Aluminum-zinc plate

By using hot dip plating process to deposit the aluminum-zinc alloy layer and coat the chromium-free passivation film and fingerprint-resistant film in the aluminum-zinc plating products for liquid crystal back plates, defects such as zinc layer cracking are solved, and product quality and user experience are improved .

CN118389981BActive Publication Date: 2024-11-12SHANDONG XINMEIDA TECH MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410497596.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-11-12
Estimated Expiration
2044-06-07

AI Technical Summary

Technical Problem

The defects such as zinc layer cracking, black spots, and horizontal white lines that appear in the downstream industries of LCD back panels, affecting user experience and product quality.

Method used

The aluminum-zinc alloy layer was deposited on the steel plate substrate by hot dip plating, and the surface was coated with chromium-free passivation film and chromium-free fingerprint-resistant fingerprint film, and finally covered with PE protective film. The aluminum-zinc alloy layer was Al-Zn-Fe- Si quadrature alloy, with surface roughness controlled between 0.6-1.2 microns, film thickness and composition are optimized to improve adhesion and corrosion resistance.

Benefits of technology

It effectively solves defects such as plating cracks, black spots, and horizontal white lines, and improves the product quality and user experience of downstream production lines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses an galvanized steel sheet, comprising a steel sheet substrate, wherein an aluminum-zinc alloy layer is deposited on the upper and lower surfaces of the steel sheet substrate by a hot-dip plating process, a chromium-free passivation film is coated on the aluminum-zinc alloy layer, a chromium-free fingerprint-resistant film is coated on the chromium-free passivation film, and a PE protective film is covered on the chromium-free fingerprint-resistant film; the galvanized steel sheet has a yield strength of 190-360 MPa, a tensile strength of 270-400 MPa, an elongation of 20-30%, and a hardness of 55-65 HRB; the application overcomes the defects of the galvanized steel sheet in the downstream production line.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of household appliances and electronic technology, and in particular to an aluminum-zinc plate. Background Art

[0002] As a new generation of energy-saving and environmentally friendly green products, aluminum-zinc-plated products for LCD backplanes are currently mainly used to make small LCD monitors and refrigerator backplanes. After replacing traditional materials with aluminum-zinc-plated products for LCD backplanes, on the one hand, the material cost is greatly reduced, and on the other hand, the manufacturing processes such as spraying that may cause environmental pollution are reduced. At the same time, its performance indicators such as strength and surface quality are more advantageous than traditional materials, so this product is widely favored by users. However, with the upgrading of materials in downstream industries and the improvement of user requirements, users are increasingly unable to accept the defects of zinc layer cracking, black spots, black spots, horizontal white lines, etc. on the surface of previous aluminum-zinc-plated products for LCD backplanes, which seriously affects the user experience. Summary of the invention

[0003] In view of the defects in the prior art, the present invention provides an aluminum-zinc plate.

[0004] The present invention is achieved through the following technical solutions:

[0005] An aluminum-zinc plate comprises a steel plate substrate, wherein an aluminum-zinc alloy layer is deposited on the upper and lower surfaces of the steel plate substrate by a hot-dip plating process, the aluminum-zinc alloy layer is coated with a chromium-free passivation film, the chromium-free passivation film is coated with a chromium-free fingerprint-resistant film, and the chromium-free fingerprint-resistant film is covered with a PE protective film; the aluminum-zinc alloy layer is a quaternary alloy layer Al-Zn-Fe-Si, and its thickness is 15 to 20 microns, wherein the mass fraction of Al is 53%-55%, the mass fraction of Zn is 43%-44%, the mass fraction of Fe is 0.5%, the mass fraction of Si is 1.2%-1.6%, and the surface roughness of the quaternary alloy layer is 0.6-1.2 microns; the yield strength of the aluminum-zinc plate is 190-360Mpa, the tensile strength is 270-400Mpa, the elongation is 20%-30%, and the hardness is 55-65HRB.

[0006] Preferably, the steel plate substrate is ordinary carbon structural steel, with a carbon content of 0.03%-0.08%, a silicon content of 0.03%-0.05%, a manganese content of 0.2%-0.3%, a sulfur content of 0.02%-0.03%, and a phosphorus content of 0.02%-0.03%.

[0007] Preferably, the steel plate substrate needs to be pretreated before the hot-dip plating process. First, the residual oil and residual iron on the surface of the steel plate substrate are removed by degreasing and cleaning, and then it enters a continuous annealing furnace. Hydrogen and nitrogen are used as media in the annealing furnace. Nitrogen is a protective gas and hydrogen is a reducing gas. Hydrogen can reduce the iron oxide on the surface of the steel plate substrate to iron.

[0008] Preferably, the pretreated steel plate substrate enters a high-temperature plating tank at 600°C, and a dense layer of quaternary crystals composed of aluminum, zinc, iron and silicon is plated on the surface of the steel plate substrate. The steel plate substrate is then quickly cooled to 40-60°C, and the surface roughness of the aluminum-zinc alloy layer is controlled to 0.6-1.2 microns through a finishing process and a straightening process.

[0009] Preferably, the thickness of the chromium-free passivation film is 0.3-0.6 micrometers, and the weight of the chromium-free passivation film is 5-10 mg / m 2 The chromium-free passivation film is coated on the aluminum-zinc alloy layer by a roller coater using a chromium-free passivating agent, and then cured in an oven at 200-300°C to form a dense chromium-free passivation film. The components of the chromium-free passivating agent include zinc oxide, aluminum oxide and magnesium oxide.

[0010] Preferably, the thickness of the chrome-free anti-fingerprint film is 1.0-2.0 microns; the chrome-free anti-fingerprint film is coated on the chrome-free passivation film by a roller coater using a chrome-free anti-fingerprint treatment liquid, and is cured in an oven at 400-500°C to form a dense chrome-free anti-fingerprint film. The chrome-free anti-fingerprint treatment liquid uses lithium silicate, glycidyloxypropyltrimethoxysilane and 1,2-bis-(trimethoxy)ethane as raw materials, wherein the mass proportion of lithium silicate is 9%-13%, the mass proportion of glycidyloxypropyltrimethoxysilane is 4%-7%, and the mass proportion of 1,2-bis-(trimethoxy)ethane is 3%-6%.

[0011] The beneficial effects of the present invention are as follows: the present invention solves the defects of coating cracking, black spots and black spots, horizontal white lines, etc. that occur in the press-forming and bending process of aluminum-zinc-plated products for liquid crystal backplanes of downstream customers, thereby improving the product quality and user experience of downstream production lines. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.

[0013] Figure 1 It is a cross-sectional view of the aluminum-zinc plate of the present invention.

[0014] Figure 2 This is a physical picture of the color difference, black spots and black spots defects on the aluminum zinc plate.

[0015] Figure 3 This is a physical picture of scratches and white stripe defects on the aluminum-zinc plate.

[0016] Figure 4 This is a real picture of the aluminum-zinc plate with excellent surface quality.

[0017] In the attached drawings, 1. steel plate substrate; 2. aluminum-zinc alloy layer; 3. chromium-free passivation film; 4. chromium-free anti-fingerprint film; 5. PE protective film. DETAILED DESCRIPTION

[0018] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0020] The present invention is described in detail below in conjunction with the accompanying drawings: an aluminum-zinc plate of the present invention comprises a steel plate substrate, an aluminum-zinc alloy layer is deposited on the upper and lower surfaces of the steel plate substrate by a hot-dip plating process, a chromium-free passivation film is coated on the aluminum-zinc alloy layer, a chromium-free fingerprint-resistant film is coated on the chromium-free passivation film, and a PE protective film is covered on the chromium-free fingerprint-resistant film; the aluminum-zinc alloy layer is a quaternary alloy layer Al-Zn-Fe-Si, and its thickness is 15 to 20 microns, wherein the mass fraction of Al is 53%-55%, the mass fraction of Zn is 43%-44%, the mass fraction of Fe is 0.5%, the mass fraction of Si is 1.2%-1.6%, and the surface roughness of the quaternary alloy layer is 0.6-1.2 microns; the yield strength of the aluminum-zinc plate is 190-360Mpa, the tensile strength is 270-400Mpa, the elongation is 20%-30%, and the hardness is 55-65HRB.

[0021] The steel plate substrate is ordinary carbon structural steel, with a carbon content of 0.03%-0.08%, a silicon content of 0.03%-0.05%, a manganese content of 0.2%-0.3%, a sulfur content of 0.02%-0.03%, and a phosphorus content of 0.02%-0.03%.

[0022] The steel plate substrate needs to be pretreated before the hot dip plating process. First, the residual oil and residual iron on the surface of the steel plate substrate are removed by degreasing and cleaning, and then it enters a continuous annealing furnace. Hydrogen and nitrogen are used as media in the annealing furnace. Nitrogen is a protective gas and hydrogen is a reducing gas. The iron oxide on the surface of the steel plate substrate can be reduced to iron by hydrogen.

[0023] After pretreatment, the steel plate substrate enters a high-temperature plating tank at 600℃, and a dense quaternary crystal is plated on the surface of the steel plate substrate. The quaternary crystal is composed of aluminum, zinc, iron and silicon. Then the steel plate substrate is quickly cooled to 40-60℃, and the surface roughness of the aluminum-zinc alloy layer is controlled to 0.6-1.2 microns through the finishing process and the straightening process. The surface roughness of the aluminum-zinc alloy layer is controlled in this range to ensure the adhesion of the subsequent chromium-free passivation film. When the surface roughness is lower than 0.6 microns, the surface friction coefficient is very small, and the adhesion of the chromium-free passivation film will be very poor. When the surface roughness is higher than 1.2 microns, it will affect the aesthetics of the aluminum-zinc plate.

[0024] The thickness of the chromium-free passivation film is 0.3-0.6 micrometers, and the weight of the chromium-free passivation film is 5-10 mg / m 2 ; When the thickness of the chromium-free passivation film is greater than 0.6 microns and the weight is greater than 10 mg / m 2 When the thickness of the chromium-free passivation film is less than 0.3 microns and the weight is less than 5 mg / m 2 The corrosion resistance of the aluminum-zinc plate will deteriorate, greatly shortening its service life; the chromium-free passivation film is coated on the aluminum-zinc alloy layer by a roller coater using a chromium-free passivating agent, and then cured in an oven at 200-300°C to form a dense chromium-free passivation film. The chromium-free passivating agent is a chemical substance used for metal surface treatment, mainly used to prevent metal oxidation and corrosion. Its main components include zinc oxide, aluminum oxide and magnesium oxide, which can effectively form a protective film on the metal surface to prevent oxidation and corrosion.

[0025] The film thickness of the chrome-free anti-fingerprint film is 1.0-2.0 microns. It is found through experiments that when the film thickness is less than 1.0 micron, defects such as black spots and black spots are prone to appear in the downstream embossing and bending process. When the film thickness is higher than 2.0 microns, the aluminum-zinc plated product is prone to color difference defects caused by anti-fingerprint adhesion. When the film thickness is within this numerical range, when the pattern is higher than 100 degrees Celsius, the anti-fingerprint coating has better fingerprint resistance, corrosion resistance and high temperature resistance. The chrome-free anti-fingerprint film is coated on the chrome-free passivation film by a roller coating method using a chrome-free anti-fingerprint treatment liquid through a roller coater, and is cured in an oven at 400-500°C to form a dense chrome-free anti-fingerprint film. The chrome-free anti-fingerprint treatment liquid uses lithium silicate, glycidyloxypropyltrimethoxysilane and 1,2-bis-(trimethoxy)ethane as raw materials, and is prepared into a chrome-free anti-fingerprint treatment liquid with excellent high-temperature baking resistance by a sol-gel method and organic-inorganic hybrid technology, and the chrome-free anti-fingerprint coating is prepared based on the treatment liquid. The mass proportion of lithium silicate in the chromium-free anti-fingerprint treatment liquid is 9%-13%, the mass proportion of glycidyloxypropyltrimethoxysilane is 4%-7%, and the mass proportion of 1,2-bis-(trimethoxy)ethane is 3%-6%.

[0026] Three experiments were conducted on the ratio of the three raw materials of the chrome-free anti-fingerprint treatment liquid:

[0027] In the first experiment, when the mass ratios of the three raw materials were higher than the above-mentioned range values, the downstream industry had color difference, black spots and black spots defects in the aluminum-zinc plate during use. The actual picture is as follows Figure 2 As shown;

[0028] In the second experiment, when the mass ratios of the three raw materials were all lower than the above-mentioned range, the galvanized aluminum sheet was scratched and had white line defects during use by the downstream industry. Figure 3 As shown;

[0029] In the third experiment, when the mass proportion of the three raw materials was controlled within the above range, there was no abnormality in the downstream industry during use, and the surface quality was excellent. The actual picture is as follows Figure 4 shown.

[0030] The product is an alloy steel sheet in which an aluminum-zinc alloy coating is deposited on a steel sheet substrate by a hot-dip coating process. It uses low-carbon steel cold-hardened coil as raw material, and removes residual oil and iron on the surface of the steel plate substrate through pre-treatment degreasing and cleaning, and then enters the continuous annealing furnace. Hydrogen and nitrogen are used as media in the annealing furnace, nitrogen is a protective gas, and hydrogen is a reducing gas. The iron oxide on the surface of the steel plate substrate is reduced to iron by hydrogen, and then enters a 600°C high-temperature plating tank to plate a dense quaternary crystal on the surface of the steel plate substrate. The entire structure is composed of aluminum-iron-silicon-zinc, and then the steel plate substrate is quickly cooled by a combination of air cooling and water cooling. After the steel plate substrate is cooled to 40-60°C, the surface roughness of the quaternary alloy layer is controlled to 0.6-1.2 microns through the finishing process and the straightening process, and then enters the post-processing stage. A layer of chromium-free passivation film and a chromium-free fingerprint-resistant film are successively coated on the surface by a roller coater. Finally, it enters the cold lamination stage, and a layer of PE protective film is attached to the surface by a laminating machine to finally obtain this product.

[0031] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.

Claims

1. An galvanized steel sheet, comprising a steel sheet substrate (1), characterized in that: The aluminum-zinc alloy layer (2) is deposited on the upper and lower surfaces of the steel plate substrate (1) by a hot-dip plating process, the aluminum-zinc alloy layer (2) is coated with a chromium-free passivation film (3), the chromium-free passivation film (3) is coated with a chromium-free fingerprint-resistant film (4), and the chromium-free fingerprint-resistant film (4) is covered with a PE protective film (5); the aluminum-zinc alloy layer (2) is a quaternary alloy layer of Al-Zn-Fe-Si, with a thickness of 15 to 20 microns, wherein the mass fraction of Al is 53% to 55%, the mass fraction of Zn is 43% to 44%, the mass fraction of Fe is 0.5%, and the mass fraction of Si is 1.2% to 1.6%, and the surface roughness of the quaternary alloy layer is 0.6 to 1.2 microns; the yield strength of the aluminum-zinc plate is 190 to 360 MPa, the tensile strength is 270 to 400 MPa, the elongation is 20% to 30%, and the hardness is 55 to 65 HRB; The thickness of the chromium-free passivation film (3) is 0.3-0.6 micrometers, and the weight of the chromium-free passivation film (3) is 5-10 mg / m 2 The chromium-free passivation film (3) is coated on the aluminum-zinc alloy layer (2) by a chromium-free passivation agent through a roller coating machine, and then cured in an oven at 200-300° C. to form a dense chromium-free passivation film (3). The components of the chromium-free passivation agent include zinc oxide, aluminum oxide and magnesium oxide. The film thickness of the chrome-free anti-fingerprint film (4) is 1.0-2.0 microns. The chrome-free anti-fingerprint film (4) is coated on the chrome-free passivation film (3) by a roller coating method using a chrome-free anti-fingerprint treatment liquid, and then cured in an oven at 400-500° C. to form a dense chrome-free anti-fingerprint film (4). The chrome-free anti-fingerprint treatment liquid uses lithium silicate, glycidyloxypropyltrimethoxysilane and 1,2-bis-(trimethoxy)ethane as raw materials, wherein the mass proportion of lithium silicate is 9%-13%, the mass proportion of glycidyloxypropyltrimethoxysilane is 4%-7%, and the mass proportion of 1,2-bis-(trimethoxy)ethane is 3%-6%.

2. The galvanized sheet according to claim 1, characterized in that: The steel plate substrate (1) is ordinary carbon structural steel, and has a carbon content of 0.03%-0.08%, a silicon content of 0.03%-0.05%, a manganese content of 0.2%-0.3%, a sulfur content of 0.02%-0.03%, and a phosphorus content of 0.02%-0.03%.

3. The galvanized sheet according to claim 1, characterized in that: The steel plate substrate (1) needs to be pretreated before the hot dip coating process. First, residual oil and residual iron on the surface of the steel plate substrate (1) are removed by degreasing and cleaning, and then the steel plate substrate (1) is placed in a continuous annealing furnace. Hydrogen and nitrogen are used as media in the annealing furnace. Nitrogen is a protective gas and hydrogen is a reducing gas. The hydrogen can reduce the iron oxide on the surface of the steel plate substrate (1) into iron.

4. The galvanized sheet according to claim 3, characterized in that: The pretreated steel plate substrate (1) enters a high-temperature plating tank at 600°C, and a dense quaternary crystal layer is plated on the surface of the steel plate substrate (1). The quaternary crystal layer is composed of aluminum, zinc, iron and silicon. The steel plate substrate (1) is then rapidly cooled to 40-60°C, and the surface roughness of the aluminum-zinc alloy layer (2) is controlled to be 0.6-1.2 microns through a finishing process and a straightening process.