A rare earth aluminum alloy material and preparation method thereof

By smelting aluminum with silica, iron and magnesium with cerium and lanthanum, and treating it with a specific surface treatment liquid, a rare earth aluminum alloy material with high mechanical properties, hydrophobicity and antibacterial ability is prepared, which solves the problem that aluminum alloys easily corrode in water. It solves the problem of damage and improves the stability and application performance of the material.

CN118389911BActive Publication Date: 2024-10-15BEIJING JUJIA MASCH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410487871.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-23
Publication Date
2024-10-15
Estimated Expiration
2044-04-23

AI Technical Summary

Technical Problem

Existing aluminum alloy materials are easily damaged by corrosion in water, and lack hydrophobic and antibacterial properties, making it difficult to meet application needs in complex environments.

Method used

The preparation method of rare earth aluminum alloy materials is adopted, by mixing aluminum with silica, iron and magnesium and then smelting with cerium and lanthanum, homogenizing and completely annealing, and treating with specific surface treatment liquids, including emulsifier solutions and initiators. agent, sonicated and dried to enhance the hydrophobic and antimicrobial properties of the material.

Benefits of technology

It improves the mechanical properties of the material, enhances the tensile strength and yield strength, and gives the material good hydrophobic and antibacterial capabilities, improving its stability in complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a rare earth aluminum alloy material and a preparation method thereof, and relates to the field of metal materials. When preparing the rare earth aluminum alloy material, the present invention first mixes aluminum with silicon dioxide, iron and magnesium, then mixes and melts with cerium and lanthanum, casts, then homogenizes and completely anneals, extrudes into plates to prepare the rare earth aluminum alloy, first reacts p-bromobenzaldehyde with 1-(pyridine-2-yl) ethyl ketone, then reacts with allyl boric acid pinacol ester, finally mixes with heptene, then mixes with an emulsifier solution, and is initiated by an initiator to prepare a surface treatment liquid, and the rare earth aluminum alloy is immersed in a hydrochloric acid solution, ultrasonicated, dried, and the surface treatment liquid is evenly applied to the surface of the rare earth aluminum alloy, dried, and a rare earth aluminum alloy material is prepared. The rare earth aluminum alloy material prepared by the present invention has hydrophobic and antibacterial capabilities.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal materials, in particular to a rare earth aluminum alloy material and a preparation method thereof. Background Art

[0002] Aluminum alloy is an alloy with aluminum as the base and a certain amount of other alloying elements added. It is one of the light metal materials. According to various uses, in order to have higher strength and improve the material's organization and other various properties, various alloying elements can be added to pure aluminum to produce aluminum alloys that meet various performance and uses. Aluminum alloy can be processed into plates, strips, bars, foils, tubes, bars, profiles, wires, free forgings and die forgings, and can also be processed into castings, die castings and other castings.

[0003] Metal aluminum and its alloys play a very important role in human daily life. Due to their excellent physical, chemical, mechanical and processing properties, they are widely used in power transportation, construction equipment, transportation, aerospace, automotive electronics and other industries. As a member of the metal material category, metal aluminum and its alloys also need to face the unavoidable problem of metal materials - corrosion by water. Therefore, this article introduces a rare earth aluminum alloy material with hydrophobic and antibacterial capabilities. Summary of the invention

[0004] The purpose of the present invention is to provide a rare earth aluminum alloy material and a preparation method thereof, so as to solve the problems existing in the prior art.

[0005] A high-performance rare earth aluminum alloy material, wherein the high-performance rare earth aluminum alloy is prepared by immersing the rare earth aluminum alloy in a hydrochloric acid solution, ultrasonicating, drying, and then evenly applying a surface treatment liquid on the surface of the rare earth aluminum alloy and drying;

[0006] As an optimization, the rare earth aluminum alloy is prepared by first mixing aluminum with silicon dioxide, iron and magnesium, then smelting with cerium and lanthanum, casting, homogenizing and fully annealing, and extruding into a plate;

[0007] As an optimization, the surface treatment liquid is prepared by mixing an emulsifier solution and an olefin mixed solution, and then initiating polymerization with an initiator;

[0008] As an optimization, the olefin mixture is prepared by first reacting p-bromobenzaldehyde with 1-(pyridin-2-yl)ethanone, then reacting with allylboronic acid pinacol ester, and finally mixing with heptene.

[0009] A method for preparing a rare earth aluminum alloy material, characterized in that the method for preparing the rare earth aluminum alloy material mainly comprises the following preparation steps:

[0010] Aluminum, silicon dioxide, iron and magnesium are mixed in a mass ratio of 98.5-99.5: 0.003-0.005: 0.001-0.002: 0.005-0.007, heated at 730-750°C for 20-30 minutes, lanthanum with a mass of 0.1-0.12 times the mass of aluminum and cerium with a mass of 0.08-0.12 times the mass of aluminum are added, stirred at 720-760°C and 200-300 r / min for 60-80 minutes, and a multi-component mixed gas is introduced for 20-30 minutes to obtain an aluminum alloy melt, which is cast into a plate to obtain an aluminum alloy crude product; the aluminum alloy crude product is kept at 510-530°C for 4-6 hours, cooled to 0-5°C, then heated to 300-400°C for 600-800 seconds, extruded into a plate to obtain a rare earth aluminum alloy;

[0011] p-bromobenzaldehyde, potassium hydroxide, ethanol and ammonia water are mixed in a mass ratio of 1.6-2:1.8-2.2:46-48:16-20, stirred at 200-300 r / min, 1-(pyridin-2-yl)ethanone (3.5-4 times the molar amount of p-bromobenzaldehyde) is added uniformly within 5-8 min, react for 30-50 min, heat to 50-60°C, react for 7-9 h under nitrogen protection, filter, and dry at 60-80°C for 22-24 h to obtain brominated terpyridine;

[0012] Mix allylboronic acid pinacol ester, brominated terpyridine, tetrakis(triphenylphosphine)palladium and potassium carbonate in a molar ratio of 1-1.4:3-5:0.1-0.14:0.1-0.14, immerse in tetrahydrofuran, stir at 200-300 r / min, react for 18-22 hours at 70-90°C, avoid light, and under nitrogen protection, dry at 60-70°C for 6-8 hours, mix petroleum ether and dichloromethane in a mass ratio of 4-6:1 as a mobile phase, undergo column chromatography, and dry at 60-80°C for 22-24 hours to obtain a terpyridine monomer;

[0013] The emulsifier solution and the olefin mixed solution are mixed at a mass ratio of 1:30-50, and an initiator solution of 0.12-0.13 times the mass of the emulsifier solution is uniformly added at 50-70°C and 200-300 r / min within 8-10 minutes, and stirred at 200-300 r / min for 2-3 hours, and filtered to obtain a surface treatment solution;

[0014] The rare earth aluminum alloy is immersed in a 2-3 mol / L hydrochloric acid solution for 4-6 minutes, ultrasonicated in deionized water for 4-6 minutes, dried at 100-120°C for 2-4 hours, the surface treatment liquid is evenly applied to the surface of the rare earth aluminum alloy, and dried at 50-70°C for 24-48 hours to obtain a rare earth aluminum alloy material.

[0015] As an optimization, the multi-component mixed gas in step (1) is prepared by uniformly mixing argon, nitrogen, carbon monoxide and chlorine in a ratio of 1:1:1:1.

[0016] As an optimization, the casting method in step (1) adopts metal mold water-cooled semi-continuous casting technology, with specific parameters as follows: furnace temperature 730°C~740°C, casting temperature 710°C~720°C, effective crystallization zone height in the continuous casting crystallizer 13~17mm, casting speed 105~115mm / min, water pressure 20~25kPa, cooling water inlet temperature 15~25°C, and outlet water temperature 35~45°C.

[0017] As an optimization, the extrusion method in step (1) is to extrude after keeping the temperature at 510°C~530°C for 4~6 hours; the extrusion parameters are: extrusion pressure 180MPa~220MPa, extrusion speed 12~15m / min, and extrusion temperature 450°C~470°C.

[0018] As an optimization, the emulsifier solution in step (4) is prepared by mixing sodium dodecyl sulfate and deionized water in a mass ratio of 1:10.

[0019] As an optimization, the initiator solution in step (4) is prepared by mixing potassium persulfate and deionized water in a mass ratio of 1:10.

[0020] As an optimization, the olefin mixture in step (4) is prepared by uniformly mixing terpyridine monomer and heptene in a mass ratio of 3-5:2-4.

[0021] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0022] When preparing the rare earth aluminum alloy material, the present invention comprises the following steps: firstly mixing aluminum with silicon dioxide, iron and magnesium, then mixing with cerium and lanthanum for smelting, casting, homogenizing and completely annealing, and extruding into a plate to obtain the rare earth aluminum alloy; firstly reacting p-bromobenzaldehyde with 1-(pyridine-2-yl)ethanone, then reacting with allylboronic acid pinacol ester, finally mixing with heptene, and then mixing with an emulsifier solution, initiating with an initiator to obtain a surface treatment liquid, immersing the rare earth aluminum alloy in a hydrochloric acid solution, ultrasonicating, drying, uniformly applying the surface treatment liquid on the surface of the rare earth aluminum alloy, and drying to obtain the rare earth aluminum alloy material.

[0023] First, aluminum is mixed with silicon dioxide, iron and magnesium, and then mixed with cerium and lanthanum for smelting, casting, homogenization and complete annealing, and extrusion into plates to obtain rare earth aluminum alloy; homogenization can improve or eliminate the organizational defects and residual stresses generated during casting, forging, rolling and welding, refine the grains, improve the organization, improve the mechanical properties of the workpiece, remove internal defects such as pores, inclusions, liquid metal, etc., make the material properties more stable, thereby improving the mechanical properties of the material; complete annealing can recrystallize and rearrange the grains of the material, while eliminating dislocations and gaps, so that the plasticity and toughness of the material are improved, and can also make the grains of the material uniformly refined and rearranged, eliminate internal defects, thereby improving the strength and hardness of the material, improving the mechanical properties of the material, and increasing the tensile strength and yield strength of the material.

[0024] Secondly, p-bromobenzaldehyde is first reacted with 1-(pyridine-2-yl)ethanone, then reacted with allylboronic acid pinacol ester, and finally mixed with heptene, and then mixed with an emulsifier solution, and a surface treatment liquid is obtained by initiation with an initiator, and the rare earth aluminum alloy is immersed in a hydrochloric acid solution, ultrasonicated, dried, and the surface treatment liquid is evenly applied to the surface of the rare earth aluminum alloy, and dried to obtain a rare earth aluminum alloy material. The long carbon chain of heptene can increase the dispersion force between molecules, so that the force between molecules is enhanced, thereby enhancing the hydrophobicity of the material; after the aluminum alloy is immersed in the hydrochloric acid solution, the surface is rich in aluminum ions, and the aluminum ions can be combined with substances such as proteins and phosphatidic acid in the cell membrane of microorganisms, affecting the integrity of the cell membrane, resulting in an imbalance of substances inside and outside the cell and cell death, thereby killing bacteria, achieving an antibacterial effect, and improving the antibacterial ability of the material. The surface treatment liquid contains a terpyridine structure, which can achieve a better adhesion effect with the aluminum alloy. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0026] The olefin mixed solution used in the following examples and comparative examples is prepared by uniformly mixing terpyridine monomer and heptene in a mass ratio of 3-5:2-4. Example

[0027] A rare earth aluminum alloy material and a preparation method thereof, mainly comprising the following preparation steps:

[0028] Aluminum, silicon dioxide, iron and magnesium are mixed in a mass ratio of 98.5:0.003:0.001:0.005, heated at 730°C for 20 minutes, lanthanum 0.1 times the mass of aluminum and cerium 0.08 times the mass of aluminum are added, stirred at 720°C and 200r / min for 60 minutes, and a multi-component mixed gas is introduced for 20 minutes to obtain an aluminum alloy melt, which is cast into a plate to obtain an aluminum alloy crude product; the aluminum alloy crude product is kept at 510°C for 4 hours, cooled to 0°C; then heated to 300°C and kept for 600 seconds, extruded into a plate to obtain a rare earth aluminum alloy;

[0029] p-Bromobenzaldehyde, potassium hydroxide, ethanol and ammonia water were mixed in a mass ratio of 1.6:1.8:46:16, stirred at 200 r / min, and 1-(pyridin-2-yl)ethanone (3.5 times the molar amount of p-bromobenzaldehyde) was uniformly added within 5 min, reacted for 30 min, heated to 50°C, reacted for 7 h under nitrogen protection, filtered, and dried at 60°C for 22 h to obtain brominated terpyridine;

[0030] Allylboronic acid pinacol ester, brominated terpyridine, tetrakis(triphenylphosphine)palladium and potassium carbonate were mixed in a molar ratio of 1:3:0.1:0.1, immersed in tetrahydrofuran, stirred at 200 r / min, reacted for 18 hours at 70°C, protected from light and under nitrogen protection, dried at 60°C for 6 hours, and petroleum ether and dichloromethane were mixed evenly in a mass ratio of 4:1 as a mobile phase, subjected to column chromatography, and dried at 60°C for 22 hours to obtain a terpyridine monomer;

[0031] The emulsifier solution and the olefin mixture were mixed at a mass ratio of 1:30, and an initiator solution of 0.12 times the mass of the emulsifier solution was uniformly added at 50°C and 200 r / min within 8 minutes, and stirred at 200 r / min for 2 hours, and filtered to obtain a surface treatment solution;

[0032] The rare earth aluminum alloy was immersed in a 2 mol / L hydrochloric acid solution for 4 min, ultrasonicated in deionized water for 4 min, dried at 100°C for 2 h, the surface treatment liquid was evenly applied to the surface of the rare earth aluminum alloy, and dried at 50°C for 24 h to obtain a rare earth aluminum alloy material.

[0033] Example 1

[0034] A rare earth aluminum alloy material and a preparation method thereof, mainly comprising the following preparation steps:

[0035] Aluminum, silicon dioxide, iron and magnesium are mixed in a mass ratio of 99:0.004:0.0015:0.006, heated at 740°C for 25 minutes, lanthanum with a mass of 0.15 times the mass of aluminum and cerium with a mass of 0.1 times the mass of aluminum are added, stirred at 740°C and 250r / min for 70 minutes, and a multi-component mixed gas is introduced for 25 minutes to obtain an aluminum alloy melt, which is cast into a plate to obtain an aluminum alloy crude product; the aluminum alloy crude product is kept at 520°C for 5 hours, cooled to 2.5°C; then heated to 350°C and kept for 700 seconds, extruded into a plate to obtain a rare earth aluminum alloy;

[0036] p-Bromobenzaldehyde, potassium hydroxide, ethanol and ammonia water were mixed in a mass ratio of 1.8:2:47:18, stirred at 250 r / min, 1-(pyridin-2-yl)ethanone (3.75 times the molar amount of p-bromobenzaldehyde) was added at a uniform rate within 6.5 min, reacted for 40 min, heated to 55°C, reacted for 8 h under nitrogen protection, filtered, and dried at 70°C for 23 h to obtain brominated terpyridine;

[0037] Allylboronic acid pinacol ester, brominated terpyridine, tetrakis(triphenylphosphine)palladium and potassium carbonate were mixed in a molar ratio of 1.2:4:0.12:0.12, immersed in tetrahydrofuran, stirred at 250r / min, reacted for 20h at 80℃, protected from light and under nitrogen protection, dried at 65℃ for 7h, and petroleum ether and dichloromethane were mixed evenly in a mass ratio of 5:1 as a mobile phase, subjected to column chromatography, and dried at 70℃ for 23h to obtain terpyridine monomer;

[0038] The emulsifier solution and the olefin mixture were mixed at a mass ratio of 1:40, and an initiator solution 0.125 times the mass of the emulsifier solution was uniformly added at 60°C and 250 r / min within 9 minutes, and stirred at 250 r / min for 2.5 hours, and filtered to obtain a surface treatment solution;

[0039] The rare earth aluminum alloy was immersed in a 2.5 mol / L hydrochloric acid solution for 5 min, ultrasonicated in deionized water for 5 min, dried at 110°C for 3 h, the surface treatment liquid was evenly applied to the surface of the rare earth aluminum alloy, and dried at 60°C for 36 h to obtain a rare earth aluminum alloy material.

[0040] Example 2

[0041] A rare earth aluminum alloy material and a preparation method thereof, mainly comprising the following preparation steps:

[0042] Aluminum, silicon dioxide, iron and magnesium are mixed in a mass ratio of 99.5:0.005:0.002:0.007, heated at 750°C for 30 minutes, lanthanum with a mass of 0.12 times the mass of aluminum and cerium with a mass of 0.12 times the mass of aluminum are added, stirred at 760°C and 300r / min for 80 minutes, and a multi-component mixed gas is introduced for 30 minutes to obtain an aluminum alloy melt, which is cast into a plate to obtain an aluminum alloy crude product; the aluminum alloy crude product is kept at 530°C for 6 hours, cooled to 5°C; then heated to 400°C for 800 seconds, extruded into a plate to obtain a rare earth aluminum alloy;

[0043] p-Bromobenzaldehyde, potassium hydroxide, ethanol and ammonia water were mixed in a mass ratio of 2:2.2:48:20, stirred at 300 r / min, and 1-(pyridin-2-yl)ethanone 4 times the molar amount of p-bromobenzaldehyde was uniformly added within 8 min, reacted for 50 min, heated to 60°C, reacted for 9 h under nitrogen protection, filtered, and dried at 80°C for 24 h to obtain brominated terpyridine;

[0044] Allylboronic acid pinacol ester, brominated terpyridine, tetrakis(triphenylphosphine)palladium and potassium carbonate were mixed in a molar ratio of 1.4:5:0.14:0.14, immersed in tetrahydrofuran, stirred at 300 r / min, reacted at 90°C, protected from light, under nitrogen protection for 22 hours, dried at 70°C for 8 hours, and petroleum ether and dichloromethane were mixed evenly in a mass ratio of 6:1 as a mobile phase, subjected to column chromatography, and dried at 80°C for 24 hours to obtain a terpyridine monomer;

[0045] The emulsifier solution and the olefin mixture were mixed at a mass ratio of 1:50, and an initiator solution of 0.13 times the mass of the emulsifier solution was uniformly added at 70°C and 300 r / min within 10 min, and stirred at 300 r / min for 3 h, and filtered to obtain a surface treatment solution;

[0046] The rare earth aluminum alloy was immersed in 3 mol / L hydrochloric acid solution for 6 minutes, ultrasonicated in deionized water for 6 minutes, dried at 120°C for 4 hours, the surface treatment liquid was evenly applied on the surface of the rare earth aluminum alloy, and dried at 70°C for 48 hours to obtain the rare earth aluminum alloy material.

[0047] Comparative Example 1

[0048] A rare earth aluminum alloy material and a preparation method thereof, mainly comprising the following preparation steps:

[0049] Aluminum, silicon dioxide, iron and magnesium are mixed in a mass ratio of 99:0.004:0.0015:0.006, heated at 740°C for 25 minutes, lanthanum with a mass of 0.15 times the mass of aluminum and cerium with a mass of 0.1 times the mass of aluminum are added, stirred at 740°C and 250r / min for 70 minutes, and a multi-component mixed gas is introduced for 25 minutes to obtain an aluminum alloy melt, which is cast into a plate to obtain an aluminum alloy crude product; the aluminum alloy crude product is kept at 350°C for 700s and extruded into a plate to obtain a rare earth aluminum alloy;

[0050] p-Bromobenzaldehyde, potassium hydroxide, ethanol and ammonia water were mixed in a mass ratio of 1.8:2:47:18, stirred at 250 r / min, 1-(pyridin-2-yl)ethanone (3.75 times the molar amount of p-bromobenzaldehyde) was added at a uniform rate within 6.5 min, reacted for 40 min, heated to 55°C, reacted for 8 h under nitrogen protection, filtered, and dried at 70°C for 23 h to obtain brominated terpyridine;

[0051] Allylboronic acid pinacol ester, brominated terpyridine, tetrakis(triphenylphosphine)palladium and potassium carbonate were mixed in a molar ratio of 1.2:4:0.12:0.12, immersed in tetrahydrofuran, stirred at 250r / min, reacted for 20h at 80℃, protected from light and under nitrogen protection, dried at 65℃ for 7h, and petroleum ether and dichloromethane were mixed evenly in a mass ratio of 5:1 as a mobile phase, subjected to column chromatography, and dried at 70℃ for 23h to obtain terpyridine monomer;

[0052] The emulsifier solution and the olefin mixture were mixed at a mass ratio of 1:40, and an initiator solution 0.125 times the mass of the emulsifier solution was uniformly added at 60°C and 250 r / min within 9 minutes, and stirred at 250 r / min for 2.5 hours, and filtered to obtain a surface treatment solution;

[0053] The rare earth aluminum alloy was immersed in a 2.5 mol / L hydrochloric acid solution for 5 min, ultrasonicated in deionized water for 5 min, dried at 110°C for 3 h, the surface treatment liquid was evenly applied to the surface of the rare earth aluminum alloy, and dried at 60°C for 36 h to obtain a rare earth aluminum alloy material.

[0054] Comparative Example 2

[0055] A rare earth aluminum alloy material and a preparation method thereof, mainly comprising the following preparation steps:

[0056] Aluminum, silicon dioxide, iron and magnesium are mixed in a mass ratio of 99:0.004:0.0015:0.006, heated at 740°C for 25 minutes, lanthanum with a mass of 0.15 times the mass of aluminum and cerium with a mass of 0.1 times the mass of aluminum are added, stirred at 740°C and 250r / min for 70 minutes, and a multi-component mixed gas is introduced for 25 minutes to obtain an aluminum alloy melt, which is cast into a plate to obtain an aluminum alloy crude product; the aluminum alloy crude product is kept at 520°C for 5 hours, cooled to 2.5°C, and a rare earth aluminum alloy is obtained;

[0057] p-Bromobenzaldehyde, potassium hydroxide, ethanol and ammonia water were mixed in a mass ratio of 1.8:2:47:18, stirred at 250 r / min, 1-(pyridin-2-yl)ethanone (3.75 times the molar amount of p-bromobenzaldehyde) was added at a uniform rate within 6.5 min, reacted for 40 min, heated to 55°C, reacted for 8 h under nitrogen protection, filtered, and dried at 70°C for 23 h to obtain brominated terpyridine;

[0058] Allylboronic acid pinacol ester, brominated terpyridine, tetrakis(triphenylphosphine)palladium and potassium carbonate were mixed in a molar ratio of 1.2:4:0.12:0.12, immersed in tetrahydrofuran, stirred at 250r / min, reacted for 20h at 80℃, protected from light and under nitrogen protection, dried at 65℃ for 7h, and petroleum ether and dichloromethane were mixed evenly in a mass ratio of 5:1 as a mobile phase, subjected to column chromatography, and dried at 70℃ for 23h to obtain terpyridine monomer;

[0059] The emulsifier solution and the olefin mixture were mixed at a mass ratio of 1:40, and an initiator solution 0.125 times the mass of the emulsifier solution was uniformly added at 60°C and 250 r / min within 9 minutes, and stirred at 250 r / min for 2.5 hours, and filtered to obtain a surface treatment solution;

[0060] The rare earth aluminum alloy was immersed in a 2.5 mol / L hydrochloric acid solution for 5 min, ultrasonicated in deionized water for 5 min, dried at 110°C for 3 h, the surface treatment liquid was evenly applied to the surface of the rare earth aluminum alloy, and dried at 60°C for 36 h to obtain a rare earth aluminum alloy material.

[0061] Comparative Example 3

[0062] A rare earth aluminum alloy material and a preparation method thereof, mainly comprising the following preparation steps:

[0063] Aluminum, silicon dioxide, iron and magnesium are mixed in a mass ratio of 99:0.004:0.0015:0.006, heated at 740°C for 25 minutes, lanthanum with a mass of 0.15 times the mass of aluminum and cerium with a mass of 0.1 times the mass of aluminum are added, stirred at 740°C and 250r / min for 70 minutes, and a multi-component mixed gas is introduced for 25 minutes to obtain an aluminum alloy melt, which is cast into a plate to obtain an aluminum alloy crude product; the aluminum alloy crude product is kept at 520°C for 5 hours, cooled to 2.5°C; then heated to 350°C and kept for 700 seconds, extruded into a plate to obtain a rare earth aluminum alloy;

[0064] p-Bromobenzaldehyde, potassium hydroxide, ethanol and ammonia water were mixed in a mass ratio of 1.8:2:47:18, stirred at 250 r / min, 1-(pyridin-2-yl)ethanone (3.75 times the molar amount of p-bromobenzaldehyde) was added at a uniform rate within 6.5 min, reacted for 40 min, heated to 55°C, reacted for 8 h under nitrogen protection, filtered, and dried at 70°C for 23 h to obtain brominated terpyridine;

[0065] Allylboronic acid pinacol ester, brominated terpyridine, tetrakis(triphenylphosphine)palladium and potassium carbonate were mixed in a molar ratio of 1.2:4:0.12:0.12, immersed in tetrahydrofuran, stirred at 250r / min, reacted for 20h at 80℃, protected from light and under nitrogen protection, dried at 65℃ for 7h, and petroleum ether and dichloromethane were mixed evenly in a mass ratio of 5:1 as a mobile phase, subjected to column chromatography, and dried at 70℃ for 23h to obtain terpyridine monomer;

[0066] The emulsifier solution and the terpyridine monomer were mixed at a mass ratio of 1:40, and an initiator solution of 0.125 times the mass of the emulsifier solution was uniformly added at 60°C and 250 r / min within 9 minutes, and stirred at 250 r / min for 2.5 hours, and filtered to obtain a surface treatment solution;

[0067] The rare earth aluminum alloy was immersed in a 2.5 mol / L hydrochloric acid solution for 5 min, ultrasonicated in deionized water for 5 min, dried at 110°C for 3 h, the surface treatment liquid was evenly applied to the surface of the rare earth aluminum alloy, and dried at 60°C for 36 h to obtain a rare earth aluminum alloy material.

[0068] Comparative Example 4

[0069] A rare earth aluminum alloy material and a preparation method thereof, mainly comprising the following preparation steps:

[0070] Aluminum, silicon dioxide, iron and magnesium are mixed in a mass ratio of 99:0.004:0.0015:0.006, heated at 740°C for 25 minutes, lanthanum with a mass of 0.15 times the mass of aluminum and cerium with a mass of 0.1 times the mass of aluminum are added, stirred at 740°C and 250r / min for 70 minutes, and a multi-component mixed gas is introduced for 25 minutes to obtain an aluminum alloy melt, which is cast into a plate to obtain an aluminum alloy crude product; the aluminum alloy crude product is kept at 520°C for 5 hours, cooled to 2.5°C; then heated to 350°C and kept for 700 seconds, extruded into a plate to obtain a rare earth aluminum alloy;

[0071] p-Bromobenzaldehyde, potassium hydroxide, ethanol and ammonia water were mixed in a mass ratio of 1.8:2:47:18, stirred at 250 r / min, 1-(pyridin-2-yl)ethanone (3.75 times the molar amount of p-bromobenzaldehyde) was added at a uniform rate within 6.5 min, reacted for 40 min, heated to 55°C, reacted for 8 h under nitrogen protection, filtered, and dried at 70°C for 23 h to obtain brominated terpyridine;

[0072] Allylboronic acid pinacol ester, brominated terpyridine, tetrakis(triphenylphosphine)palladium and potassium carbonate were mixed in a molar ratio of 1.2:4:0.12:0.12, immersed in tetrahydrofuran, stirred at 250r / min, reacted for 20h at 80℃, protected from light and under nitrogen protection, dried at 65℃ for 7h, and petroleum ether and dichloromethane were mixed evenly in a mass ratio of 5:1 as a mobile phase, subjected to column chromatography, and dried at 70℃ for 23h to obtain terpyridine monomer;

[0073] The emulsifier solution and the olefin mixture were mixed at a mass ratio of 1:40, and an initiator solution 0.125 times the mass of the emulsifier solution was uniformly added at 60°C and 250 r / min within 9 minutes, and stirred at 250 r / min for 2.5 hours, and filtered to obtain a surface treatment solution;

[0074] The surface treatment liquid was evenly applied on the surface of the rare earth aluminum alloy, and dried at 60° C. for 36 hours to obtain the rare earth aluminum alloy material.

[0075] Test Example 1

[0076] Mechanical properties test

[0077] The samples were made into 18 cm × 2.5 cm × 1 cm strips and tested for tensile strength and yield strength. The results are shown in Table 1.

[0078] Table 1

[0079]

[0080] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 1, it can be found that the rare earth aluminum alloy material prepared by the present invention has good mechanical properties.

[0081] From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 1 in Table 1, it can be found that the tensile strength and yield strength of Examples 1, 2, 3 are greater than those of Comparative Example 2, which shows that homogenization can improve or eliminate the structural defects and residual stresses generated during casting, forging, rolling and welding, refine the grains, improve the structure, improve the mechanical properties of the workpiece, remove internal defects such as pores, inclusions, liquid metal, etc., make the material properties more stable, thereby improving the mechanical properties of the material and increasing the tensile strength and yield strength of the material;

[0082] From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 2, it can be found that the tensile strength and yield strength of Examples 1, 2, 3 are greater than those of Comparative Example 2, which shows that complete annealing can recrystallize and rearrange the grains of the material, while eliminating dislocations and gaps, so that the plasticity and toughness of the material are improved, and the grains of the material can be uniformly refined and rearranged, and internal defects can be eliminated, thereby improving the strength and hardness of the material, improving the mechanical properties of the material, and increasing the tensile strength and yield strength of the material.

[0083] Test Example 2

[0084] Hydrophobicity test

[0085] Test method: Test water contact angle. The results are shown in Table 2.

[0086] Table 2

[0087]

[0088] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 2, it can be found that the rare earth aluminum alloy material prepared by the present invention has good hydrophobicity.

[0089] From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 3 in Table 2, it can be found that the water contact angles of Examples 1, 2, 3 are larger than that of Comparative Example 3, which shows that the long carbon chain of heptene can increase the dispersion force between molecules and enhance the interaction force between molecules, thereby enhancing the hydrophobicity of the material and increasing the water contact angle of the material surface.

[0090] Test Example 3

[0091] Antimicrobial testing

[0092] Test method: According to GB / T20944.3-2008 standard, Staphylococcus aureus and Cladosporium were used for testing respectively. The results are shown in Table 3.

[0093] Table 3

[0094]

[0095] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 3, it can be found that the rare earth aluminum alloy material prepared by the present invention has good antibacterial ability.

[0096] From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 4 in Table 3, it can be found that the antibacterial rates of Examples 1, 2, 3 are higher than those of Comparative Example 4, which shows that aluminum ions can combine with substances such as proteins and phosphatidic acid in the cell membrane of microorganisms, affect the integrity of the cell membrane, lead to an imbalance of substances inside and outside the cell and cell death, thereby killing bacteria, achieving an antibacterial effect, and improving the antibacterial ability of the material.

[0097] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a rare earth aluminum alloy material, characterized in that: The preparation method of the rare earth aluminum alloy material mainly includes the following preparation steps: (1) Aluminum, silicon dioxide, iron and magnesium are mixed in a mass ratio of 98.5-99.5: 0.003-0.005: 0.001-0.002: 0.005-0.007, heated at 730-750°C for 20-30 min, 0.1-0.12 times the mass of aluminum lanthanum and 0.08-0.12 times the mass of aluminum cerium are added, stirred at 720-760°C and 200-300 r / min for 60-80 min, and a multi-component mixed gas is introduced for 20-30 min to obtain an aluminum alloy melt, which is then cast to obtain an aluminum alloy crude product; the aluminum alloy crude product is kept at 510-530°C for 4-6 h, cooled to 0-5°C, then heated to 300-400°C for 600-800 s, extruded into a plate to obtain a rare earth aluminum alloy; (2) p-Bromobenzaldehyde, potassium hydroxide, ethanol and aqueous ammonia are mixed in a mass ratio of 1.6-2:1.8-2.2:46-48:16-20, stirred at 200-300 r / min, and 1-(pyridin-2-yl)ethanone (3.5-4 times the molar amount of p-Bromobenzaldehyde) is added at a uniform rate within 5-8 min, reacted for 30-50 min, heated to 50-60 °C, reacted for 7-9 h under nitrogen protection, filtered, and dried at 60-80 °C for 22-24 h to obtain brominated terpyridine; (3) Allylboronic acid pinacol ester, brominated terpyridine, tetrakis(triphenylphosphine)palladium and potassium carbonate were mixed in a molar ratio of 1-1.4:3-5:0.1-0.14:0.1-0.14, immersed in tetrahydrofuran, stirred at 200-300 r / min, reacted at 70-90°C, protected from light, under nitrogen protection for 18-22 hours, dried at 60-70°C for 6-8 hours, and petroleum ether and dichloromethane were mixed evenly in a mass ratio of 4-6:1 as a mobile phase, subjected to column chromatography, and dried at 60-80°C for 22-24 hours to obtain terpyridine monomer; (4) The terpyridine monomer and heptene are uniformly mixed in a mass ratio of 3-5:2-4 to obtain an olefin mixed solution; the emulsifier solution and the olefin mixed solution are mixed in a mass ratio of 1:30-50, and an initiator solution of 0.12-0.13 times the mass of the emulsifier solution is uniformly added at 50-70°C and 200-300 r / min within 8-10 minutes, and the mixture is stirred at 200-300 r / min for 2-3 hours, and filtered to obtain a surface treatment solution; (5) The rare earth aluminum alloy is immersed in a 2-3 mol / L hydrochloric acid solution for 4-6 min, ultrasonicated in deionized water for 4-6 min, dried at 100-120° C. for 2-4 h, the surface treatment liquid is evenly applied to the surface of the rare earth aluminum alloy, and dried at 50-70° C. for 24-48 h to obtain a rare earth aluminum alloy material.

2. The method for preparing a rare earth aluminum alloy material according to claim 1, characterized in that: The multi-component mixed gas in step (1) is prepared by uniformly mixing argon, nitrogen, carbon monoxide and chlorine in a ratio of 1:1:1:

1.

3. The method for preparing a rare earth aluminum alloy material according to claim 1, characterized in that: The casting method of step (1) adopts metal mold water-cooled semi-continuous casting technology, and the specific parameters are: furnace temperature 730°C~740°C, casting temperature 710°C~720°C, effective crystallization zone height in the continuous casting crystallizer 13~17mm, casting speed 105~115mm / min, water pressure 20~25kPa, cooling water inlet temperature 15~25°C, and outlet water temperature 35~45°C.

4. The method for preparing a rare earth aluminum alloy material according to claim 1, characterized in that: The extrusion method of step (1) is to extrude after keeping the temperature at 510°C to 530°C for 4 to 6 hours; the extrusion parameters are: extrusion pressure 180MPa to 220MPa, extrusion speed 12 to 15m / min, and extrusion temperature 450°C to 470°C.

5. The method for preparing a rare earth aluminum alloy material according to claim 1, characterized in that: The emulsifier solution in step (4) is prepared by mixing sodium dodecyl sulfate and deionized water in a mass ratio of 1:

10.

6. The method for preparing a rare earth aluminum alloy material according to claim 1, characterized in that: The initiator solution in step (4) is prepared by mixing potassium persulfate and deionized water in a mass ratio of 1:10.