell metallization method using silver-coated nickel paste and a solar cell. Background Art

[0002] Among crystalline silicon solar cells, tunnel oxide passivated contact solar cells (TOPCon solar cells) are new high conversion efficiency cells. The tunnel oxide layer and passivation contact layer of TOPCon solar cells provide good surface passivation, greatly reducing metal contact recombination and improving the conversion efficiency of the cell.

[0003] In order to achieve high photoelectric conversion efficiency, the metallization of TOPCon solar cells currently mainly uses silver paste for screen printing, drying, and high-temperature sintering. Due to the high silver content in the paste, the metallization process cost of TOPCon solar cells is relatively high.

[0004] In order to reduce the silver content in the slurry, the patent with publication number CN114334215A discloses an electrode slurry for ohmic contact of the P-type emitter region of a silicon solar cell. The components (wt%) of the electrode slurry are: 78-89 metallic silver powder, 2-10 base metal powder, 0.5-5 glass powder, 0.5-3 additives, and 8-12 organic carriers. Base metal powder (one or more of Al powder, Ni powder, Cu powder, Sn powder, and Sb powder) is used to replace part of the silver powder, thereby reducing the cost of the electrode slurry. The base metal powder has a low melting point and is easy to form an alloy with silicon, which is beneficial to reducing the contact resistance of the electrode.

[0005] However, the inventors discovered during the research process that nickel powder is easily oxidized to nickel oxide during the metallization process of high-temperature sintering of TOPCon solar cells, which increases the line resistance of TOPCon solar cells and thus limits the improvement of the conversion efficiency of TOPCon solar cells. Summary of the invention

[0006] In order to simultaneously meet the requirements of cost reduction and efficiency improvement of TOPCon solar cells, the present invention provides a TOPCon solar cell metallization method using silver-coated nickel paste and a solar cell.

[0007] In a first aspect, the present invention provides a TOPCon solar cell metallization method using silver-coated nickel paste, which is implemented by the following technical solution:

[0008] A TOPCon solar cell metallization method using silver-coated nickel paste comprises the following steps:

[0009] The surface of the TOPCon solar cell is screen-printed with silver-coated nickel conductive paste, dried, and sintered in air at 500-750°C to obtain the first sintered cell;

[0010] The first sintered cell is subjected to laser enhanced sintering, and a reverse bias voltage is applied to complete the metallization of the TOPCon solar cell.

[0011] The present invention adopts low-cost silver-coated nickel powder to replace silver powder for TOPCon solar cell metallization, thereby reducing production costs. Compared with nickel powder, silver-coated nickel powder has better conductivity and oxidation resistance, reduces the line resistance of TOPCon solar cells, and improves the conversion efficiency of TOPCon solar cells. The high temperature generated instantly by the laser enhanced sintering process is conducive to the excitation of nickel in the silver-coated nickel powder into an ionic state, and diffuses to the interface between the battery cell and the grid line under the drive of bias voltage, and is reduced to nano-nickel particles by electron compensation in the photogenerated current, and the interface resistance is reduced by tunneling, so that the contact performance of the silver-coated nickel powder is better than that of pure silver powder, which is conducive to further reducing the contact resistance of the electrode and improving the conversion efficiency of the TOPCon solar cell. Therefore, the present invention can simultaneously meet the needs of cost reduction and efficiency improvement of TOPCon solar cells.

[0012] Preferably, the silver-coated nickel conductive paste comprises, by mass percentage, 25-95% silver-coated nickel powder, 0-70% silver powder, 1-6% glass powder, 0.1-3% organic resin, 0.1-1% dispersant, 0-5% nickel diffusion regulator and the remainder solvent.

[0013] More preferably, the content of nickel element in the silver-coated nickel conductive paste is not less than 24wt%; the content of silver-coated nickel powder in the silver-coated nickel conductive paste is 40-95wt%, the content of silver powder is 0-40wt%, and the content of nickel diffusion regulator is 0.01-5wt%.

[0014] In the present application, the nickel diffusion regulator is used to adjust the content of free nickel during the metallization process, and the free nickel forms a nano-nickel tunneling layer with controllable concentration and size under the action of the laser enhanced sintering process.

[0015] Adding nickel diffusion regulator to silver-coated nickel conductive paste can improve the conversion efficiency of TOPCon solar cells. Specifically, when the free nickel content is low, the nickel diffusion regulator can prevent nickel oxidation and ensure sufficient free nickel content to form a nano-nickel tunneling layer and improve contact performance; when the free nickel content is high, the nickel diffusion regulator can absorb and prevent excessive free nickel from diffusing, prevent the formation of large nickel metal particles that pierce the PN junction, and prevent the residual nickel from forming a "dead layer" that causes carrier recombination losses, thereby improving the conversion efficiency of TOPCon solar cells.

[0016] Preferably, the content of the nickel diffusion regulator is 0.1-5wt%.

[0017] More preferably, the content of the nickel diffusion regulator is 3-5wt%.

[0018] Preferably, the nickel diffusion regulator is selected from one or more of silver alloy powder, solid solution, polymer containing metal ions, and metal organic framework material.

[0019] More preferably, the nickel diffusion regulator is selected from one or more of silver alloy powder, solid solution, and polymer containing metal ions.

[0020] Preferably, the silver alloy powder is selected from one or more of silver-cerium alloy, silver-zinc alloy, silver-tin alloy, silver-magnesium alloy, silver-strontium alloy, silver-bismuth alloy, silver-lithium alloy and silver-cesium alloy.

[0021] More preferably, the silver alloy powder is silver-cerium alloy.

[0022] In the present application, the cerium content in the silver-cerium alloy is 0.3-0.8wt%; preferably, the cerium content in the silver-cerium alloy is 0.5wt%.

[0023] As a nickel diffusion regulator, silver-cerium alloy can adjust the nano-nickel tunneling layer by adjusting the content of free nickel in the silver-coated nickel powder during the metallization process. Specifically, the cerium in the silver-cerium alloy easily combines with oxygen, which can prevent nickel from oxidizing into nickel oxide. When the free nickel content is low, the silver-cerium alloy can prevent the free nickel from oxidizing, ensuring sufficient free nickel content to form a nano-nickel tunneling layer and improve contact performance; when the free nickel concentration is high, the microscopic cerium oxide atmosphere generated by the silver-cerium alloy can be coated on the surface of the silver-coated nickel powder and fill the gaps in the silver-coated nickel conductive paste during the metallization process. It can absorb and block the excessive free nickel from diffusing to the interface during the metallization process to form large-sized nickel metal particles that pierce the PN junction, affecting the efficiency of the solar cell, and preventing the residual nickel from forming a "dead layer" to cause carrier recombination losses. Therefore, as a nickel diffusion regulator, silver-cerium alloy can improve the conversion efficiency of TOPCon solar cells.

[0024] Preferably, the solid solution is selected from one or more of a silicate solid solution, a borate solid solution, and a plumbite solid solution.

[0025] As a nickel diffusion regulator, the solid solution has the characteristics of fixed melting point and controllable solubility. Under the same metallization conditions, the solid solution can control the total amount of free nickel absorbed by it through composition design and content adjustment. When the free nickel concentration is high, it can absorb excess free nickel to prevent the formation of large nickel metal particles that pierce the PN junction, and prevent the residual nickel from forming a "dead layer" that causes carrier recombination losses, thereby improving the conversion efficiency of TOPCon solar cells.

[0026] More preferably, the solid solution is a borate solid solution.

[0027] Preferably, the composition of the borate solid solution is represented by the chemical formula Si 0.8 Ti 0.2 B2O5.

[0028] Preferably, the polymer containing metal ions is selected from one or more of ethylene-acrylic acid copolymers containing sodium ions, ethylene-acrylic acid copolymers containing zinc ions, ethylene-methacrylic acid copolymers containing sodium ions, ethylene-methacrylic acid copolymers containing zinc ions, acrylic acid-ethylene-methacrylic acid copolymers containing sodium ions, acrylic acid-ethylene-methacrylic acid copolymers containing zinc ions, sulfonated polystyrene sodium salt ionomers, and sulfonated polystyrene zinc salt ionomers.

[0029] More preferably, the polymer containing metal ions is a polymer containing zinc ions; the polymer containing zinc ions is one or more of ethylene-acrylic acid copolymer containing zinc ions, ethylene-methacrylic acid copolymer containing zinc ions, and acrylic acid-ethylene-methacrylic acid copolymer containing zinc ions.

[0030] In the present application, the polymer containing zinc ions includes but is not limited to SURLYN™ 1652 Ionomer, SURLYN™ 1652SR Ionomer, SURLYN™ AD8273 Ionomer, SURLYN™ 1650 Ionomer, SURLYN™ 1702 Ionomer, SURLYN™ 1652SB Ionomer, SURLYN™ 1825 Ionomer, SURLYN™ 1706 Ionomer, SURLYN™ 9910 Ionomer, SURLYN™ 1705 Ionomer, SURLYN™ 1857 Ionomer, SURLYN™ 9320 Ionomer, SURLYN™ 9120 Ionomer, SURLYN™ 9020 Ionomer, SURLYN™ 9520 Ionomer, SURLYN™ 9720 Ionomer, SURLYN™ One or more of SURLYN™ 9910D Ionomer, SURLYN™ 9150 Ionomer, SURLYN™ 9945 Ionomer, SURLYN™ 9722 Ionomer, and SURLYN™ 1557 Ionomer.

[0031] The polymer containing zinc ions is used as a nickel diffusion regulator. During the metallization process, the zinc ions of the polymer containing zinc ions are converted into zinc oxide, and the generated zinc oxide can be coated on the surface of the silver-coated nickel powder to prevent the silver-coated nickel powder from generating excessive free nickel during the metallization process. At the same time, the carboxylic acid groups contained in the polymer containing zinc ions are converted into carbon dioxide during the metallization process. The generated carbon dioxide atmosphere can prevent the oxidation of nickel by oxygen and regulate the content of free nickel.

[0032] Preferably, the nickel diffusion regulator is a mixture of a solid solution and a polymer containing metal ions.

[0033] Preferably, the mass ratio of the solid solution to the polymer containing metal ions is (3-5):1.

[0034] More preferably, the mass ratio of the solid solution to the polymer containing metal ions is 3:1.

[0035] The nickel diffusion regulator is a compound of a solid solution and a polymer containing metal ions. The polymer containing metal ions can not only prevent the silver-coated nickel powder from generating excessive free nickel during the metallization process, but the polymer containing metal ions can also enhance the solid solubility of the solid solution, present a better diffusion control ability, better regulate the contact between free nickel and silicon, and form a nano-nickel tunneling layer with controllable concentration and size under the instantaneous action of the laser enhanced sintering process, better prevent the formation of large-sized nickel metal particles piercing the PN junction and affecting the efficiency of the solar cell, and better prevent the residual nickel from forming a "dead layer" causing carrier recombination loss, thereby further improving the conversion efficiency of the TOPCon solar cell.

[0036] Preferably, the content of silver-coated nickel powder in the silver-coated nickel conductive paste is 40-60wt%, and the content of silver powder is 20-40wt%; the content of silver in the silver-coated nickel powder is 10-40wt%.

[0037] Preferably, the content of nickel element in the silver-coated nickel conductive paste is 24-54wt%.

[0038] Preferably, the glass powder comprises PbO, B2O3, SiO2 and Al2O3.

[0039] More preferably, the composition of the glass powder also includes one or more of the following elements or compounds containing the elements: Zn, Sn, Ti, Ag, Ce, Cs, Cu, Fe, K, Na, Rb, Ge, Ga, In, Ni, Ca, Mg, Sr, Ba, Se, Mo, Y, As, La, Nd, Co, Pr, Gd, Sm, Dy, Eu, Ho, Yb, Lu, Ta, V, Hf, Cr, Cd, Sb, F, Zr, Mn, Ru, Re, Nb, Te, Li, Bi and W.

[0040] In the present application, the organic resin includes but is not limited to one or more of ethyl cellulose, ethyl hydroxyethyl cellulose, wood rosin, phenolic resin, and polymethacrylate of lower alcohol.

[0041] In the present application, the dispersant includes but is not limited to one or more of oleic acid, polyethylene wax, polyethylene glycol, and polyvinyl alcohol.

[0042] In the present application, the solvent includes but is not limited to one or more of terpene, kerosene, dibutyl phthalate, butyl carbitol, hexylene glycol, butyl carbitol acetate and alcohol ester.

[0043] Preferably, the sintering temperature in air is 600-700°C.

[0044] More preferably, the sintering temperature in air is 640°C.

[0045] Preferably, the TOPCon solar cell includes a solar cell with a front P region and a back N region, a solar cell with a front N region and a back P region, and a BC back contact solar cell with a back P region and a back N region.

[0046] In a second aspect, the present invention provides a solar cell, which is implemented by the following technical solution:

[0047] A solar cell is made by the above-mentioned TOPCon solar cell metallization method using silver-coated nickel paste.

[0048] In summary, the present invention has the following beneficial effects:

[0049] 1. The present invention uses low-cost silver-coated nickel powder to replace silver powder for TOPCon solar cell metallization, thereby reducing production costs. Compared with nickel powder, silver-coated nickel powder has better conductivity and oxidation resistance, which reduces the line resistance of TOPCon solar cells and improves the conversion efficiency of TOPCon solar cells. The high temperature and bias voltage generated instantly by the laser enhanced sintering process are conducive to the formation of a nano-nickel tunneling layer by the nickel in the silver-coated nickel powder, making the contact performance of the silver-coated nickel powder better than that of pure silver powder, which is conducive to further reducing the contact resistance of the electrode and improving the conversion efficiency of TOPCon solar cells, and can simultaneously meet the needs of cost reduction and efficiency improvement of TOPCon solar cells.

[0050] 2. Nickel diffusion regulator is used to adjust the content of free nickel in the metallization process. Under the action of laser enhanced sintering process, free nickel forms a nano nickel tunneling layer with controllable concentration and size. When the free nickel content is low, the nickel diffusion regulator can prevent the free nickel from oxidation, ensure a certain content of free nickel, so as to form a nano nickel tunneling layer and improve the contact performance; when the free nickel content is high, the nickel diffusion regulator can absorb and prevent the excessive free nickel from diffusing, prevent the formation of large nickel metal particles piercing the PN junction, and prevent the residual nickel from forming a "dead layer" to cause carrier recombination loss, thereby improving the conversion efficiency of TOPCon solar cells. DETAILED DESCRIPTION

[0051] The present invention is further described in detail below with reference to the embodiments.

[0052] Example

[0053] Example 1 provides a TOPCon solar cell metallization method using silver-coated nickel paste, the steps of which are:

[0054] S1. Silver-coated nickel conductive paste was screen-printed on the back of the TOPCon cell (screen parameters: 480 mesh 11μm screen wire diameter, 14μm yarn thickness, 4μm latex thickness, 148 22μm secondary grid lines and 16 main grid lines) at a belt speed of 12000mm / min and dried at a peak temperature of 200℃ for 30s.

[0055] S2. Silver-coated nickel conductive paste was screen-printed on the front side of the TOPCon cell with printed back grid lines using a screen (screen parameters: 480 mesh 11μm screen wire diameter, 14μm yarn thickness, 4μm latex thickness, 148 22μm secondary grid lines and 16 main grid lines) at a belt speed of 12000mm / min and dried at a temperature peak of 200℃ for 30s.

[0056] S3. Place the TOPCon cell obtained in step S2 in a sintering furnace and sinter it in an air atmosphere at a belt speed of 12000 mm / min, wherein the peak temperature is 500° C. and the sintering time is 1.5 min, to obtain the first sintered cell.

[0057] S4, performing laser enhanced sintering on the first sintered cell sheet, and applying a reverse deflection voltage to complete the metallization of the TOPCon solar cell sheet, wherein the laser beam power corresponding to the laser enhanced sintering is 30W, the scanning time of the laser beam is 1s, and the reverse deflection voltage is 20V.

[0058] The preparation steps of silver-coated nickel conductive paste are:

[0059] Sa. Weigh 40 g of silver-coated nickel powder, 40 g of silver powder, 2 g of glass powder, 1.5 g of organic resin, 0.5 g of dispersant, and 16 g of solvent.

[0060] Sb, first put the weighed glass powder, organic resin, dispersant and solvent into the wide-mouth bottle of the planetary mixer, then add the silver-coated nickel powder and silver powder into the wide-mouth bottle, and stir evenly with a scraper; then mix with the planetary mixer at 800rpm for 3min to obtain the sample slurry. Then grind the sample slurry with a three-roll grinder for 5 times, and test its grinding fineness is less than 10μm, and the Brookfield viscosity is between 300-350Pa.s, to obtain the silver-coated nickel conductive slurry.

[0061] Among them, the silver content of the silver-coated nickel powder is 40wt%;

[0062] The glass powder is made by mixing PbO, B2O3, SiO2, and Al2O3 in a mass ratio of 75:10:10:5, quenching, and grinding;

[0063] The organic resin is ethyl cellulose;

[0064] The dispersant is oleic acid;

[0065] The solvent is a mixture of butyl carbitol acetate and alcohol ester 12 in a mass ratio of 1:1.

[0066] Example 2 provides a TOPCon solar cell metallization method using silver-coated nickel paste, which is different from Example 1 only in that the composition of the silver-coated nickel conductive paste contains 0.1g of nickel diffusion regulator, and the nickel diffusion regulator is a silver-cerium alloy (cerium content is 0.5wt%); the mass of the solvent is 15.9g.

[0067] The preparation steps of silver-coated nickel conductive paste are:

[0068] Sa, weigh 40g silver-coated nickel powder, 40g silver powder, 2g glass powder, 1.5g organic resin, 0.5g dispersant, 0.1g nickel diffusion regulator, and 15.9g solvent.

[0069] Sb, first put the weighed glass powder, organic resin, dispersant, nickel diffusion regulator and solvent into the wide-mouth bottle of the planetary mixer, then add the silver-coated nickel powder and silver powder into the wide-mouth bottle, and stir evenly with a spatula; then mix with the planetary mixer at 800rpm for 3min to obtain the sample slurry. Then grind the sample slurry with a three-roll grinder for 5 times, and test its grinding fineness is less than 10μm, and the Brookfield viscosity is between 300-350Pa.s, to obtain the silver-coated nickel conductive slurry.

[0070] Example 3 provides a TOPCon solar cell metallization method using silver-coated nickel paste, which is different from Example 2 only in that: the mass of the nickel diffusion regulator is 3g, the mass of the solvent is 13g; the peak temperature of sintering in the air atmosphere in step S3 is 750°C, and the sintering time is 1.5min.

[0071] Example 4 provides a TOPCon solar cell metallization method using silver-coated nickel paste, which is different from Example 3 only in that the mass of the nickel diffusion regulator is 5 g and the mass of the solvent is 11 g.

[0072] Example 5 provides a TOPCon solar cell metallization method using silver-coated nickel paste, which is different from Example 3 only in that the nickel diffusion regulator is a copolymer containing zinc ions, SURLYN™ 1652 Ionomer, purchased from Dow Chemical Company, USA.

[0073] Example 6 provides a TOPCon solar cell metallization method using silver-coated nickel paste, which is different from Example 3 only in that the nickel diffusion regulator is a borate solid solution.

[0074] The preparation steps of borate solid solution are:

[0075] SiO2, TiO2 and B2O3 were mixed evenly in a molar ratio of 0.8:0.2:1, poured into a crucible, and then placed in a muffle furnace, heated to 1000°C, and kept warm for 2 hours. The sintered borate solid solution was then placed in a ball mill and ball milled for 24 hours to obtain a borate solid solution powder with a particle size of 1 μm.

[0076] Example 7 provides a TOPCon solar cell metallization method using silver-coated nickel paste, which is different from Example 6 only in that the nickel diffusion regulator is a mixture of a borate solid solution and a copolymer SURLYN™ 1652 Ionomer containing zinc ions, and the mass ratio of the borate solid solution to the copolymer SURLYN™ 1652 Ionomer containing zinc ions is 3:1.

[0077] Example 8 provides a TOPCon solar cell metallization method using silver-coated nickel paste, which is different from Example 7 only in that the silver content of the silver-coated nickel powder is 10wt%, the mass of the silver-coated nickel powder is 60g, and the mass of the silver powder is 20g.

[0078] Example 9 provides a TOPCon solar cell metallization method using silver-coated nickel paste, which is different from Example 7 only in that the silver content of the silver-coated nickel powder is 30wt%, the mass of the silver-coated nickel powder is 50g, and the mass of the silver powder is 30g.

[0079] Example 10 provides a TOPCon solar cell metallization method using silver-coated nickel paste, which is different from Example 7 only in that the peak temperature of sintering in air atmosphere in step S3 is 640° C. and the sintering time is 1.5 min.

[0080] Comparative Example

[0081] Comparative Example 1 provides a TOPCon solar cell metallization method using silver-coated nickel paste, the steps of which are:

[0082] S1. Screen-print silver-coated nickel conductive paste (same as in Example 1) on the back of the TOPCon solar cell using a screen (screen parameters: 480 mesh 11μm screen wire diameter, 14μm yarn thickness, 4μm latex thickness, 148 22μm secondary grid lines and 16 main grid lines), at a belt speed of 12000mm / min, and dry at a temperature peak of 200°C for 30s.

[0083] S2. Silver-coated nickel conductive paste (same as in Example 1) was screen-printed on the front side of the TOPCon cell with printed back grid lines using a screen (screen parameters: 480 mesh 11μm screen wire diameter, 14μm yarn thickness, 4μm latex thickness, 148 22μm secondary grid lines and 16 main grid lines), and dried at a peak temperature of 200°C for 30s at a belt speed of 12000mm / min.

[0084] S3. Place the TOPCon cell obtained in step S2 in a sintering furnace and sinter in an air atmosphere at a belt speed of 12000 mm / min, wherein the peak temperature is 500° C. and the sintering time is 1.5 min, thereby completing the metallization of the TOPCon solar cell.

[0085] Comparative Example 2 provides a TOPCon solar cell metallization method, the steps of which are:

[0086] S1. Screen print conductive paste 1 on the back of TOPCon cell (screen parameters: 480 mesh 11μm screen wire diameter, 14μm yarn thickness, 4μm latex thickness, 148 22μm secondary grid lines and 16 main grid lines) at a belt speed of 12000mm / min and dry at a temperature peak of 200℃ for 30s.

[0087] S2. On the front side of the TOPCon cell with printed back grid lines, screen-print conductive paste 1 using a screen (screen parameters: 480 mesh 11μm screen wire diameter, 14μm yarn thickness, 4μm latex thickness, 148 22μm secondary grid lines and 16 main grid lines), at a belt speed of 12000mm / min, and dry at a temperature peak of 200℃ for 30s.

[0088] S3. Place the TOPCon cell obtained in step S2 in a sintering furnace and sinter it in an air atmosphere at a belt speed of 12000 mm / min, wherein the peak temperature is 500° C. and the sintering time is 1.5 min, to obtain the first sintered cell.

[0089] S4, performing laser enhanced sintering on the first sintered cell sheet, and applying a reverse deflection voltage to complete the metallization of the TOPCon solar cell sheet, wherein the laser beam power corresponding to the laser enhanced sintering is 30W, the scanning time of the laser beam is 1s, and the reverse deflection voltage is 20V.

[0090] The preparation steps of the conductive paste 1 are as follows:

[0091] Sa, weigh 24g nickel powder, 56g silver powder, 2g glass powder, 1.5g organic resin, 0.5g dispersant, and 16g solvent.

[0092] Sb, first put the weighed glass powder, organic resin, dispersant and solvent into the wide-mouth bottle of the planetary mixer, then add nickel powder and silver powder into the wide-mouth bottle, and stir evenly with a spatula; then mix with the planetary mixer at 800 rpm for 3 minutes to obtain a sample slurry. Then grind the sample slurry with a three-roll grinder for 5 times, and test its grinding fineness is less than 10μm, and the Brookfield viscosity is between 300-350Pa.s, to obtain conductive slurry 1.

[0093] The glass powder is made by mixing PbO, B2O3, SiO2 and Al2O3 in a mass ratio of 75:10:10:5, quenching and grinding;

[0094] The organic resin is ethyl cellulose;

[0095] The dispersant is oleic acid;

[0096] The solvent is a mixture of butyl carbitol acetate and alcohol ester 12 in a mass ratio of 1:1.

[0097] Comparative Example 3 provides a TOPCon solar cell metallization method, the steps of which are:

[0098] S1. Screen print conductive paste 2 on the back of TOPCon solar cell using screen (screen parameters: 480 mesh 11μm screen wire diameter, 14μm yarn thickness, 4μm latex thickness, 148 22μm secondary grid lines and 16 main grid lines) at a belt speed of 12000mm / min, and dry at a temperature peak of 200℃ for 30s.

[0099] S2. Conductive paste 2 was screen-printed on the front side of the TOPCon cell with printed back grid lines using a screen (screen parameters: 480 mesh 11μm screen wire diameter, 14μm yarn thickness, 4μm latex thickness, 148 22μm secondary grid lines and 16 main grid lines) at a belt speed of 12000mm / min and dried at a peak temperature of 200℃ for 30s.

[0100] S3. Place the TOPCon cell obtained in step S2 in a sintering furnace and sinter it in an air atmosphere at a belt speed of 12000 mm / min, wherein the peak temperature is 750° C. and the sintering time is 1.5 min, to obtain the first sintered cell.

[0101] S4, performing laser enhanced sintering on the first sintered cell sheet, and applying a reverse deflection voltage to complete the metallization of the TOPCon solar cell sheet, wherein the laser beam power corresponding to the laser enhanced sintering is 30W, the scanning time of the laser beam is 1s, and the reverse deflection voltage is 20V.

[0102] The preparation steps of conductive paste 2 are:

[0103] Sa, weigh 80g silver powder, 2g glass powder, 1.5g organic resin, 0.5g dispersant, and 16g solvent.

[0104] Sb, first put the weighed glass powder, organic resin, dispersant and solvent into the wide-mouth bottle of the planetary mixer, then add the silver powder into the wide-mouth bottle and stir evenly with a spatula; then mix with the planetary mixer at 800 rpm for 3 minutes to obtain a sample slurry. Then grind the sample slurry with a three-roll grinder for 5 times, and test its grinding fineness to be less than 10 μm, and the Brookfield viscosity is between 300-350 Pa.s, to obtain conductive slurry 2.

[0105] The glass powder is made by mixing PbO, B2O3, SiO2 and Al2O3 in a mass ratio of 75:10:10:5, quenching and grinding;

[0106] The organic resin is ethyl cellulose;

[0107] The dispersant is oleic acid;

[0108] The solvent is a mixture of butyl carbitol acetate and alcohol ester 12 in a mass ratio of 1:1.

[0109] Performance testing

[0110] The electrical performance of the TOPCon solar cells produced by the metallization process of Examples 1-10 of the present invention and Comparative Examples 1-3 was tested.

[0111] 1. IV test

[0112] The solar cells were characterized at 25°C ± 1.0°C using a commercially available IV tester “YP-CX5000” from YP Intelligence. The stroboscopic pulse light simulated sunlight, and its AM1.5 intensity on the cell surface was known to be 1000 W / m 2 . In order to give the simulator this intensity, the strobe pulse light flashes several times in a short period of time until a stable level is reached which is monitored by the "1.0.0.0" software of the IV tester. The Yanpu IV tester uses a multi-point contact method to measure current (I) and voltage (V) to determine the IV curve of the battery. All values ​​are automatically determined from this curve with the aid of a running software package. As a reference standard, a calibrated solar cell obtained from ISE Freiburg and made of the same area size, the same wafer material and using the same front pattern was tested and the data compared with the certified values. At least 5 wafers processed in the very same way were measured and the data were analyzed by calculating the average of the values. The software provides values ​​for conversion efficiency, open circuit voltage, short circuit current, fill factor and line resistance.

[0113] Among them, the line resistance is calibrated by the resistance value between two adjacent main grids. Specifically, the resistance value between the 1st and 2nd main grids, the resistance value between the 2nd and 3rd main grids, the resistance value between the 3rd and 4th main grids, the resistance value between the 4th and 5th main grids, the resistance value between the 5th and 6th main grids and the average value of the resistance value between the 6th and 7th main grids are selected to represent the line resistance.

[0114] 2. Contact resistance

[0115] All equipment and materials were balanced in an air conditioning room at a temperature of 22 ± 1 ° C before measurement. In order to measure the contact resistance of the fired electrode on the doped front layer of the silicon solar cell, the MLR-5104 on-resistance test system from Xinchong Electronic Technology Co., Ltd. was used. The device applied the 4-point measurement principle to estimate the contact resistance by the transfer length method (TLM). In order to measure the contact resistance, two strips of 1 cm wide were cut from the wafer perpendicular to the printed grid lines of the wafer. Each strip was measured with an accuracy of 0.05 mm for its accurate width. The width of the fired secondary grid lines was measured at 3 different points on the strip using a digital microscope "VHX-970F" equipped with a wide-range zoom lens VH-Z250 from Keyence Corp. The width was measured 10 times at each point with 2-point measurements. The grid line width value is the average value of all 30 measurements. The contact resistance is calculated by the software package using the pointer number, the strip width and the distance between the printed secondary grids. The measuring current is set to 14 mA. A multi-contact measuring head suitable for contacting 11 adjacent grid lines is installed and made to contact 11 adjacent grid lines. 10 points equidistantly distributed on each bar are measured. After starting the measurement, the software determines the value (mohm) of the contact resistance for each point on the bar. The average value of all 20 points is used as the value of the contact resistance.

[0116] The test data of conversion efficiency, open circuit voltage, short circuit current, fill factor, line resistance and contact resistance of the crystalline silicon solar cells prepared in Examples 1-10 and Comparative Examples 1-3 are shown in Table 1, wherein Ncell refers to the conversion efficiency value, Uoc refers to the open circuit voltage value, Isc refers to the short circuit current value, FF refers to the fill factor value, Rgl refers to the line resistance value, and Rc refers to the contact resistance value.

[0117] Table 1 Data of electrical properties of Examples 1-10 and Comparative Examples 1-3

[0118] Ncell(%) Uoc(mV) Isc(A) FF(%) Rgl(mohm) Rc(mohm) Example 1 26.22 724.06 14.188 85.44 18.368 0.844 Example 2 26.25 724.89 14.179 85.50 18.556 0.819 Example 3 26.27 723.02 14.157 85.91 18.836 0.518 Example 4 26.30 725.50 14.190 85.53 24.818 0.516 Example 5 26.32 722.93 14.188 85.89 19.195 0.474 Example 6 26.32 722.72 14.190 85.92 24.737 0.473 Example 7 26.35 723.05 14.172 86.08 23.701 0.454 Example 8 26.31 722.54 14.192 85.88 25.284 0.509 Example 9 26.33 722.91 14.187 85.94 25.027 0.460 Example 10 26.38 723.12 14.166 86.24 24.984 0.451 Comparative Example 1 1.21 719.04 1.949 28.84 18.427 21.302 Comparative Example 2 23.72 701.92 13.608 83.11 54.269 3.001 Comparative Example 3 26.11 722.40 14.173 85.34 14.994 1.846

[0119] It can be seen from the experimental data of Example 1 and Comparative Example 1 that the only difference between Example 1 and Comparative Example 1 is that Example 1 has a laser enhanced sintering process, while Comparative Example 1 does not have a laser enhanced sintering process. The contact resistance of Example 1 is significantly lower than that of Comparative Example 1, and the filling factor, short-circuit current and conversion efficiency of Example 1 are significantly higher than those of Comparative Example 1, indicating that the laser enhanced sintering process is a necessary condition for forming a nano-nickel tunneling layer. The nano-nickel tunneling layer makes the contact performance of silver-coated nickel powder better than that of pure silver powder, reduces the contact resistance, and improves the filling factor and short-circuit current, thereby greatly improving the conversion efficiency of TOPCon solar cells.

[0120] From the experimental data of Example 1 and Comparative Example 2, it can be seen that Example 1 uses silver-coated nickel powder, and Comparative Example 2 uses nickel powder. The conversion efficiency, open circuit voltage, short circuit current, and fill factor of the TOPCon battery corresponding to Example 1 are all higher than those of Comparative Example 2. The line resistance and contact resistance of the TOPCon battery corresponding to Example 1 are all lower than those of Comparative Example 2, indicating that the silver-coated nickel powder has better conductivity and oxidation resistance than nickel powder. Nickel powder is easily oxidized to nickel oxide when sintered in air at 500°C. Nickel oxide cannot form a nano-nickel tunneling layer under the action of laser enhanced sintering process. Only free nickel can form a nano-nickel tunneling layer under the action of laser enhanced sintering process. Therefore, the silver-coated nickel powder reduces the line resistance and contact resistance of the TOPCon solar cell and improves the conversion efficiency of the TOPCon solar cell.

[0121] It can be seen from the experimental data of Example 1 and Comparative Example 3 that Example 1 uses silver-coated nickel powder sintered in air at 500°C, and Comparative Example 3 uses pure silver powder sintered in air at 750°C. The conversion efficiency, open circuit voltage, short circuit current, and filling factor of the TOPCon battery corresponding to Example 1 are all higher than those of Comparative Example 3, and the contact resistance of the TOPCon battery corresponding to Example 1 is significantly lower than that of Comparative Example 3, indicating that compared with pure silver powder sintered in air at 750°C, the contact performance of the nano-nickel tunneling layer formed by the silver-coated nickel powder under the laser enhanced sintering process is better than the contact performance of the silver-silicon alloy formed by the pure silver powder under the laser enhanced sintering process, and the filling factor of the TOPCon solar cell corresponding to the silver-coated nickel powder sintered in air at 500°C is high, thereby improving the conversion efficiency of the TOPCon solar cell.

[0122] It can be seen from the experimental data of Example 2 and Example 1 that, compared with Example 1, Example 2 only adds a nickel diffusion regulator, and the nickel diffusion regulator is a silver-cerium alloy, and the contact resistance of Example 2 is low, and the filling factor and conversion efficiency of Example 2 are high. This is because the cerium in the silver-cerium alloy is easily combined with oxygen when sintered in air at 500°C, and the silver-cerium alloy can prevent the oxidation of free nickel, ensure sufficient free nickel content, so as to form a nano-nickel tunneling layer, improve contact performance, and thus improve the conversion efficiency of the TOPCon solar cell.

[0123] It can be seen from the experimental data of Example 7 and Example 5-6 that Example 5 uses a copolymer containing zinc ions as a nickel diffusion regulator, Example 6 uses a borate solid solution as a nickel diffusion regulator, and Example 7 uses a mixture of a borate solid solution and a copolymer containing zinc ions as a nickel diffusion regulator. The contact resistance of the TOPCon solar cell corresponding to Example 7 is the lowest, and the filling factor, open circuit voltage and conversion efficiency are the highest. It is explained that the nickel diffusion regulator compounded with a borate solid solution and a copolymer containing zinc ions can further improve the conversion efficiency of the TOPCon solar cell. This is because the polymer containing zinc ions can not only prevent the silver-coated nickel powder from generating excessive free nickel during the metallization process, but also strengthen the solid solubility of the solid solution, and can present a more outstanding diffusion control ability, better regulate the contact between free nickel and silicon, and form a nano-nickel tunneling layer with controllable concentration and size under the instantaneous action of the laser enhanced sintering process, better prevent the formation of large-sized nickel metal particles to pierce the PN junction, affect the efficiency of the solar cell, and better prevent the residual nickel from forming a "dead layer" to cause carrier recombination loss.

[0124] It can be seen from the experimental data of Example 10 and Example 7 that the silver-coated nickel powder in Example 10 was sintered in the air at 640°C, and the silver-coated nickel powder in Example 7 was sintered in the air at 750°C. The conversion efficiency, open circuit voltage, and fill factor of the TOPCon solar cell corresponding to Example 10 were higher than those of Example 7, and the contact resistance and line resistance of the TOPCon solar cell corresponding to Example 10 were lower than those of Example 7. This indicates that the sintering of the silver-coated nickel powder in the air at 640°C is better matched with the laser enhanced sintering process, and the sintering in the air at 640°C can produce a better content of free nickel, and form a better nano-nickel tunneling layer under the instantaneous action of the laser enhanced sintering process, achieving better contact performance, and at the same time, the conductivity is also better.

[0125] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A TOPCon solar cell metallization method using silver-coated nickel paste, characterized in that: The steps include: The surface of the TOPCon solar cell is screen-printed with silver-coated nickel conductive paste, dried, and sintered in air at 500-750°C to obtain the first sintered cell; The first sintered cell is subjected to laser enhanced sintering, and a reverse bias voltage is applied to complete the metallization of the TOPCon solar cell; The silver-coated nickel conductive paste comprises, in terms of mass percentage, 25-95wt% of silver-coated nickel powder, 0-70wt% of silver powder, 1-6wt% of glass powder, 0.1-3wt% of organic resin, 0.1-1wt% of dispersant, 0.01-5wt% of nickel diffusion regulator and the remainder of solvent; the content of nickel element in the silver-coated nickel conductive paste is not less than 24wt%; The nickel diffusion regulator is selected from one or more of silver alloy powder, solid solution, polymer containing metal ions, and metal organic framework material.

2. A TOPCon solar cell metallization method using silver-coated nickel paste according to claim 1, characterized in that: The content of silver-coated nickel powder in the silver-coated nickel conductive paste is 40-95wt%, and the content of silver powder is 0-40wt%.

3. A TOPCon solar cell metallization method using silver-coated nickel paste according to claim 1, characterized in that: The silver alloy powder is selected from one or more of silver-cerium alloy, silver-zinc alloy, silver-tin alloy, silver-magnesium alloy, silver-strontium alloy, silver-bismuth alloy, silver-lithium alloy and silver-cesium alloy.

4. A TOPCon solar cell metallization method using silver-coated nickel paste according to claim 1, characterized in that: The solid solution is selected from one or more of a silicate solid solution, a borate solid solution, and a plumbite solid solution.

5. The method for metallizing a TOPCon solar cell using a silver-coated nickel paste according to claim 1, characterized in that: The polymer containing metal ions is selected from one or more of ethylene-acrylic acid copolymer containing sodium ions, ethylene-acrylic acid copolymer containing zinc ions, ethylene-methacrylic acid copolymer containing sodium ions, ethylene-methacrylic acid copolymer containing zinc ions, acrylic acid-ethylene-methacrylic acid copolymer containing sodium ions, acrylic acid-ethylene-methacrylic acid copolymer containing zinc ions, sulfonated polystyrene sodium salt ionomer, and sulfonated polystyrene zinc salt ionomer.

6. A TOPCon solar cell metallization method using silver-coated nickel paste according to claim 2, characterized in that: The content of silver-coated nickel powder in the silver-coated nickel conductive paste is 40-60wt%, and the content of silver powder is 20-40wt%; the content of silver in the silver-coated nickel powder is 10-40wt%.

7. A TOPCon solar cell metallization method using silver-coated nickel paste according to claim 6, characterized in that: The content of nickel element in the silver-coated nickel conductive paste is 24-54 wt %.

8. A TOPCon solar cell metallization method using silver-coated nickel paste according to claim 1 or 2, characterized in that: The glass powder comprises PbO, B2O3, SiO2 and Al2O3.

9. A TOPCon solar cell metallization method using silver-coated nickel paste according to claim 8, characterized in that: The composition of the glass powder also includes one or more of the following elements or compounds containing the elements: Zn, Sn, Ti, Ag, Ce, Cs, Cu, Fe, K, Na, Rb, Ge, Ga, In, Ni, Ca, Mg, Sr, Ba, Se, Mo, Y, As, La, Nd, Co, Pr, Gd, Sm, Dy, Eu, Ho, Yb, Lu, Ta, V, Hf, Cr, Cd, Sb, F, Zr, Mn, Ru, Re, Nb, Te, Li, Bi and W.

10. The method for metallizing a TOPCon solar cell using a silver-coated nickel paste according to claim 1, characterized in that: The sintering temperature in air is 600-700°C.

11. A TOPCon solar cell metallization method using silver-coated nickel paste according to claim 1, characterized in that: The TOPCon solar cell includes a solar cell with a front P region and a back N region, a solar cell with a front N region and a back P region, and a BC back contact solar cell with a back P region and a back N region.

12. A solar cell, characterized in that: The solar cell is prepared by the TOPCon solar cell metallization method using silver-coated nickel paste as described in any one of claims 1 to 11.