A high temperature resistant insulating plastic dipping liquid and preparation method thereof

By using PVC resin and other materials, the existing plastic immersion liquid has solved the shortcomings in high temperature and insulation performance, and achieved better high temperature and insulation performance, which is suitable for applications in high temperature environments.

CN118374110BActive Publication Date: 2024-11-15SHANDONG DONGLI POLYMER MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410828143.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-11-15
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

The existing immersion liquid has shortcomings in high temperature resistance and insulation performance, and it is difficult to meet the application needs in high temperature environments.

Method used

Using PVC resin, acrylic resin, functional filler, functional additive, alkyd resin, defoaming agent, plasticizer, antioxidant and deionized water as raw materials, the modified base is prepared by stirring in a vacuum stirred tank. High temperature resistant insulating plastic immersion liquid of materials and functional additives.

Benefits of technology

It has achieved good high temperature resistance and excellent insulation performance of immersion liquid, ensured product quality and quality, and expanded market application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of dipping liquid production, specifically to a high temperature resistant insulating dipping liquid and a preparation method thereof; the high temperature resistant insulating dipping liquid is composed of the following raw materials by weight: 20 to 30 parts of PVC resin, 10 to 20 parts of acrylic resin, 2 to 4 parts of functional fillers, 4 to 7 parts of functional additives, 5 to 8 parts of alkyd resin, 5 to 7 parts of defoamers, 5 to 7 parts of plasticizers, 2 to 5 parts of antioxidants and 100 to 200 parts of deionized water; by placing PVC resin, acrylic resin, alkyd resin, plasticizer and deionized water in a vacuum stirring kettle for stirring, then adding functional fillers, functional additives, defoamers and antioxidants, and continuing to stir, the final product is a high temperature resistant insulating dipping liquid. The dipping liquid prepared by the present invention not only has good high temperature resistance, but also has excellent insulation performance, effectively ensuring its quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastic dipping liquid production, in particular to a high temperature resistant insulating plastic dipping liquid and a preparation method thereof. Background Art

[0002] Plastic dipping liquid can be widely used in the coating of sports fitness equipment, labor protection PVC gloves, hardware tool handles, handles, wire hangers, hooks, electrical insulation materials, soft rubber sleeves, handicrafts, valve handles, automobile (motorcycle) anti-theft lock sheaths and other products. When used in electrical insulation materials, plastic liquids of various colors (mainly red, yellow and green) are usually required.

[0003] In the patent document with application number "CN201310043427.5" and titled "An antistatic dip-molded product and its preparation method", it is recorded that "its ingredients include 50-100 parts of PVC resin, 20-100 parts of plasticizer, 1-15 parts of antistatic agent, 0.5-15 parts of dispersant, and 0.2-10 parts of stabilizer. The above ingredients are prepared into a dipping liquid; the mold is preheated to 120-250°C and then immersed in the dipping liquid, and taken out after 1-120 seconds; the mold attached with plastic is plasticized at 200-550°C for 2-80 seconds, then taken out and cooled for 5-60 seconds, and a dip-molded product with flame retardant and antistatic properties is obtained after demolding. The dip-molded product prepared by this method has a surface resistivity of 105-109Ω, and the vertical burning meets the UL94-V0 standard, and has good antistatic and flame retardancy." Dispersants and antistatic agents are added to the dipping liquid to reduce the resistance of the material and improve the distribution uniformity, but its own high temperature resistance is relatively insufficient and still needs further improvement.

[0004] For another example, the patent document with application number "CN201710864461.7" and titled "An elastomer dipping solution and its preparation method" records that "the dipping solution contains the following components in parts by weight: 20-40 parts of modified resin, 10-30 parts of filler, 10-20 parts of thickener, 0-1 part of ultraviolet absorber, 100 parts of solvent, 2-5 parts of carbon black, 0.1-0.5 parts of dispersant. The raw materials are added in a certain order according to the formula, and mixed evenly at an appropriate temperature and stirring speed to obtain the elastomer dipping solution; the elastomer dipping solution is suitable for dipping and encapsulation of high-end metal tools and has broad market application prospects." It uses modified SBS and SEBS as raw materials, and its mechanical properties and environmental protection are improved, but its own high temperature resistance and insulation properties are relatively insufficient, and still need further improvement.

[0005] Based on this, the present invention provides a high temperature resistant insulating dipping liquid and a preparation method thereof to solve the above-mentioned technical problems. Summary of the invention

[0006] The purpose of the present invention is to provide a high temperature resistant insulating dipping liquid and a preparation method thereof. The prepared dipping liquid not only has good high temperature resistance, but also has excellent insulating performance, effectively ensuring its quality.

[0007] To achieve the above object, the present invention provides the following technical solutions: In the first aspect of the present invention, a high temperature resistant insulating dipping liquid is provided, which is composed of the following raw materials by weight: 20 to 30 parts of PVC resin, 10 to 20 parts of acrylic resin, 2 to 4 parts of functional fillers, 4 to 7 parts of functional additives, 5 to 8 parts of alkyd resin, 5 to 7 parts of defoamers, 5 to 7 parts of plasticizers, 2 to 5 parts of antioxidants and 100 to 200 parts of deionized water. The present invention is further configured as follows: the preparation process of the functional filler is as follows:

[0008] The base material is placed in an ethanol aqueous solution with a volume concentration of 70-74% at a solid-liquid ratio of 0.12-0.32 g / mL, and then γ-aminopropyltrimethoxysilane is added thereto in an amount of 8-10% by mass of the base material, and treated at 22-26° C. and 80-100 r / min for 30-40 min. After suction filtration, the base material is dried at 80° C. for 100-120 min to obtain a modified base material. The modified base material is placed in a reaction chamber of a BMD reactor, and after vacuuming, a mixed gas is introduced to a gas pressure of 11.2-12.5 kPa, and the base material is treated at a voltage of 5 kV and a frequency of 8 kHz for 12-15 min to obtain a functional filler.

[0009] The present invention is further configured as follows: the preparation process of the base material is as follows:

[0010] The nano silicon nitride is placed in a muffle furnace, treated at 900-1000°C for 180-200 minutes, cooled, washed with deionized water 2-4 times, and then uniformly dispersed in an ethanol aqueous solution with a volume concentration of 40-60% at a solid-liquid ratio of 0.02-0.12 g / mL to obtain a mixed solution;

[0011] Add dimethylhydroxy silicone oil and dibutyltin dilaurate to the mixed solution, and treat at 100-110°C for 7-8h;

[0012] After filtration, the filter cake is washed with anhydrous ethanol and deionized water for 2 to 4 times, and then placed in a vacuum oven and dried at 80° C. for 300 to 330 minutes to obtain a base material.

[0013] The present invention is further configured as follows: the addition amount of the dimethyl hydroxy silicone oil is 1.2-2.4% of the mass of the mixed liquid, and the addition amount of the dibutyltin dilaurate is 0.4-1.3% of the mass of the mixed liquid.

[0014] The present invention is further configured as follows: the mixed gas is formed by mixing carbon tetrafluoride and nitrogen in a volume ratio of 22 to 20:1.

[0015] The present invention is further configured as follows: the preparation process of the functional additive is as follows:

[0016] The nano-beryllium oxide is placed in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.03-0.23 g / mL and ultrasonically dispersed for 40-50 minutes, (3-aminopropyl)triethoxysilane is added thereto at a mass of 0.2-1.2% of the nano-beryllium oxide, and the mixture is treated at 100°C and 230-330 r / min for 10-12 hours, and after filtration, the mixture is washed with N,N-dimethylformamide and deionized water for 2-4 times, and then dried at 80-86°C in vacuum for 50-70 minutes to obtain the modified nano-beryllium oxide;

[0017] The modified nano-beryllium oxide is placed in an appropriate amount of toluene at a solid-liquid ratio of 0.02-0.08 g / mL and ultrasonically dispersed for 20-40 minutes, and then glass fiber and triethylamine are added thereto, and the mixture is treated at 90-94° C. for 6-8 hours. After filtration, the mixture is washed with deionized water for 2-4 times, and then dried at 80-86° C. in vacuum for 50-70 minutes to obtain a functional additive.

[0018] The present invention is further configured as follows: the defoaming agent is selected from any one of emulsified silicone oil and polydimethylsiloxane.

[0019] The present invention is further configured as follows: the plasticizer is selected from any one of citrate and diolein.

[0020] The present invention is further configured as follows: the antioxidant is selected from any one of antioxidant 1010, antioxidant 1076, and antioxidant CA.

[0021] The second aspect of the present invention: also provides a method for preparing the above-mentioned high temperature resistant insulating dipping solution, comprising the following steps:

[0022] Step 1: Accurately weigh PVC resin, acrylic resin, functional filler, functional additive, alkyd resin, defoamer, plasticizer, antioxidant and deionized water, and add PVC resin, acrylic resin, alkyd resin, plasticizer and deionized water into a vacuum stirring kettle, and stir at a medium speed of 120-220 r / min and 40-60° C. in a water bath for 22-32 minutes;

[0023] Step 2: Add functional fillers, functional additives, defoamers and antioxidants, and continue stirring at 80-120 r / min and 50-70° C. for 30-40 minutes. The final product is a high-temperature resistant insulating dipping liquid.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] In the present invention, PVC resin, acrylic resin, functional filler, functional additive, alkyd resin, defoamer, plasticizer, antioxidant and deionized water are used as raw materials. The PVC resin, acrylic resin, alkyd resin, plasticizer and deionized water are placed in a vacuum stirring kettle and stirred, and then the functional filler, functional additive, defoamer and antioxidant are added, and the stirring is continued. The final product is a high-temperature resistant insulating dipping liquid. The dipping liquid prepared by the present invention not only has good high-temperature resistance, but also has excellent insulation performance, which effectively guarantees its quality. The high-temperature resistant insulating dipping liquid and the preparation method thereof provided by the present invention have a broader market prospect and are more suitable for promotion. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0027] The present embodiment provides a high temperature resistant insulating dipping liquid, which is composed of the following raw materials in parts by weight: 20 parts of PVC resin, 10 parts of acrylic resin, 2 parts of functional filler, 4 parts of functional additives, 5 parts of alkyd resin, 5 parts of defoamer, 5 parts of plasticizer, 2 parts of antioxidant and 100 parts of deionized water.

[0028] In this embodiment, it should be noted that the PVC resin was purchased from Dongguan Jinma Plastic Co., Ltd., the acrylic resin was purchased from Guangzhou Xingzhengyuan Chemical Co., Ltd., and the alkyd resin was purchased from Shandong Duoju Chemical Co., Ltd.

[0029] The preparation process of the functional filler is as follows:

[0030] The base material was placed in an ethanol aqueous solution with a volume concentration of 70% at a solid-liquid ratio of 0.12 g / mL, and γ-aminopropyltrimethoxysilane with a volume concentration of 8% by mass of the base material was added thereto, and the mixture was treated at 22°C and 80 r / min for 30 minutes. After suction filtration, the mixture was dried at 80°C for 100 minutes to obtain a modified base material.

[0031] The obtained modified base material was placed in the reaction chamber of the BMD reactor, and after evacuation, a mixed gas was introduced to a gas pressure of 11.2 kPa, and the mixture was treated for 12 minutes at a voltage of 5 kV and a frequency of 8 kHz to obtain a functional filler.

[0032] Further, the preparation process of the base material is as follows:

[0033] The nano-silicon nitride was placed in a muffle furnace and treated at 900°C for 180 minutes. After cooling, the nano-silicon nitride was washed twice with deionized water, and then the nano-silicon nitride was uniformly dispersed in an ethanol aqueous solution with a volume concentration of 40% at a solid-liquid ratio of 0.02 g / mL to obtain a mixed solution.

[0034] Add dimethylhydroxy silicone oil and dibutyltin dilaurate into the mixed solution and treat at 100°C for 7 hours;

[0035] After filtration, the filter cake was washed twice with anhydrous ethanol and deionized water respectively, and then dried in a vacuum oven at 80° C. for 300 min to obtain a base material.

[0036] In addition, the added amount of dimethylhydroxysilicone oil is 1.2% of the mass of the mixed liquid, and the added amount of dibutyltin dilaurate is 0.4% of the mass of the mixed liquid.

[0037] The mixed gas is formed by mixing carbon tetrafluoride and nitrogen in a volume ratio of 22:1.

[0038] Further, the preparation process of the functional additive is as follows:

[0039] Nano-beryllia was placed in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.03 g / mL and ultrasonically dispersed for 40 minutes, (3-aminopropyl)triethoxysilane was added thereto at a mass of 0.2% of the nano-beryllia, and treated at 100°C and 230 r / min for 10 hours. After filtration, the nano-beryllia was washed twice with N,N-dimethylformamide and deionized water, and then dried at 80°C in vacuum for 50 minutes to obtain modified nano-beryllia.

[0040] The modified nano-beryllium oxide was placed in an appropriate amount of toluene at a solid-liquid ratio of 0.02 g / mL and ultrasonically dispersed for 20 minutes. Glass fiber and triethylamine were then added thereto. The mixture was treated at 90°C for 6 hours. After filtration, the mixture was washed twice with deionized water and dried at 80°C in vacuum for 50 minutes to obtain a functional additive.

[0041] In this embodiment, it should be noted that the glass fiber was purchased from Suzhou Fuliying Plastic Chemical Co., Ltd.

[0042] Among them, the defoaming agent is emulsified silicone oil.

[0043] Citrate is selected as the plasticizer.

[0044] The antioxidant used is antioxidant 1010.

[0045] In addition, this embodiment also provides a method for preparing the above-mentioned high temperature resistant insulating dipping solution, comprising the following steps:

[0046] Step 1: Accurately weigh PVC resin, acrylic resin, functional filler, functional additive, alkyd resin, defoamer, plasticizer, antioxidant and deionized water, and add PVC resin, acrylic resin, alkyd resin, plasticizer and deionized water into a vacuum stirring kettle, and stir at medium speed for 22 minutes at 120 r / min and 40° C. in a water bath;

[0047] Step 2: Add functional fillers, functional additives, defoamers and antioxidants, and continue stirring at 80 r / min and 50° C. for 30 minutes. The final product is a high-temperature resistant insulating dipping liquid. Example 2

[0048] The preparation method of the high temperature resistant insulating dipping solution provided in this embodiment is basically the same as that in embodiment 1, except that: the specific raw material composition and the specific preparation method of the high temperature resistant insulating dipping solution in this embodiment are different; the specific raw material composition and the specific preparation method of the high temperature resistant insulating dipping solution in this embodiment are as follows:

[0049] A high temperature resistant insulating dipping liquid is composed of the following raw materials in parts by weight: 25 parts of PVC resin, 15 parts of acrylic resin, 3 parts of functional fillers, 5 parts of functional additives, 6 parts of alkyd resin, 6 parts of defoamers, 6 parts of plasticizers, 3 parts of antioxidants and 150 parts of deionized water.

[0050] In this embodiment, it should be noted that the PVC resin was purchased from Dongguan Jinma Plastic Co., Ltd., the acrylic resin was purchased from Guangzhou Xingzhengyuan Chemical Co., Ltd., and the alkyd resin was purchased from Shandong Duoju Chemical Co., Ltd.

[0051] The preparation process of the functional filler is as follows:

[0052] The base material was placed in an ethanol aqueous solution with a volume concentration of 72% at a solid-liquid ratio of 0.22 g / mL, and γ-aminopropyltrimethoxysilane with a mass percentage of 9% of the base material was added thereto, and the mixture was treated at 24°C and 90 r / min for 35 min. After filtration, the mixture was dried at 80°C for 110 min to obtain a modified base material.

[0053] The obtained modified base material was placed in the reaction chamber of the BMD reactor, and after evacuation, a mixed gas was introduced to a gas pressure of 11.8 kPa, and the mixture was treated for 13 minutes at a voltage of 5 kV and a frequency of 8 kHz to obtain a functional filler.

[0054] Further, the preparation process of the base material is as follows:

[0055] The nano-silicon nitride was placed in a muffle furnace and treated at 950°C for 190 minutes. After cooling, the nano-silicon nitride was washed with deionized water for three times, and then the nano-silicon nitride was uniformly dispersed in an ethanol aqueous solution with a volume concentration of 50% at a solid-liquid ratio of 0.07 g / mL to obtain a mixed solution.

[0056] Add dimethylhydroxy silicone oil and dibutyltin dilaurate to the mixed solution and treat at 105°C for 8 hours;

[0057] After filtration, the filter cake was washed three times with anhydrous ethanol and deionized water respectively, and then dried in a vacuum oven at 80° C. for 325 min to obtain a base material.

[0058] In addition, the added amount of dimethylhydroxysilicone oil is 1.8% of the mass of the mixed liquid, and the added amount of dibutyltin dilaurate is 0.8% of the mass of the mixed liquid.

[0059] The mixed gas is formed by mixing carbon tetrafluoride and nitrogen in a volume ratio of 21:1.

[0060] Further, the preparation process of the functional additive is as follows:

[0061] Nano-beryllia was placed in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.13 g / mL and ultrasonically dispersed for 45 minutes, (3-aminopropyl)triethoxysilane was added thereto at a mass of 0.7% of the nano-beryllia, and treated at 100°C and 280 r / min for 11 hours. After filtration, the nano-beryllia was washed with N,N-dimethylformamide and deionized water for three times, and then dried at 83°C in vacuum for 60 minutes to obtain modified nano-beryllia.

[0062] The modified nano-beryllium oxide was placed in an appropriate amount of toluene at a solid-liquid ratio of 0.06 g / mL and ultrasonically dispersed for 30 minutes. Glass fiber and triethylamine were then added thereto and treated at 92°C for 7 hours. After filtration, the mixture was washed three times with deionized water and dried at 84°C under vacuum for 60 minutes to obtain a functional additive.

[0063] In this embodiment, it should be noted that the glass fiber was purchased from Suzhou Fuliying Plastic Chemical Co., Ltd.

[0064] Among them, the defoaming agent is polydimethylsiloxane.

[0065] The plasticizer is diolein.

[0066] Antioxidant 1076 was selected as the antioxidant.

[0067] In addition, this embodiment also provides a method for preparing the above-mentioned high temperature resistant insulating dipping solution, comprising the following steps:

[0068] Step 1: Accurately weigh PVC resin, acrylic resin, functional filler, functional additive, alkyd resin, defoamer, plasticizer, antioxidant and deionized water, and add PVC resin, acrylic resin, alkyd resin, plasticizer and deionized water into a vacuum stirring kettle, and stir at a medium speed of 170 r / min and 50° C. in a water bath for 27 minutes;

[0069] Step 2: Add functional fillers, functional additives, defoamers and antioxidants, and continue stirring at 100 r / min and 60° C. for 35 minutes. The final product is a high-temperature resistant insulating dipping liquid. Example 3

[0070] The preparation method of the high temperature resistant insulating dipping solution provided in this embodiment is basically the same as that in embodiment 1, except that: the specific raw material composition and the specific preparation method of the high temperature resistant insulating dipping solution in this embodiment are different; the specific raw material composition and the specific preparation method of the high temperature resistant insulating dipping solution in this embodiment are as follows:

[0071] A high temperature resistant insulating dipping liquid is composed of the following raw materials in parts by weight: 30 parts of PVC resin, 20 parts of acrylic resin, 4 parts of functional fillers, 7 parts of functional additives, 8 parts of alkyd resin, 7 parts of defoamers, 7 parts of plasticizers, 5 parts of antioxidants and 200 parts of deionized water.

[0072] In this embodiment, it should be noted that the PVC resin was purchased from Dongguan Jinma Plastic Co., Ltd., the acrylic resin was purchased from Guangzhou Xingzhengyuan Chemical Co., Ltd., and the alkyd resin was purchased from Shandong Duoju Chemical Co., Ltd.

[0073] The preparation process of the functional filler is as follows:

[0074] The base material was placed in an ethanol aqueous solution with a volume concentration of 74% at a solid-liquid ratio of 0.32 g / mL, and γ-aminopropyltrimethoxysilane with a mass percentage of 10% of the base material was added thereto, and the mixture was treated at 26°C and 100 r / min for 40 minutes. After filtration, the mixture was dried at 80°C for 120 minutes to obtain a modified base material.

[0075] The obtained modified base material was placed in the reaction chamber of the BMD reactor, and after evacuation, a mixed gas was introduced to a gas pressure of 12.5 kPa, and the mixture was treated for 15 minutes at a voltage of 5 kV and a frequency of 8 kHz to obtain a functional filler.

[0076] Further, the preparation process of the base material is as follows:

[0077] The nano-silicon nitride was placed in a muffle furnace and treated at 1000°C for 200 minutes. After cooling, the nano-silicon nitride was washed with deionized water for 4 times, and then the nano-silicon nitride was uniformly dispersed in an ethanol aqueous solution with a volume concentration of 60% at a solid-liquid ratio of 0.12 g / mL to obtain a mixed solution.

[0078] Add dimethylhydroxy silicone oil and dibutyltin dilaurate to the mixed solution and treat at 110°C for 8 hours;

[0079] After filtration, the filter cake was washed four times with anhydrous ethanol and deionized water respectively, and then dried in a vacuum oven at 80° C. for 330 min to obtain a base material.

[0080] In addition, the added amount of dimethylhydroxysilicone oil is 2.4% of the mass of the mixed liquid, and the added amount of dibutyltin dilaurate is 1.3% of the mass of the mixed liquid.

[0081] The mixed gas is formed by mixing carbon tetrafluoride and nitrogen in a volume ratio of 20:1.

[0082] Further, the preparation process of the functional additive is as follows:

[0083] The nano-beryllium oxide was placed in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.23 g / mL and ultrasonically dispersed for 50 minutes, (3-aminopropyl)triethoxysilane was added thereto at a mass of 1.2% of the nano-beryllium oxide, and treated at 100°C and 330 r / min for 12 hours. After filtration, the nano-beryllium oxide was washed with N,N-dimethylformamide and deionized water for 4 times, and then dried at 86°C in vacuum for 70 minutes to obtain the modified nano-beryllium oxide.

[0084] The modified nano-beryllium oxide was placed in an appropriate amount of toluene at a solid-liquid ratio of 0.08 g / mL and ultrasonically dispersed for 40 minutes. Glass fiber and triethylamine were then added thereto. The mixture was treated at 94°C for 8 hours. After filtration, the mixture was washed with deionized water for 4 times and dried under vacuum at 86°C for 70 minutes to obtain a functional additive.

[0085] In this embodiment, it should be noted that the glass fiber was purchased from Suzhou Fuliying Plastic Chemical Co., Ltd.

[0086] Among them, the defoaming agent is emulsified silicone oil.

[0087] Citrate is selected as the plasticizer.

[0088] The antioxidant used is antioxidant CA.

[0089] In addition, this embodiment also provides a method for preparing the above-mentioned high temperature resistant insulating dipping solution, comprising the following steps:

[0090] Step 1, accurately weigh PVC resin, acrylic resin, functional filler, functional additive, alkyd resin, defoamer, plasticizer, antioxidant and deionized water, and add PVC resin, acrylic resin, alkyd resin, plasticizer and deionized water into a vacuum stirring kettle, and stir at medium speed for 32 minutes in a water bath at 220r / min and 60°C;

[0091] Step 2: Add functional fillers, functional additives, defoamers and antioxidants, and continue stirring at 120 r / min and 70° C. for 40 minutes. The final product is a high-temperature resistant insulating dipping liquid.

[0092] Comparative Example 1: The difference from Example 1 is that in this example, nano silicon nitride replaces the functional filler.

[0093] Comparative Example 2: The difference from Example 1 is that this example does not contain a functional additive.

[0094] Performance test: The high temperature resistant insulating dipping liquid samples provided in Examples 1 to 3 and Comparative Examples 1 to 2 are marked as Examples 1 to 3 and Comparative Examples 1 to 2, respectively; and the relevant properties of the high temperature resistant insulating dipping liquid cured specimens provided in Examples 1 to 3 and Comparative Examples 1 to 2 are tested as follows:

[0095] 1. Temperature resistance test: The test method is to place it in a 200℃ environment for 120 minutes, and then test its tensile strength retention rate according to GB / T1040-1992.

[0096] The obtained test data are recorded in Table 1 and Table 2 below:

[0097]

[0098] By comparing and analyzing the relevant data in Table 1 and Table 2, it can be seen that the dipping solution prepared by the present invention not only has good high temperature resistance, but also has excellent insulation performance, which effectively guarantees its quality. This shows that the high temperature resistant insulating dipping solution and the preparation method thereof provided by the present invention have a broader market prospect and are more suitable for promotion.

[0099] In the present invention, PVC resin, acrylic resin, functional filler, functional additive, alkyd resin, defoamer, plasticizer, antioxidant and deionized water are used as raw materials, PVC resin, acrylic resin, alkyd resin, plasticizer and deionized water are placed in a vacuum stirring kettle for stirring, and then functional filler, functional additive, defoamer and antioxidant are added, and stirring is continued, and finally the obtained product is a high temperature resistant insulating dipping liquid. The dipping liquid prepared by the present invention not only has good high temperature resistance, but also has excellent insulation performance, and its quality is effectively guaranteed.

[0100] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0101] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A high temperature resistant insulating dipping liquid, characterized in that: The invention is composed of the following raw materials in parts by weight: 20 to 30 parts of PVC resin, 10 to 20 parts of acrylic resin, 2 to 4 parts of functional fillers, 4 to 7 parts of functional additives, 5 to 8 parts of alkyd resin, 5 to 7 parts of defoamers, 5 to 7 parts of plasticizers, 2 to 5 parts of antioxidants and 100 to 200 parts of deionized water; The preparation process of the functional filler is as follows: The base material is placed in an ethanol aqueous solution with a volume concentration of 70-74% at a solid-liquid ratio of 0.12-0.32 g / mL, and then 8-10% of the mass of the base material is added thereto, and the base material is treated at 22-26° C. and 80-100 r / min for 30-40 min. After suction filtration, the base material is dried at 80° C. for 100-120 min to obtain a modified base material; The obtained modified base material is placed in the reaction chamber of the BMD reactor, and after evacuation, a mixed gas is introduced to a pressure of 11.2 to 12.5 kPa, and the mixture is treated for 12 to 15 minutes at a voltage of 5 kV and a frequency of 8 kHz to obtain a functional filler; The preparation process of the base material is as follows: The nano silicon nitride is placed in a muffle furnace, treated at 900-1000° C. for 180-200 min, cooled, washed with deionized water 2-4 times, and then uniformly dispersed in an ethanol aqueous solution with a volume concentration of 40-60% at a solid-liquid ratio of 0.02-0.12 g / mL to obtain a mixed solution; Add dimethylhydroxy silicone oil and dibutyltin dilaurate to the mixed solution, and treat at 100-110°C for 7-8h; After filtration, the filter cake is washed with anhydrous ethanol and deionized water for 2 to 4 times, and then placed in a vacuum oven and dried at 80° C. for 300 to 330 minutes to obtain a base material; The preparation process of the functional additive is as follows: The nano-beryllium oxide is placed in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.03-0.23 g / mL and ultrasonically dispersed for 40-50 minutes, (3-aminopropyl)triethoxysilane is added thereto at a mass of 0.2-1.2% of the nano-beryllium oxide, and the mixture is treated at 100° C. and 230-330 r / min for 10-12 hours, and after filtration, the mixture is washed with N,N-dimethylformamide and deionized water for 2-4 times, and then dried at 80-86° C. under vacuum for 50-70 minutes to obtain the modified nano-beryllium oxide; The modified nano-beryllium oxide is placed in an appropriate amount of toluene at a solid-liquid ratio of 0.02-0.08 g / mL and ultrasonically dispersed for 20-40 minutes, and then glass fiber and triethylamine are added thereto, and the mixture is treated at 90-94° C. for 6-8 hours. After filtration, the mixture is washed with deionized water for 2-4 times, and then dried at 80-86° C. in vacuum for 50-70 minutes to obtain a functional additive.

2. The high temperature resistant insulating dipping liquid according to claim 1, characterized in that: The added amount of the dimethyl hydroxy silicone oil is 1.2-2.4% of the mass of the mixed liquid, and the added amount of the dibutyltin dilaurate is 0.4-1.3% of the mass of the mixed liquid.

3. The high temperature resistant insulating dipping liquid according to claim 1, characterized in that: The mixed gas is formed by mixing carbon tetrafluoride and nitrogen in a volume ratio of 22 to 20:

1.

4. The high temperature resistant insulating dipping liquid according to claim 1, characterized in that: The defoaming agent is selected from any one of emulsified silicone oil and polydimethylsiloxane.

5. The high temperature resistant insulating dipping liquid according to claim 1, characterized in that: The plasticizer is selected from any one of citrate and diolein.

6. The high temperature resistant insulating dipping liquid according to claim 1, characterized in that: The antioxidant is selected from any one of antioxidant 1010, antioxidant 1076, and antioxidant CA.

7. A method for preparing a high temperature resistant insulating dipping solution according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1: Accurately weigh PVC resin, acrylic resin, functional filler, functional additive, alkyd resin, defoamer, plasticizer, antioxidant and deionized water, and add PVC resin, acrylic resin, alkyd resin, plasticizer and deionized water into a vacuum stirring kettle, and stir at a medium speed of 120-220 r / min and 40-60° C. in a water bath for 22-32 minutes; Step 2: Add functional fillers, functional additives, defoamers and antioxidants, and continue stirring at 80-120 r / min and 50-70° C. for 30-40 minutes. The final product is a high-temperature resistant insulating dipping liquid.