A kind of preparation method of synthetic borneol
By using the coordination effect of TiO2/γ-cyclodextrin-siliotungstic acid catalyst and lithium salt, the problem of harsh preparation conditions and unstable catalytic activity in the process of synthesis of hormonal brain is solved, and efficient and stable Longannaopynia synthesis, suitable for industrial promotion.
Patent Information
- Application Number
- CN202410464032.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-17
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-04-17
AI Technical Summary
The existing solid acid catalysts are harsh in the preparation conditions of the synthesis of ponchia, complex in the process of synthesis of ponchia, unstable catalytic activity, and risk of violent reaction exothermic and explosion. The catalysts are difficult to separate and recycle, resulting in low yield and poor quality of ponchia , it is difficult to achieve industrial promotion.
Using TiO2/γ-cyclodextrin-siliotungstic acid catalyst, the TiO2 and oxygen-tungsten groups are supported by γ-cyclodextrin as a support, providing polyacid properties and pore structure, improving catalytic activity and surface area, and combining the coordination of lithium salts Effects, a highly efficient and stable catalyst was prepared for the reaction of α-pinene with anhydrous oxalate and NaOH saponification.
The high-efficiency catalytic conversion rate of α-pinene exceeds 98%, the yield of hormonal brain exceeds 78%, the catalyst performance is stable, and the efficiency does not significantly decrease after 10 reuses, which avoids hazards and quality problems in the reaction and is suitable for industrial applications.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of borneol preparation, and in particular to a method for preparing synthetic borneol. Background Art
[0002] Borneol, also known as borneol, is a monoterpene alcohol with the effects of refreshing the mind, clearing away heat and relieving pain, and plays an important role in Chinese patent medicine preparations. In addition, borneol has the aroma of pine forest and camphor, and a slightly peppermint cool and spicy taste. It is an important raw material for high-grade fixatives and the preparation of high-grade perfumes. Since the Tang Dynasty, there have been records of using borneol as a precious medicinal material and precious incense in my country. With the development of the pharmaceutical and spice industries, the demand for borneol is increasing day by day. Natural borneol resources are scarce and the production cost is high, which cannot meet people's needs. Therefore, replacing natural borneol with synthetic borneol is an inevitable trend for future development. Using a-pinene and oxalic acid as raw materials to synthesize borneol is the most widely used method in industry. The key to the synthesis of this method is the catalytic esterification part. Therefore, the development of efficient catalysts suitable for industrialization has always been the goal of academia and industry.
[0003] At present, the research on the synthesis of borneol is mostly focused on the screening of catalysts. Since liquid catalysts are difficult to separate after the reaction, which hinders their industrial application, many studies have focused on the development of solid acid catalysts. Although there are many reports on the use of homemade solid acid catalysts to synthesize borneol, which not only has high catalytic activity but also is easy to separate, such as solid acid SO 4 2- / ZrO 2 -SnO 2 、SO 4 2- / TiO 2 -Al 2 O 3 、SO 4 2- / TiO 2 、SO 4 2- / Al 2 O 3 、SO 4 2- / TiO 2 -SiO 2 、SO 4 2- / ZrO 2 -La 2 O 3 , S 2 O 8 2- / ZrO 2 -NiO、La 3+ / CNMS-SO 3H catalyst, but it still has problems in terms of industrialization, the yield and quality control of borneol. This is because on the one hand, the preparation conditions of these solid acid catalysts are closely related to their catalytic activity, resulting in harsh preparation conditions of catalysts, complex process, inconvenient and uneconomical production, and the performance of catalysts is difficult to control, which is unfavorable for industrial promotion. On the other hand, these solid acid catalysts are used for the production process of synthetic borneol and there are many obvious defects, such as the presence of violent heat release in the reaction, the danger of material impact and explosion in the production process, or the presence of reaction is difficult to control, the borneol yield is low, or the content of positive borneol is low, or the catalyst is easily deactivated, and it is difficult to recycle and other shortcomings that are difficult to industrialization. High-quality borneol depends on the content of positive borneol, and the prerequisite for improving the content of positive borneol is to avoid the generation of camphene isoborneol ester as much as possible. Therefore, suitable catalysts should not only consider their catalytic performance, but also need to consider their catalytic selectivity, i.e., reduce the catalytic α-pinene isomerization to camphene reaction, so that the synthetic borneol prepared not only has high yield, but also has good quality. In addition, a good catalyst must not only meet the above conditions but also be easy to prepare, economical, have mild catalytic reaction conditions, be easy to separate the catalyst and product, and be reusable, which are advantages conducive to industrial promotion. Summary of the invention
[0004] In view of this, the present invention proposes a method for utilizing TiO 2 A new method for synthesizing borneol by α-pinene / anhydrous oxalate esterification-NaOH saponification reaction catalyzed by γ-cyclodextrin-silicotungstic acid solid catalyst.
[0005] The technical solution of the present invention is achieved as follows: The present invention provides a method for preparing a synthetic borneol, comprising the following steps:
[0006] S1, TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst catalyzes the esterification of α-pinene and anhydrous oxalate, after the reaction is completed, the catalyst is filtered off, and the filtrate is distilled to remove the light oil to obtain diborneol oxalate;
[0007] S2, adding diborneol oxalate to an anhydrous ethanol solution containing NaOH to carry out a saponification reaction, and distilling to obtain borneol after the saponification reaction is completed.
[0008] Specifically, TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst can improve the conversion rate of α-pinene and the yield of borneol, because TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst uses γ-cyclodextrin as a carrier and loads TiO 2 , titanium oxide groups and tungsten oxide groups. The titanium oxide groups and tungsten oxide groups make the catalyst polyacidic, providing more catalytic active sites, making it easier for the catalyst to react with the reactants, thereby improving the catalytic efficiency. 2The pores of the catalyst are increased, the surface properties of the catalyst are improved, and the surface area of the catalyst is increased, thereby enhancing the contact between the catalyst and the reactants and promoting the reaction.
[0009] Based on the above technical solution, preferably, in step S1, the α-pinene: TiO 2 The mass ratio of / γ-cyclodextrin-silicotungstic acid catalyst: anhydrous oxalic acid is 1: (0.03-0.05): (0.3-0.5).
[0010] On the basis of the above technical solution, preferably, the temperature of the esterification reaction in step S1 is 60-70° C. for 0.5-1 h, 70-80° C. for 1-3 h, and 80-100° C. for 4-6 h.
[0011] Based on the above technical solution, preferably, the mass concentration of the anhydrous ethanol solution of NaOH in step S2 is 20%-30%, and the mass ratio of the anhydrous ethanol solution of diborneol oxalate:NaOH is (3-5):(1-2).
[0012] Based on the above technical solution, preferably, in step S2, the saponification reaction temperature is 60-80° C., and the reaction time is 1-2 h.
[0013] On the basis of the above technical solution, preferably, the TiO 2 The preparation method of the γ-cyclodextrin-silicotungstic acid catalyst comprises the following steps:
[0014] S11, adding n-butanol to the γ-cyclodextrin aqueous solution and stirring evenly, then slowly adding ethyl titanate dropwise, and stirring under alkaline conditions to react to form a gel, filtering after the reaction, drying and calcining to obtain TiO 2 / γ-cyclodextrin;
[0015] S12, the TiO 2 / γ-cyclodextrin was immersed in an alcohol solution of silicotungstic acid for reaction. After the reaction was completed, it was filtered, washed with water until neutral, dried, and calcined to obtain TiO 2 / γ-cyclodextrin-silicotungstic acid.
[0016] On the basis of the above technical solution, preferably, after drying in step S12, lithium salt and the dried solid powder are mixed in a mass ratio of 1: (5-8), and then calcined to obtain lithium salt-TiO 2 / γ-cyclodextrin-silicotungstic acid.
[0017] Specifically, the lithium ions in the lithium salt can react with TiO 2The active centers in the / γ-cyclodextrin-silicotungstic acid catalyst form coordination bonds, which enhances the activity of the catalyst. This coordination effect can promote the reaction and improve the efficiency of the catalyst. Lithium salts can improve the surface properties of the catalyst and increase the surface area of the catalyst, thereby enhancing the contact between the catalyst and the reactants and promoting the reaction. In addition, lithium salts can also enhance the TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst stability, protect the catalyst active center from being easily affected by reaction conditions, prevent the catalyst from being contaminated or corroded, maintain the activity of the catalyst, and thus extend the service life and catalytic efficiency of the catalyst.
[0018] On the basis of the above technical solution, preferably, in step S11, the mass fraction of the γ-cyclodextrin aqueous solution is 30%-50%, and the volume ratio of the γ-cyclodextrin aqueous solution: n-butanol: ethyl titanate is 1:(2-3):(5-7).
[0019] Based on the above technical solution, preferably, in step S12, the concentration of the alcohol solution of silicotungstic acid is 0.01-0.03 mol / L, TiO 2 The mass ratio of / γ-cyclodextrin: silicotungstic acid alcohol solution is 1:(15-20); the soaking temperature is 30-40℃, the soaking time is 4-8h; the drying temperature is 100-110℃, and the time is 1-3h.
[0020] On the basis of the above technical solution, preferably, the calcination temperature and time in step S12 are 40-60°C, 1h; 60-100°C, 1h; 100-300°C, 1h; 300-500°C, 1h.
[0021] The method for preparing a synthetic borneol of the present invention has the following beneficial effects compared with the prior art:
[0022] The TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst uses γ-cyclodextrin as a carrier and loads TiO 2 , titanium oxide groups and tungsten oxide groups, providing more catalytic active sites, increasing the surface area of the catalyst, making it easier for the catalyst to react with the reactants, and thus improving the catalytic efficiency. The catalyst of the present invention has strong catalytic activity, the conversion rate of α-pinene exceeds 98%, and the yield of borneol exceeds 78%; the catalyst performance is stable, and after repeated use for 10 times, the conversion rate of α-pinene, the yield of borneol and the yield of normal borneol are not significantly reduced.
[0023] Lithium salts can improve TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst surface properties, increase the surface area of the catalyst, thereby enhancing the contact between the catalyst and the reactants and promoting the reaction. Lithium salts can also protect the active center of the catalyst from contamination or corrosion, maintain the activity of the catalyst, and thus extend the service life and catalytic efficiency of the catalyst.
[0024] Compared with the existing solid catalyst, the catalyst lithium salt-TiO 2 / γ-cyclodextrin-silicotungstic acid avoids many obvious shortcomings of the synthetic catalysts currently used in the production process of synthetic borneol, such as the synthetic process of the synthetic catalyst is closely related to the catalytic activity, resulting in harsh synthetic process, unstable catalytic activity, or the catalytic synthesis of borneol reaction is difficult to control, the production process has the risk of material impact and explosion, or the catalyst is difficult to separate, or the product quality is poor (high isoborneol content) and other defects. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The reagents used in the present invention are all purchased from the market, wherein α-pinene is purchased from Hubei Wonder Chemical Co., Ltd. with a purity of 99%; γ-cyclodextrin is purchased from Hubei Hengshuo Chemical Co., Ltd., and silicotungstic acid is purchased from Wuhan Xingzhongcheng Technology Co., Ltd.
[0027] Example 1
[0028] The preparation method of the synthetic borneol of the present embodiment comprises the following steps:
[0029] S1, Preparation of TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst
[0030] S11, add 20 mL of n-butanol to 10 mL of 30% γ-cyclodextrin aqueous solution and stir evenly, then slowly drop 50 mL of ethyl titanate, and stir to react under alkaline conditions of pH 8 to form a gel. After the reaction is completed, filter, dry and calcine to obtain TiO 2 / γ-cyclodextrin. The calcination heating time is 40-60℃, 1h; 60-100℃, 1h; 100-300℃, 1h; 300-500℃, 1h.
[0031] S12, take 10g TiO 2 / γ-cyclodextrin was immersed in 150g of 0.03mol / L silicotungstate alcohol solution, reacted at 30℃ for 8h, filtered after the reaction, washed with water until neutral, dried at 100℃ for 1h, and calcined to obtain TiO 2 / γ-cyclodextrin-silicotungstic acid. The calcination temperature and time are 40-60°C, 1h; 60-100°C, 1h; 100-300°C, 1h; 300-500°C, 1h.
[0032] S2, esterification reaction
[0033] 20g α-pinene, 0.6g TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst and 6g of anhydrous oxalic acid were added into the reactor for esterification reaction. The temperature and time of the esterification reaction were as follows: 60℃ for 0.5h, 70℃ for 1h, and 80℃ for 4h. After the reaction, the catalyst was filtered out and the filtrate was distilled with water vapor to remove the light oil to obtain diborneol oxalate.
[0034] S3, saponification reaction
[0035] Diborneol oxalate was added to an anhydrous ethanol solution containing 20% NaOH, and the saponification reaction was carried out at 60°C for 1 hour. The mass ratio of diborneol oxalate:NaOH was 3:1. After the saponification reaction, borneol was obtained by distillation.
[0036] Example 2
[0037] The preparation method of the synthetic borneol of the present embodiment comprises the following steps:
[0038] S1, Preparation of TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst
[0039] S11, add 20 mL of n-butanol to 10 mL of 30% γ-cyclodextrin aqueous solution and stir evenly, then slowly drop 50 mL of ethyl titanate, and stir to react under alkaline conditions of pH 8 to form a gel. After the reaction is completed, filter, dry and calcine to obtain TiO 2 / γ-cyclodextrin. The calcination heating time is 40-60℃, 1h; 60-100℃, 1h; 100-300℃, 1h; 300-500℃, 1h.
[0040] S12, take 10g TiO 2 / γ-cyclodextrin was immersed in 150g of an alcohol solution of 0.03mol / L silicotungstic acid, and reacted at 30°C for 8h. After the reaction, it was filtered, washed with water until neutral, and dried at 100°C for 1h. After drying, lithium chloride was mixed with the dried solid powder in a mass ratio of 1:5, and the mixture was calcined to obtain TiO containing lithium chloride.2 / γ-cyclodextrin-silicotungstic acid catalyst. The calcination temperature and time are 40-60℃, 1h; 60-100℃, 1h; 100-300℃, 1h; 300-500℃, 1h.
[0041] S2, esterification reaction
[0042] 20g α-pinene, 0.6g TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst and 6g of anhydrous oxalic acid were added into the reactor for esterification reaction. The temperature and time of the esterification reaction were as follows: 60℃ for 0.5h, 70℃ for 1h, and 80℃ for 4h. After the reaction, the catalyst was filtered out and the filtrate was distilled with water vapor to remove the light oil to obtain diborneol oxalate.
[0043] S3, saponification reaction
[0044] Diborneol oxalate was added to an anhydrous ethanol solution containing 20% NaOH, and the saponification reaction was carried out at 60°C for 1 hour. The mass ratio of diborneol oxalate:NaOH was 3:1. After the saponification reaction, borneol was obtained by distillation.
[0045] Example 3
[0046] The preparation method of the synthetic borneol of the present embodiment comprises the following steps:
[0047] S1, Preparation of TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst
[0048] S11, 22 mL of n-butanol was added to 10 mL of a 35% γ-cyclodextrin aqueous solution and stirred evenly, then 55 mL of ethyl orthotitanate was slowly added dropwise, and stirred under alkaline conditions of pH 9 to react to form a gel. After the reaction was completed, the gel was filtered, dried and calcined to obtain TiO 2 / γ-cyclodextrin. The calcination temperature and time are 40-60°C, 1h; 60-100°C, 1h; 100-300°C, 1h; 300-500°C, 1h.
[0049] S12, take 10g TiO 2 / γ-cyclodextrin was immersed in 160g of an alcohol solution of 0.02mol / L silicotungstic acid, and reacted at 335°C for 7h. After the reaction, the mixture was filtered, washed with water until neutral, and dried at 105°C for 2h. After drying, lithium chloride was mixed with the dried solid powder in a mass ratio of 1:6, and the mixture was calcined to obtain TiO containing lithium salt. 2 / γ-cyclodextrin-silicotungstic acid. The calcination temperature and time are 40-60°C, 1h; 60-100°C, 1h; 100-300°C, 1h; 300-500°C, 1h.
[0050] S2, esterification reaction
[0051] 20g α-pinene, 0.7g TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst and 7g of anhydrous oxalic acid were added into the reactor for esterification reaction. The temperature and time of the esterification reaction were as follows: 65°C for 1h, 75°C for 2h, and 85°C for 5h. After the reaction, the catalyst was filtered out and the filtrate was distilled with water vapor to remove the light oil to obtain diborneol oxalate.
[0052] S3, saponification reaction
[0053] Diborneol oxalate was added to an anhydrous ethanol solution containing 25% NaOH, and the saponification reaction was carried out at 70°C for 1.5 hours. The mass ratio of diborneol oxalate:NaOH was 4:1. After the saponification reaction, borneol was obtained by distillation.
[0054] Example 4
[0055] The preparation method of the synthetic borneol of the present embodiment comprises the following steps:
[0056] S1, Preparation of TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst
[0057] S11, add 25 mL of n-butanol to 10 mL of 40% γ-cyclodextrin aqueous solution and stir evenly, then slowly drop 60 mL of ethyl titanate, and stir to react under alkaline conditions of pH 10 to form a gel. After the reaction is completed, filter, dry and calcine to obtain TiO 2 / γ-cyclodextrin. The calcination temperature and time are 40-60°C, 1h; 60-100°C, 1h; 100-300°C, 1h; 300-500°C, 1h.
[0058] S12, take 10g TiO 2 / γ-cyclodextrin was immersed in 180g of an alcohol solution of 0.01mol / L silicotungstic acid, and reacted at 40°C for 8h. After the reaction, it was filtered, washed with water until neutral, and dried at 110°C for 1h. After drying, lithium chloride was mixed with the dried solid powder in a mass ratio of 1:7, and the mixture was calcined to obtain TiO containing lithium salt. 2 / γ-cyclodextrin-silicotungstic acid. The calcination temperature and time are 40-60°C, 1h; 60-100°C, 1h; 100-300°C, 1h; 300-500°C, 1h.
[0059] S2, esterification reaction
[0060] 20g α-pinene, 0.8g TiO2 / γ-cyclodextrin-silicotungstic acid catalyst and 9g of anhydrous oxalic acid were added into the reactor for esterification reaction. The temperature and time of the esterification reaction were as follows: 70℃ for 1h, 80℃ for 3h, and 90℃ for 6h. After the reaction, the catalyst was filtered out and the filtrate was distilled with water vapor to remove the light oil to obtain diborneol oxalate.
[0061] S3, saponification reaction
[0062] Diborneol oxalate was added to an anhydrous ethanol solution containing 30% NaOH, and the saponification reaction was carried out at 80°C for 2 hours. The mass ratio of diborneol oxalate:NaOH was 5:1. After the saponification reaction, borneol was obtained by distillation.
[0063] Example 5
[0064] The preparation method of the synthetic borneol of the present embodiment comprises the following steps:
[0065] S1, Preparation of TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst
[0066] S11, 28 mL of n-butanol was added to 10 mL of a 45% γ-cyclodextrin aqueous solution and stirred evenly, then 65 mL of ethyl orthotitanate was slowly added dropwise, and stirred to react under alkaline conditions of pH 9 to form a gel. After the reaction was completed, the mixture was filtered, dried and calcined to obtain TiO 2 / γ-cyclodextrin. The calcination temperature and time are 40-60°C, 1h; 60-100°C, 1h; 100-300°C, 1h; 300-500°C, 1h.
[0067] S12, take 10g TiO 2 / γ-cyclodextrin was immersed in 190g of an alcohol solution of 0.02mol / L silicotungstic acid, and reacted at 40°C for 8h. After the reaction, it was filtered, washed with water until neutral, and dried at 110°C for 1h. After drying, lithium chloride was mixed with the dried solid powder in a mass ratio of 1:8, and the mixture was calcined to obtain TiO containing lithium salt. 2 / γ-cyclodextrin-silicotungstic acid. The calcination temperature and time are 40-60°C, 1h; 60-100°C, 1h; 100-300°C, 1h; 300-500°C, 1h.
[0068] S2, esterification reaction
[0069] 20g α-pinene, 0.9g TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst and 8g of anhydrous oxalic acid were added into the reactor for esterification reaction. The temperature and time of the esterification reaction were as follows: 70°C for 1h, 80°C for 2h, and 100°C for 5h. After the reaction, the catalyst was filtered out, and the filtrate was distilled with water vapor to remove the light oil to obtain diborneol oxalate.
[0070] S3, saponification reaction
[0071] Diborneol oxalate was added to an anhydrous ethanol solution containing 26% NaOH, and the saponification reaction was carried out at 80°C for 1 hour. The mass ratio of diborneol oxalate:NaOH was 5:2. After the saponification reaction, borneol was obtained by distillation.
[0072] Example 6
[0073] The preparation method of the synthetic borneol of the present embodiment comprises the following steps:
[0074] S1, Preparation of TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst
[0075] S11, 30 mL of n-butanol was added to 10 mL of 50% γ-cyclodextrin aqueous solution and stirred evenly, then 70 mL of ethyl orthotitanate was slowly added dropwise, and stirred to react under alkaline conditions of pH 10 to form a gel. After the reaction was completed, the gel was filtered, dried and calcined to obtain TiO 2 / γ-cyclodextrin. The calcination temperature and time are 40-60°C, 1h; 60-100°C, 1h; 100-300°C, 1h; 300-500°C, 1h.
[0076] S12, take 10g TiO 2 / γ-cyclodextrin was immersed in 200g of an alcohol solution of 0.01-0.03mol / L silicotungstic acid, reacted at 40°C for 6h, filtered after the reaction, washed with water until neutral, and dried at 100°C for 3h; after drying, lithium chloride was mixed with the dried solid powder in a mass ratio of 1:6, and calcined after mixing to obtain TiO containing lithium salt 2 / γ-cyclodextrin-silicotungstic acid. The calcination temperature and time are 40-60°C, 1h; 60-100°C, 1h; 100-300°C, 1h; 300-500°C, 1h.
[0077] S2, esterification reaction
[0078] 20g α-pinene, 1g TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst and 10g of anhydrous oxalic acid were added into the reactor for esterification reaction. The temperature and time of the esterification reaction were as follows: 60°C for 40min, 80°C for 3h, and 100°C for 6h. After the reaction, the catalyst was filtered out, and the filtrate was distilled with water vapor to remove the light oil to obtain diborneol oxalate.
[0079] S3, saponification reaction
[0080] Diborneol oxalate was added to an anhydrous ethanol solution containing 30% NaOH, and the saponification reaction was carried out at 80°C for 1 hour. The mass ratio of diborneol oxalate:NaOH was 2:1. After the saponification reaction, borneol was obtained by distillation.
[0081] Example 7
[0082] The preparation method of the synthetic borneol of the present embodiment comprises the following steps:
[0083] S1, Preparation of TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst
[0084] S11, 20 mL of n-butanol was added to 10 mL of 50% γ-cyclodextrin aqueous solution and stirred evenly, then 60 mL of ethyl orthotitanate was slowly added dropwise, and stirred under alkaline conditions of pH 10 to react to form a gel. After the reaction was completed, the gel was filtered, dried and calcined to obtain TiO 2 / γ-cyclodextrin. The calcination temperature and time are 40-60°C, 1h; 60-100°C, 1h; 100-300°C, 1h; 300-500°C, 1h.
[0085] S12, take 10g TiO 2 / γ-cyclodextrin was immersed in 180g of an alcohol solution of 0.03mol / L silicotungstic acid, and reacted at 40°C for 6h. After the reaction, it was filtered, washed with water until neutral, and dried at 105°C for 2h. After drying, lithium chloride was mixed with the dried solid powder in a mass ratio of 1:7, and the mixture was calcined to obtain TiO containing lithium salt. 2 / γ-cyclodextrin-silicotungstic acid. The calcination temperature and time are 40-60°C, 1h; 60-100°C, 1h; 100-300°C, 1h; 300-500°C, 1h.
[0086] S2, esterification reaction
[0087] 20g α-pinene, 1g TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst and 10g anhydrous oxalic acid were added into the reactor for esterification reaction. The temperature and time of the esterification reaction were as follows: 65℃ for 50min, 80℃ for 2h, and 95℃ for 5h. After the reaction, the catalyst was filtered out and the filtrate was distilled with water vapor to remove the light oil to obtain diborneol oxalate.
[0088] S3, saponification reaction
[0089] Diborneol oxalate was added to an anhydrous ethanol solution containing 30% NaOH, and the saponification reaction was carried out at 80°C for 1 hour. The mass ratio of diborneol oxalate:NaOH was 3:2. After the saponification reaction, borneol was obtained by distillation.
[0090] Comparative Example 1
[0091] The difference between Comparative Example 1 and Example 1 is that the catalyst TiO 2 / γ-cyclodextrin, no silicotungstic acid, catalyst TiO 2 The preparation method of / γ-cyclodextrin does not include step S12, and the rest of the contents are the same as those in Example 1.
[0092] Comparative Example 2
[0093] The difference between Comparative Example 2 and Example 1 is that γ-cyclodextrin is replaced by microcrystalline cellulose, and the rest of the contents are the same.
[0094] Comparative Example 3
[0095] The difference between Comparative Example 3 and Example 1 is that sulfuric acid is used to replace silicotungstic acid, and the rest of the contents are the same.
[0096] Comparative Example 4
[0097] The difference between Comparative Example 4 and Example 1 is that TiO 2 The amount of / γ-cyclodextrin-silicotungstic acid exceeds the range specified in this application, α-pinene: TiO 2 The mass ratio of / γ-cyclodextrin-silicotungstic acid catalyst is 1:0.08, the specific dosage is 16g, and the other steps are the same.
[0098] Comparative Example 5
[0099] The difference between Comparative Example 5 and Example 2 is that the lithium salt is replaced by ammonium chloride, and the other steps are the same.
[0100] Comparative Example 6
[0101] The difference between Comparative Example 6 and Example 2 is that the lithium salt is replaced by the iron salt ferric chloride, and the other steps are the same.
[0102] The product was qualitatively analyzed by gas chromatography-mass spectrometry in combination with the gas chromatography retention time of the standard product, and the product was quantitatively analyzed by gas chromatography. The conversion rate of α-pinene, the yields of borneol, n-borneol and isoborneol can be obtained by calculation. The results are shown in the table below.
[0103] Table 1 Content of synthetic borneol
[0104]
[0105] As shown in Table 1, the yield of borneol synthesized in the embodiment of the present invention is more than 70%, and the conversion rate is more than 98%. The best embodiment is Example 7, with a conversion rate of 99.98% and a yield of 79.48. The yield of Example 2 is significantly higher than that of Example 1, indicating that the addition of lithium salt increases the amount of TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst, which is due to the lithium salt improving the catalytic performance of TiO 2 The surface properties of the / γ-cyclodextrin-silicotungstic acid catalyst increase the surface area of the catalyst, enhance the contact between the catalyst and the reactants, and promote the reaction. The yield and conversion rate of borneol synthesized in Comparative Examples 1-4 are significantly lower than those in Examples 1-7, which proves that TiO 2 / Technical effect of γ-cyclodextrin-silicotungstic acid catalyst. Comparative Examples 5-6 show that the effect of lithium salt is significantly higher than that of ammonium salt and iron salt. This is because lithium salt has higher ionic charge density and smaller ionic radius than ammonium salt and iron salt, and is more likely to react with other compounds in the catalyst, thereby improving the activity and selectivity of the catalyst; lithium salt has stronger polarity and can more effectively interact with the bonds between reactant molecules to promote the reaction.
[0106] Catalyst reuse results: The catalysts prepared in the examples and comparative examples were subjected to ten repeated catalytic esterification-saponification reactions according to the corresponding methods. After the tenth catalysis-saponification, the conversion rate of α-pinene, the yields of borneol, orthoborneol and isoborneol were detected, and the results are as follows.
[0107] Table 2 Catalytic performance after catalyst was reused 10 times
[0108]
[0109] As shown in Table 2, when the catalyst synthesized in Example 1 is reused for the tenth time, the conversion rate decreases by 2.39%, the yield decreases by 5.36%, and the catalytic effect of the catalyst is significantly reduced. When the catalyst synthesized in Examples 2 and 7 is reused for the tenth time, the conversion rate is almost unaffected, and the yield only decreases by about 2%. This is because lithium salts also improve the stability of the catalyst and extend the service life of the catalyst. Lithium salts reduce the deactivation of the catalyst during the reaction, prevent the catalyst from being contaminated or corroded, and play a role in maintaining the activity of the catalyst. Therefore, adding lithium salts to the catalyst can improve the performance of the catalyst and make the catalytic reaction more efficient and stable. As can be seen from Comparative Examples 5-6, the catalyst repetition effect is better after adding lithium salts. This is because lithium salts are more stable in the catalyst than ammonium salts and iron salts, and can better maintain the activity and life of the catalyst.
[0110] Table 3 Comparison between the present invention and existing solid catalysts
[0111]
[0112] As shown in Table 3, compared with the existing solid catalysts, the catalyst TiO 2 / γ-cyclodextrin-silicotungstic acid (or lithium salt-TiO 2 / γ-cyclodextrin-silicotungstic acid) uses γ-cyclodextrin as a carrier to load TiO 2 , titanium oxide groups and tungsten oxide groups, providing more catalytic active sites. More importantly, the addition of lithium salt further improves the TiO 2 The surface properties of / γ-cyclodextrin-silicotungstic acid increase the surface area of the catalyst, thereby extending the service life of the catalyst and improving the catalytic efficiency. The catalyst of the present invention has strong catalytic activity, the conversion rate of α-pinene exceeds 98%, and the yield of borneol exceeds 71%; the catalyst performance is stable, and after repeated use for 10 times, the conversion rate of α-pinene, the yield of borneol and the yield of normal borneol are not significantly reduced.
[0113] References
[0114] [1] Wang Helin et al. Solid superacid SO 4 2- / TiO 2 -Al 2 O 3 Preparation and catalytic synthesis of borneol. Materials Review. 2017, 31(22): 43-49.
[0115] [2] Chen Huizong et al. SO 4 2- / TiO 2Study on the synthesis of borneol catalyzed by solid superacid. Journal of Jiangxi Normal University (Natural Science Edition). 2002, (04): 363-365.
[0116] [3] Yang Yiwen et al. Solid superacid SO 4 2- / A1 2 O 3 Catalytic synthesis of borneol from a-pinene. Chemical Reagents. 2009,31(5): 331-333.
[0117] [4] Wang Helin et al. Solid superacid SO 4 2- / TiO 2 -SiO 2 Catalytic synthesis of borneol from a-pinene. Chemical Engineering. 2017, 45(11): 7-11+28.
[0118] [5] Yang Yiwen et al. Solid superacid S 2 O 8 2- / ZrO 2 -NiO catalyzed synthesis of borneol from a-pinene. Progress in Fine Petrochemicals. 2009, 10(09): 36-39.
[0119] [6] Guo Wei et al. 3+ / CNMS-SO 3 Preparation of H solid acid and its catalytic synthesis of borneol. Modern Chemical Industry. 2021, 41(02): 107-113+119.
[0120] [7] Liu Xiaoqin et al. Preparation of anatase-type mesoporous metatitanic acid catalyst and its catalytic esterification performance. Chemical Industry Progress. 2013, 32(07): 1573-1576+1597.
[0121] [8] Yu Jinquan et al. A new method for synthesizing borneol by esterification-saponification of α-pinene catalyzed by solid acid. CN 1074210A.
[0122] [9] Guo Yi. A method for preparing borneol. CN 110818530 A.
[0123]
[10] Wang Yaming et al. Preparation method and application of esterification-saponification reaction catalyst. CN 110327939B.
[0124] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing synthetic borneol, Features: The following steps are involved: S1, TiO 2 / γ-cyclodextrin-silicotungstic acid catalyst catalyzes the esterification of α-pinene and anhydrous oxalate, after the reaction is completed, the catalyst is filtered off, and the filtrate is distilled to remove the light oil to obtain diborneol oxalate; S2, adding diborneol oxalate to an anhydrous ethanol solution containing NaOH to carry out a saponification reaction, and after the saponification reaction is completed, distilling to obtain borneol; The TiO 2 The preparation method of the γ-cyclodextrin-silicotungstic acid catalyst comprises the following steps: S11, adding n-butanol to the γ-cyclodextrin aqueous solution and stirring evenly, then slowly adding ethyl titanate dropwise, and stirring under alkaline conditions to react to form a gel, filtering after the reaction, drying and calcining to obtain TiO 2 / γ-cyclodextrin; S12, the TiO 2 / γ-cyclodextrin was immersed in an alcohol solution of silicotungstic acid for reaction. After the reaction was completed, it was filtered, washed with water until neutral, dried, and calcined to obtain TiO 2 / γ-cyclodextrin-silicotungstic acid; In step S11, the mass fraction of the γ-cyclodextrin aqueous solution is 30%-50%, and the volume ratio of the γ-cyclodextrin aqueous solution: n-butanol: ethyl titanate is 1: (2-3): (5-7); In step S12, the concentration of the alcohol solution of silicotungstic acid is 0.01-0.03 mol / L, TiO 2 The mass ratio of / γ-cyclodextrin: silicotungstic acid alcohol solution is 1:(15-20); the soaking temperature is 30-40℃, the soaking time is 4-8h; the drying temperature is 100-110℃, and the time is 1-3h.
2. A method for preparing a synthetic borneol according to claim 1, Features: In step S1, the α-pinene:TiO 2 The mass ratio of / γ-cyclodextrin-silicotungstic acid catalyst: anhydrous oxalic acid is 1: (0.03-0.05): (0.3-0.5).
3. A method for preparing a synthetic borneol according to claim 1, Features: The temperature of the esterification reaction in step S1 is 60-70° C. for 0.5-1 h, 70-80° C. for 1-3 h, and 80-100° C. for 4-6 h.
4. A method for preparing a synthetic borneol according to claim 1, Features: The mass concentration of the anhydrous ethanol solution of NaOH in step S2 is 20%-30%, and the mass ratio of the diborneol oxalate: the anhydrous ethanol solution of NaOH is (3-5): (1-2).
5. A method for preparing a synthetic borneol according to claim 1, Features: In step S2, the saponification reaction temperature is 60-80° C., and the reaction time is 1-2 h.
6. A method for preparing a synthetic borneol according to claim 1, Features: Step S12: After drying, lithium salt and the dried solid powder are mixed in a mass ratio of 1:(5-8), and then calcined to obtain lithium salt-TiO 2 / γ-cyclodextrin-silicotungstic acid, the lithium salt is lithium chloride.
7. A method for preparing a synthetic borneol according to claim 1, Features: The calcination temperature and time in step S12 are 40-60°C, 1h; 60-100°C, 1h; 100-300°C, 1h; 300-500°C, 1h.