A gadolinium-praseodymium zirconate ceramic target material, preparation method and application thereof
Through the low-temperature sintering and secondary high-temperature sintering processes of gadolinium priseratidyl zirconate ceramic materials, the problem of limited service life of existing thermal barrier coatings at high temperatures is solved, and the performance of low thermal conductivity, high thermal expansion coefficient and high fracture toughness is achieved. Improves the thermal cycling performance and high temperature stability of the thermal barrier coating.
Patent Information
- Application Number
- CN202410492678.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-04-23
AI Technical Summary
Existing yttrium oxide-stabilized zirconia (8YSZ) thermal barrier coatings have limited service life at high temperatures and cannot meet the needs of gas turbines and turbine engines with higher thrust-to-weight ratios and higher combustion temperatures, while rare earth zirconate materials are low in fracture Toughness and thermal expansion coefficient lead to poor thermal cycling performance of thermal barrier coatings.
Using gadolinium priseratidium zirconate ceramic material (Gd1-xPrx) 2Zr2O7, secondary high-temperature sintering is carried out after low temperature sintering and mechanical processing to form nanostructure agglomerates with low thermal conductivity, high thermal expansion coefficient and high fracture toughness, used to prepare thermal barriers coating.
It improves the mechanical properties of gadolinium priseratidium zirconate ceramic materials, reduces thermal conductivity, improves the thermal expansion coefficient, enhances the thermal cycle performance and high temperature stability of the thermal barrier coating, and extends the life of the coating.
Smart Images

Figure CN118390000B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of ceramic target materials, and in particular to a gadolinium-praseodymium zirconate ceramic target material, a preparation method and an application thereof. Background Art
[0002] Thermal barrier coatings usually refer to a layer of ceramic coating deposited on the surface of high-temperature alloys. Its main purpose is to reduce the surface temperature of the base alloy, thereby ensuring that the alloy (such as engine turbine blades) can operate at higher temperatures and further improve its safety. The most widely used thermal barrier coating ceramic material is yttria-stabilized zirconia (8YSZ). However, due to the phase change and sintering problems of 8YSZ, its long-term service temperature cannot exceed 1200°C, which cannot meet the needs of gas turbines and turbine engines with higher thrust-to-weight ratios and higher combustion temperatures. There is an urgent need to develop new ultra-high temperature thermal barrier coating materials.
[0003] Rare earth zirconates represented by Gd2Zr2O7 have become one of the most promising new generation thermal barrier coating ceramic materials due to their lower thermal conductivity, higher phase stability and thermal expansion coefficient closer to 8YSZ. However, gadolinium zirconate ceramic materials have poor thermal cycling performance in thermal barrier coatings due to their lower fracture toughness and thermal expansion coefficient.
[0004] Therefore, how to further reduce thermal conductivity while improving properties such as fracture toughness and thermal expansion coefficient is a key issue that Gd2Zr2O7 ceramic materials need to solve as a new generation of thermal barrier coating materials. Summary of the invention
[0005] The present application provides a gadolinium-praseodymium zirconate ceramic target material, a preparation method and an application thereof to solve the above-mentioned problems.
[0006] In a first aspect of an embodiment of the present application, a gadolinium zirconate praseodymium ceramic target is provided, wherein the chemical formula of the gadolinium zirconate is (Gd 1-x Pr x )2Zr2O7, where 0<x≤0.15.
[0007] In an optional embodiment of the present application, the relative density of the gadolinium praseodymium zirconate ceramic target is 60% to 85%, and the physical phase structure of the gadolinium praseodymium zirconate ceramic target is a fluorite structure.
[0008] In an optional embodiment of the present application, the 1200K material thermal conductivity of the gadolinium-praseodymium zirconate ceramic target is 1-2 W / m·K, and the thermal expansion coefficient is 10-12K -1 , fracture toughness is 1~2MPa·m 1 / 2 .
[0009] In a second aspect of an embodiment of the present application, there is provided a method for preparing a gadolinium-praseodymium zirconate ceramic target as described in any one of the first aspects above, the method comprising the following steps:
[0010] Step 1: According to the chemical formula (Gd 1-x Pr x )2Zr2O7, Gd2O3, ZrO2 and praseodymium oxide were weighed as reaction raw materials, and gadolinium zirconate praseodymium powder with the morphology of nanostructured aggregates was synthesized;
[0011] Step 2: spray granulating the gadolinium zirconate powder to obtain granulated powder with an average particle size of 1-30 microns;
[0012] Step 3: sequentially cold isostatic pressing and first high-temperature sintering the granulated powder, machining the blank after the first high-temperature sintering and then performing a second high-temperature sintering to obtain the gadolinium zirconate praseodymium ceramic target;
[0013] The molding pressure of the cold isostatic pressing is 100MPa to 300MPa, and the holding time is 1min to 10min;
[0014] The temperature of the first high temperature sintering is 900°C to 1300°C, and the holding time is 2h to 6h;
[0015] The temperature of the second high-temperature sintering is 1300°C ~ 1650°C, and the insulation time is 2h ~ 6h.
[0016] In an optional embodiment of the present application, the first high-temperature sintering is performed by a gradient temperature increase method, including:
[0017] The high temperature sintering under gradient temperature increase is to heat to 300-500°C at a temperature increase rate of 0.5-10°C / min in a high temperature sintering furnace in an air or oxygen-enriched air atmosphere, and sinter for 30-60min; then heat to 900-1300°C at a temperature increase rate of 0.5-10°C / min, sinter for 2-6h; and finally cool to room temperature at a temperature reduction rate of 0.5-10°C / min.
[0018] In an optional embodiment of the present application, the second high-temperature sintering is performed by a gradient temperature increase method, including:
[0019] The high temperature sintering under gradient temperature increase is to heat to 600-800°C at a temperature increase rate of 5-10°C / min in a high temperature sintering furnace in an air or oxygen-enriched air atmosphere, and sinter for 30-60min; then heat to 1300-1650°C at a temperature increase rate of 1-3°C / min, sinter for 2-6h; and finally cool to room temperature at a temperature decrease rate of 1-3°C / min.
[0020] In an optional embodiment of the present application, in step 1, the gadolinium praseodymium zirconate powder with the morphology of nanostructure agglomerates is synthesized by the following steps:
[0021] Step 1-1: dissolving the reaction raw materials in concentrated nitric acid to prepare a 0.3-0.9 mol / L rare earth solution;
[0022] Step 1-2: adding the rare earth solution dropwise into ammonia water, controlling the pH value of the rare earth solution to 9-12, and obtaining a precursor precipitate after precipitation;
[0023] Step 1-3: filtering, washing and drying the precursor precipitate to obtain a precursor powder through sieving, the drying temperature is 100-150° C. and the drying time is 10-30 h;
[0024] Step 1-4: calcining the precursor powder at high temperature to generate the desired physical structure of gadolinium praseodymium zirconate. The calcined powder is ball-milled to obtain gadolinium praseodymium zirconate powder with the morphology of nanostructured agglomerates. The high-temperature calcination temperature is 700-1200° C. for 1-5 hours. The desired physical structure of gadolinium praseodymium zirconate is a fluorite structure.
[0025] In an optional embodiment of the present application, in the steps 1-4, the temperature for high-temperature calcination of the precursor powder is 900°C.
[0026] In an optional embodiment of the present application, in step 1, the praseodymium oxide in the reaction raw material is Pr2O3 or Pr6O 11 .
[0027] In a third aspect of the embodiment of the present application, an application of a gadolinium-praseodymium zirconate ceramic target is provided, wherein the gadolinium-praseodymium zirconate ceramic target is used to prepare a thermal barrier coating for aero-engine and gas turbine blades by electron beam physical vapor deposition.
[0028] The chemical formula of gadolinium zirconate praseodymium in the gadolinium zirconate ceramic target is (Gd 1-x Pr x )2Zr2O7; wherein 0<x≤0.15.
[0029] The present application has the following advantages: The present application provides a gadolinium zirconate praseodymium ceramic target, a preparation method and an application thereof, wherein the chemical formula of the gadolinium zirconate is (Gd 1-x Pr x)2Zr2O7, where 0<x≤0.15. The mechanical properties of gadolinium zirconate praseodymium ceramic targets can be improved by first sintering at low temperature, processing and then secondary sintering. Compared with gadolinium zirconate, the targets have lower thermal conductivity and higher thermal expansion coefficient. The lower thermal conductivity is conducive to improving the thermal cycle performance and high temperature stability of the thermal barrier coating of the aircraft engine, and the higher thermal expansion coefficient is conducive to the matching of the thermal barrier coating with the substrate, thereby improving the thermal cycle life of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the description of the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0031] Figure 1 It is a flow chart of the steps of a method for preparing a gadolinium-praseodymium zirconate ceramic target provided in an embodiment of the present application;
[0032] Figure 2 It is a schematic diagram of the phase structure of a gadolinium-praseodymium zirconate ceramic target prepared in Example 1 provided in the examples of the present application;
[0033] Figure 3 This is a schematic diagram of the phase structure of a gadolinium-praseodymium zirconate ceramic target prepared in Example 2 provided in the examples of the present application;
[0034] Figure 4 This is a schematic diagram of the phase structure of a gadolinium-praseodymium zirconate ceramic target prepared in Example 3 provided in the examples of the present application. DETAILED DESCRIPTION
[0035] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0036] Thermal barrier coatings usually refer to a layer of ceramic coating deposited on the surface of high-temperature alloys. Its main purpose is to reduce the surface temperature of the base alloy, thereby ensuring that the alloy (such as engine turbine blades) can operate at higher temperatures and further improve its safety. The most widely used thermal barrier coating ceramic material is yttria-stabilized zirconia (8YSZ). However, due to the phase change and sintering problems of 8YSZ, its long-term service temperature cannot exceed 1200°C, which cannot meet the needs of gas turbines and turbine engines with higher thrust-to-weight ratios and higher combustion temperatures. There is an urgent need to develop new ultra-high temperature thermal barrier coating materials.
[0037] Rare earth zirconates represented by Gd2Zr2O7 have become one of the most promising new generation thermal barrier coating ceramic materials due to their lower thermal conductivity, higher phase stability and thermal expansion coefficient closer to 8YSZ. However, gadolinium zirconate ceramic materials have poor thermal cycling performance in thermal barrier coatings due to their lower fracture toughness and thermal expansion coefficient.
[0038] Based on this, the present application proposes a thermal barrier coating material with low thermal conductivity, high thermal expansion coefficient and excellent high-temperature stability, and a ceramic target material and a manufacturing method for the thermal barrier coating.
[0039] In a first aspect of the present application, a gadolinium zirconate praseodymium ceramic target is provided, wherein the chemical formula is (Gd 1-x Pr x )2Zr2O7, where 0<x≤0.15. When x=0.05, the chemical formula of the gadolinium zirconate ceramic target is (Gd 0.95 Pr 0.05 )2Zr2O7; when x = 0.1, the chemical formula of the gadolinium zirconate ceramic target is (Gd 0.9 Pr 0.1 )2Zr2O7; when x = 0.15, the chemical formula of the gadolinium zirconate ceramic target is (Gd 0.85 Pr 0.15 )2Zr2O7. The relative density of the gadolinium-praseodymium zirconate ceramic target is 60% to 85%, and the physical structure of the gadolinium-praseodymium zirconate ceramic target is a fluorite structure.
[0040] The thermal conductivity, thermal expansion coefficient and fracture toughness of the above-mentioned gadolinium zirconate praseodymium ceramic target at 1200K were evaluated, and the thermal conductivity of the above-mentioned gadolinium zirconate praseodymium ceramic target at 1200K was 1-2W / m·K, and the thermal expansion coefficient was 10-12K. -1 , fracture toughness is 1~2MPa·m 1 / 2 It can be seen that the gadolinium-praseodymium zirconate ceramic target in the present application is a ceramic target with low thermal conductivity, high thermal expansion coefficient and high temperature stability, which can be used to prepare thermal barrier coatings.
[0041] In a second aspect of the present application, a method for preparing a gadolinium zirconate praseodymium ceramic target is provided. Figure 1 , Figure 1 1 is a flow chart of a method for preparing a gadolinium zirconate praseodymium ceramic target provided in an embodiment of the present application, the method comprising the following steps:
[0042] Step 1: According to the chemical formula (Gd 1-x Pr x )2Zr2O7, Gd2O3, ZrO2 and praseodymium oxide were weighed as reaction raw materials, and gadolinium zirconate praseodymium powder with the morphology of nanostructured aggregates was synthesized;
[0043] Step 2: spray granulating the gadolinium zirconate powder to obtain granulated powder with an average particle size of 1-30 microns;
[0044] Step 3: The granulated powder is subjected to cold isostatic pressing and the first high-temperature sintering in sequence, and the blank after the first high-temperature sintering is subjected to mechanical processing and then to a second high-temperature sintering to obtain the gadolinium zirconate praseodymium ceramic target; wherein the molding pressure of the cold isostatic pressing is 100MPa~300MPa, and the holding time is 1min~10min; the temperature of the first high-temperature sintering is 900℃~1300℃, and the holding time is 2h~6h; the temperature of the second high-temperature sintering is 1300℃~1650℃, and the holding time is 2h~6h.
[0045] In step 1, the praseodymium oxide in the above reaction raw materials is Pr2O3 or Pr6O 11 That is, the above reaction raw materials can be Gd2O3, ZrO2 and Pr2O3, or Gd2O3, ZrO2 and Pr6O 11 .
[0046] In an optional embodiment of the present application, in step 1, the gadolinium praseodymium zirconate powder with the morphology of nanostructure agglomerates is synthesized by the following steps:
[0047] Step 1-1: dissolving the reaction raw materials in concentrated nitric acid to prepare a 0.3-0.9 mol / L rare earth solution;
[0048] Step 1-2: adding the rare earth solution dropwise into ammonia water, controlling the pH value of the rare earth solution to 9-12, and obtaining a precursor precipitate after precipitation;
[0049] Step 1-3: filtering, washing and drying the precursor precipitate to obtain a precursor powder through sieving, the drying temperature is 100-150° C. and the drying time is 10-30 h;
[0050] Step 1-4: calcining the precursor powder at high temperature to generate the desired physical structure of gadolinium praseodymium zirconate. The calcined powder is ball-milled to obtain gadolinium praseodymium zirconate powder with the morphology of nanostructured agglomerates. The high-temperature calcination temperature is 700-1200° C. for 1-5 hours. The desired physical structure of gadolinium praseodymium zirconate is a fluorite structure.
[0051] In the above step 1-2, dilute ammonia water is used as a precipitant, and the rare earth solution is added dropwise into the dilute ammonia water. In this step, the rare earth ions react with the ammonia water to generate a precursor precipitate.
[0052] In the above steps 1-3, after a period of standing, the structure of the precursor precipitate becomes more stable. Then, through the steps of washing, filtering and drying, excess water and impurities are removed to obtain a precursor powder.
[0053] In the above steps 1-4, the precursor powder is calcined to cause a solid phase reaction at high temperature to generate the desired fluorite structure. The calcined powder is then ball milled to make its particle size more uniform to obtain the final gadolinium praseodymium zirconate powder. The temperature for high temperature calcination of the above precursor powder can be 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, preferably 900°C.
[0054] In an optional embodiment of the present application, in step 1, gadolinium zirconate praseodymium powder with the morphology of nanostructured agglomerates can also be synthesized by a sol-gel method. In addition, gadolinium zirconate praseodymium powder with a particle size distribution of D90 less than 20 microns can also be prepared by a high-temperature solid phase synthesis method. Specifically, the above-mentioned reaction raw materials are mixed by ball milling, and then after a high-temperature solid phase reaction, the reaction product is ball milled to obtain gadolinium zirconate praseodymium powder. The physical phase structure of the gadolinium zirconate powder with the morphology of nanostructured agglomerates obtained by the above reaction and the gadolinium zirconate powder with a particle size distribution of D90 less than 20 microns are both fluorite structures.
[0055] In step 2, the gadolinium praseodymium zirconate powder obtained in step 1 is subjected to spray granulation treatment to obtain granulated powder with an average particle size of 1-30 microns. Optionally, granulated powder can be obtained by a molding granulation method, wherein the spray granulation or molding granulation method is the same as that in the related art. Please refer to the description of the related art for details, which will not be repeated here.
[0056] In step 3, the granulated powder obtained in step 2 is subjected to cold isostatic pressing at a pressure of preferably 150 MPa to 250 MPa.
[0057] After the cold isostatic pressing treatment, the first high-temperature sintering and the second high-temperature sintering are both carried out in a gradient temperature increase manner. Specifically, the first high-temperature sintering is carried out in a gradient temperature increase manner, including: the high-temperature sintering under the above-mentioned gradient temperature increase is to heat to 300-500°C at a heating rate of 0.5-10°C / min in a high-temperature sintering furnace in an air or oxygen-enriched air atmosphere, and sinter for 30-60min; then heat to 900-1300°C at a heating rate of 0.5-10°C / min, sinter for 2-6h; finally cool to room temperature at a cooling rate of 0.5-10°C / min. The second high-temperature sintering is carried out in a gradient heating method, including: the high-temperature sintering under the above-mentioned gradient heating is to heat to 600-800°C at a heating rate of 5-10°C / min in a high-temperature sintering furnace in an air or oxygen-enriched air atmosphere, and sinter for 30-60min; then heat to 1300-1650°C at a heating rate of 1-3°C / min, sinter for 2-6h; finally cool to room temperature at a cooling rate of 1-3°C / min.
[0058] The powder morphology of gadolinium zirconate and praseodymium is a nanostructured agglomerate, which can improve the sintering performance of the powder and reduce the sintering temperature of the target material. Combined with the method of first sintering at a low temperature and then performing a secondary sintering after processing, it can improve the mechanical properties of the gadolinium zirconate and praseodymium ceramic target material and avoid the problems of poor mechanical properties of the target material after high-temperature sintering, easy cracking and difficult processing.
[0059] In a third aspect of the embodiment of the present application, an application of a gadolinium-praseodymium zirconate ceramic target is provided, wherein the gadolinium-praseodymium zirconate ceramic target is used to prepare thermal barrier coatings for turbine blades of aircraft engines and gas turbines by electron beam physical vapor deposition; wherein the chemical formula of gadolinium-praseodymium zirconate in the gadolinium-praseodymium zirconate ceramic target is (Gd 1-x Pr x )2Zr2O7; wherein 0<x≤0.15.
[0060] In order to enable those skilled in the art to understand the present application more clearly, the gadolinium zirconate praseodymium ceramic target material, preparation method and application thereof described in the present application are now described in detail through the following examples.
[0061] Example 1
[0062] Step 1: According to (Gd 0.95 Pr 0.05 )2Zr2O7 The reaction raw materials were weighed in a mass ratio of Gd2O3:Pr2O3:ZrO2 = 56.74:40.43:2.83, and the coprecipitation method was used to prepare (Gd 0.95 Pr 0.05 )2Zr2O7 powder.
[0063] Step 2: (Gd 0.95 Pr 0.05)2Zr2O7 powder is subjected to centrifugal spray granulation to obtain granulated powder, and the average particle size of the granulated powder is 3 microns.
[0064] Step 3: After the granulated powder is loaded into the mold, it is cold isostatically pressed with a molding pressure of 150 MPa. After the pressure holding time is 5 minutes, it is heated to 350°C in a high-temperature sintering furnace at a heating rate of 3°C / min, sintered for 30 minutes, and then heated to 1200°C at a heating rate of 10°C / min, sintered for 2 hours, and then processed by a precision lathe to the target size (not exceeding 0.5mm dimensional positive tolerance), heated to 650°C at a heating rate of 5°C / min, sintered for 30 minutes, and then heated to 1400°C at a heating rate of 2°C / min and sintered for 2 hours to obtain a gadolinium zirconate praseodymium ceramic target.
[0065] The coprecipitation method in step 1 is specifically:
[0066] Step 1-1: dissolving the reaction raw materials in concentrated nitric acid to prepare a 0.7 mol / L rare earth solution;
[0067] Step 1-2: adding the rare earth solution dropwise into ammonia water, controlling the pH value of the rare earth solution to 10, and obtaining a precursor precipitate after precipitation;
[0068] Step 1-3: filtering, washing and drying the precursor precipitate to obtain a precursor powder through sieving, with the drying temperature being 150° C. and the drying time being 30 h;
[0069] Step 1-4: The precursor powder is calcined at 900° C. for 3 hours to generate the desired gadolinium praseodymium zirconate phase structure. The calcined powder is ball-milled to obtain gadolinium praseodymium zirconate powder with the morphology of nanostructured agglomerates. The desired gadolinium praseodymium zirconate phase structure is a fluorite structure.
[0070] Example 2
[0071] Step 1: According to (Gd 0.95 Pr 0.05 )2Zr2O7 weigh the reaction raw materials in proportion, the mass ratio is Gd2O3:Pr6O 11 :ZrO2=53.7:40.65:5.65, prepared by coprecipitation method (Gd 0.9 Pr 0.1 )2Zr2O7 powder, the powder particle size D50 is 18 microns.
[0072] Step 2: (Gd 0.9 Pr 0.1 )2Zr2O7 powder is refined by ball milling and then granulated by molding. The average particle size of the granulated powder is 5 microns.
[0073] Step 3: After the granulated powder is loaded into the mold, it is cold isostatically pressed with a molding pressure of 180 MPa. After the pressure holding time is 8 minutes, it is heated to 350°C in a high-temperature sintering furnace at a heating rate of 3°C / min, sintered for 30 minutes, and then heated to 1300°C at a heating rate of 10°C / min, sintered for 5 hours, and then processed by a precision lathe to the target size (not exceeding 0.5mm dimensional positive tolerance), heated to 650°C at a heating rate of 5°C / min, sintered for 30 minutes, and then heated to 1600°C at a heating rate of 2°C / min and sintered for 5 hours to obtain a gadolinium zirconate praseodymium ceramic target.
[0074] The coprecipitation method in step 1 is specifically:
[0075] Step 1-1: dissolving the reaction raw materials in concentrated nitric acid to prepare a 0.5 mol / L rare earth solution;
[0076] Step 1-2: adding the rare earth solution dropwise into ammonia water, controlling the pH value of the rare earth solution to 10, and obtaining a precursor precipitate after precipitation;
[0077] Step 1-3: filtering, washing and drying the precursor precipitate, sieving to obtain the precursor powder, the drying temperature is 150° C. and the drying time is 25 h;
[0078] Step 1-4: The precursor powder is calcined at 900° C. for 3 hours to generate the desired gadolinium praseodymium zirconate phase structure. The calcined powder is ball-milled to obtain gadolinium praseodymium zirconate powder with the morphology of nanostructured agglomerates. The desired gadolinium praseodymium zirconate phase structure is a fluorite structure.
[0079] Example 3
[0080] Step 1: According to (Gd 0.85 Pr 0.15 )2Zr2O7 weigh the reaction raw materials in proportion, the mass ratio is Gd2O3:Pr6O 11 :ZrO2=50.87:40.65:8.48, prepared by coprecipitation method (Gd 0.85 Pr 0.15 )2Zr2O7 powder, powder particle size D50 is 15 microns.
[0081] Step 2: (Gd 0.85 Pr 0.15 )2Zr2O7 powder is refined by ball milling and then granulated by molding. The average particle size of the granulated powder is 4 microns.
[0082] Step 3: After the granulated powder is loaded into the mold, it is cold isostatically pressed with a molding pressure of 250 MPa. After the pressure holding time is 10 minutes, it is heated to 350°C in a high-temperature sintering furnace at a heating rate of 3°C / min, sintered for 30 minutes, and then heated to 1300°C at a heating rate of 10°C / min, sintered for 5 hours, and then processed by a precision lathe to the target size (not exceeding 0.5mm dimensional positive tolerance), heated to 650°C at a heating rate of 5°C / min, sintered for 30 minutes, and then heated to 1650°C at a heating rate of 2°C / min and sintered for 6 hours to obtain a gadolinium zirconate praseodymium ceramic target.
[0083] The coprecipitation method in step 1 is specifically:
[0084] Step 1-1: dissolving the reaction raw materials in concentrated nitric acid to prepare a 0.4 mol / L rare earth solution;
[0085] Step 1-2: adding the rare earth solution dropwise into ammonia water, controlling the pH value of the rare earth solution to 11, and obtaining a precursor precipitate after precipitation;
[0086] Step 1-3: filtering, washing and drying the precursor precipitate to obtain a precursor powder through sieving, with the drying temperature being 150° C. and the drying time being 30 h;
[0087] Step 1-4: calcining the precursor powder at 900° C. for 5 hours to generate the desired gadolinium praseodymium zirconate phase structure. The calcined powder is ball-milled to obtain gadolinium praseodymium zirconate powder with the morphology of nanostructured agglomerates. The desired gadolinium praseodymium zirconate phase structure is a fluorite structure.
[0088] Example 4
[0089] Step 1: According to (Gd 0.9 Yb 0.1 )2Zr2O7 The reaction raw materials were weighed in a mass ratio of Gd2O3:Yb2O3:ZrO2 = 53.30:6.44:40.26, and the coprecipitation method was used to prepare (Gd 0.9 Yb 0.1 )2Zr2O7 powder.
[0090] Step 2: (Gd 0.9 Yb 0.1 )2Zr2O7 powder is refined by ball milling and then granulated by molding.
[0091] Step 3: After the granulated powder is loaded into the mold, it is cold isostatically pressed with a molding pressure of 250 MPa and a holding time of 10 minutes. Then, it is heated to 350°C in a high-temperature sintering furnace at a heating rate of 3°C / min, sintered for 30 minutes, and then heated to 1300°C at a heating rate of 10°C / min, sintered for 5 hours, and then processed to the target size (not exceeding 0.5mm dimensional positive tolerance) by a precision lathe, heated to 650°C at a heating rate of 5°C / min, sintered for 30 minutes, and then heated to 1650°C at a heating rate of 2°C / min and sintered for 6 hours to obtain (Gd 0.9 Yb 0.1 )2Zr2O7 target.
[0092] The coprecipitation method in step 1 is specifically:
[0093] Step 1-1: dissolving the reaction raw materials in concentrated nitric acid to prepare a 0.4 mol / L rare earth solution;
[0094] Step 1-2: adding the rare earth solution dropwise into ammonia water, controlling the pH value of the rare earth solution to 11, and obtaining a precursor precipitate after precipitation;
[0095] Step 1-3: filtering, washing and drying the precursor precipitate to obtain a precursor powder through sieving, with the drying temperature being 150° C. and the drying time being 30 h;
[0096] Step 1-4: The precursor powder is calcined at 900°C for 5 hours, and the calcined powder is ball-milled to obtain (Gd 0.9 Yb 0.1 )2Zr2O7 powder.
[0097] Example 5
[0098] Step 1: According to (Gd 0.9 Sm 0.1 )2Zr2O7 The reaction raw materials were weighed in a mass ratio of Gd2O3:Sm2O3:ZrO2 = 53.7:5.74:40.56, and the coprecipitation method was used to prepare (Gd 0.9 Sm 0.1 )2Zr2O7 powder.
[0099] Step 2: (Gd 0.9 Sm 0.1 )2Zr2O7 powder is refined by ball milling and then granulated by molding.
[0100] Step 3: After the granulated powder is loaded into the mold, it is cold isostatically pressed with a molding pressure of 250 MPa and a holding time of 10 minutes. Then, it is heated to 350°C in a high-temperature sintering furnace at a heating rate of 3°C / min, sintered for 30 minutes, and then heated to 1300°C at a heating rate of 10°C / min, sintered for 5 hours, and then processed to the target size (not exceeding 0.5mm dimensional positive tolerance) by a precision lathe, heated to 650°C at a heating rate of 5°C / min, sintered for 30 minutes, and then heated to 1650°C at a heating rate of 2°C / min and sintered for 6 hours to obtain (Gd 0.9 Sm 0.1 )2Zr2O7 target.
[0101] The coprecipitation method in step 1 is specifically:
[0102] Step 1-1: dissolving the reaction raw materials in concentrated nitric acid to prepare a 0.4 mol / L rare earth solution;
[0103] Step 1-2: adding the rare earth solution dropwise into ammonia water, controlling the pH value of the rare earth solution to 11, and obtaining a precursor precipitate after precipitation;
[0104] Step 1-3: filtering, washing and drying the precursor precipitate to obtain a precursor powder through sieving, with the drying temperature being 150° C. and the drying time being 30 h;
[0105] Step 1-4: The precursor powder is calcined at 900°C for 5 hours, and the calcined powder is ball-milled to obtain (Gd 0.9 Sm 0.1 )2Zr2O7 powder.
[0106] Example 6
[0107] X-ray diffraction analysis was used to characterize the phases of the gadolinium-praseodymium zirconate ceramic targets prepared in Examples 1, 2 and 3. The characterization results are shown in Figure 2 , Figure 3 and Figure 4 . Figure 2 1 is a schematic diagram of the phase structure of a gadolinium-praseodymium zirconate ceramic target prepared in Example 1 provided in the present application. Figure 3 1 is a schematic diagram of the physical structure of a gadolinium-praseodymium zirconate ceramic target prepared in Example 2 provided in the present application. Figure 4 This is a schematic diagram of the phase structure of a gadolinium-praseodymium zirconate ceramic target prepared in Example 3 provided in the examples of the present application. Figure 2 , Figure 3 and Figure 4 PDF#80-0417-Zr2Gd2O7 in represents the fluorite structure.
[0108] pass Figure 2 , Figure 3 and Figure 4 It can be seen that the physical structure of the gadolinium-praseodymium zirconate ceramic targets prepared in Examples 1, 2 and 3 of the present application is a fluorite structure.
[0109] Example 7
[0110] The gadolinium zirconate ceramic targets prepared in Examples 1, 2 and 3, and the (Gd 0.9 Yb 0.1 )2Zr2O7 and (Gd 0.9 Sm 0.1 )2Zr2O7 was characterized in terms of fracture toughness, thermal conductivity at 1200K and coefficient of thermal expansion.
[0111] The characterization operation of fracture toughness is as follows: obtain the gadolinium zirconate praseodymium ceramic targets prepared in Example 1, Example 2 and Example 3, and the (Gd 0.9 Yb 0.1 )2Zr2O7 and (Gd 0.9 Sm 0.1 )2Zr2O7 is taken as the test sample, the surface of the test sample is polished, and the fracture toughness test of the polished test sample is carried out by the indentation method, and the fracture toughness parameters of the test sample are calculated according to the test data.
[0112] The characterization operation of the thermal conductivity at 1200K is as follows: obtain the gadolinium zirconate ceramic targets prepared in Examples 1, 2 and 3, and the (Gd 0.9 Yb 0.1 )2Zr2O7 and (Gd 0.9 Sm 0.1 )2Zr2O7 is used as the sample to be tested, and the 1200K thermal conductivity of the sample to be tested is tested by the laser pulse method. The sample to be tested is placed on the thermal conductivity test equipment, and it is ensured that the thermal contact between the sample to be tested and the test equipment is good. The test temperature and heating conditions are set to ensure that the test is carried out at 1200K, and the test equipment is started to start heating the sample and record the temperature change during the heating process. According to the laser pulse method, the temperature gradient, heat flux density and other test data are measured and recorded, and the thermal conductivity value of the sample to be tested at 1200K is calculated based on the test data.
[0113] The characterization operation of the thermal expansion coefficient is as follows: obtain the gadolinium zirconate praseodymium ceramic targets prepared in Examples 1, 2 and 3, and the (Gd 0.9 Yb 0.1 )2Zr2O7 and (Gd 0.9 Sm0.1 )2Zr2O7 is taken as the sample to be tested, and the sample to be tested is placed on the test fixture of the thermal dilatometer, and it is ensured that the thermal contact between the sample to be tested and the thermal dilatometer is good. The sample to be tested is heated at a constant heating rate, and the length change of the sample to be tested at different temperatures is recorded. According to the obtained test data, the thermal expansion coefficient of the sample to be tested at different temperatures is calculated.
[0114] The gadolinium zirconate ceramic targets prepared in Examples 1, 2 and 3, and the (Gd 0.9 Yb 0.1 )2Zr2O7 and (Gd 0.9 Sm 0.1 The characterization results of the material properties of fracture toughness, thermal conductivity at 1200K and thermal expansion coefficient of 2Zr2O7 are shown in Table 1.
[0115] Table 1 Characterization results of target materials prepared in Examples 1 to 5
[0116]
[0117] As can be seen from Table 1, the gadolinium zirconate ceramic target prepared in Example 1 has a relative density of 60%, a fluorite structure, a thermal conductivity of 1200K material of 1.35W / m·K, and a thermal expansion coefficient of 10.9K. -1 , fracture toughness is 1.25MPa·m 1 / 2 , which can be used to prepare thermal barrier coatings by electron beam physical vapor deposition. The gadolinium zirconate praseodymium ceramic target prepared in Example 2 has a relative density of 73%, a phase structure of fluorite, a thermal conductivity of 1200K material of 1.20W / m·K, and a thermal expansion coefficient of 11.3K -1 , fracture toughness is 1.21MPa·m 1 / 2 The gadolinium-praseodymium zirconate ceramic target prepared in Example 3 has a relative density of 85%, a fluorite structure, a thermal conductivity of 1.12 W / m·K at 1200K, and a thermal expansion coefficient of 11.5K. -1 , fracture toughness is 1.17MPa·m 1 / 2 It can be seen that the gadolinium zirconate praseodymium ceramic target prepared in Example 3 has the lowest thermal conductivity, the highest thermal expansion coefficient, and the lowest fracture toughness, indicating that the gadolinium zirconate praseodymium ceramic target prepared in Example 3 has the best performance.
[0118] Example 4 Preparation of (Gd 0.9 Yb 0.1 )2Zr2O7, 1200K material thermal conductivity is 1.19W / m·K, thermal expansion coefficient is 11.1K -1 , fracture toughness is 1.22MPa·m 1 / 2Example 5 Preparation of (Gd 0.9 Sm 0.1 )2Zr2O7, 1200K material thermal conductivity is 1.29W / m·K, thermal expansion coefficient is 11.0K -1 , fracture toughness is 1.27MPa·m 1 / 2 .
[0119] It can be seen that doping Pr into gadolinium zirconate can effectively reduce the thermal conductivity of the material, increase the thermal expansion coefficient, and has little effect on the fracture toughness of the material. Compared with other rare earth (Yb, Sm) doped gadolinium zirconate, it has lower thermal conductivity and higher thermal expansion coefficient. Lower thermal conductivity is beneficial to improving the thermal cycling performance and high-temperature stability of aero-engine thermal barrier coatings, and higher thermal expansion coefficient is beneficial to the matching of thermal barrier coatings with the substrate, thereby improving the thermal cycling life of the coating.
[0120] The above is a detailed introduction to a gadolinium zirconate praseodymium ceramic target material, a preparation method and an application thereof provided by the present application. Specific examples are used herein to illustrate the principle and implementation method of the present application. The description of the above embodiments is only used to help understand the method and core idea of the present application. At the same time, for a person skilled in the art, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A method for preparing a gadolinium-praseodymium zirconate ceramic target, characterized in that: The method comprises the following steps: Step 1: According to the chemical formula (Gd 1-x Pr x )2Zr2O7 The element ratio in Gd2O3, ZrO2 and praseodymium oxide were weighed as reaction raw materials, and gadolinium zirconate praseodymium powder with the morphology of nanostructured agglomerates was synthesized by coprecipitation method, with a mass ratio of Gd2O3:Pr6O 11 : ZrO2=50.87:40.65:8.48, where x=0.15, and the powder particle size D50 is 15 microns; Step 2: The gadolinium praseodymium zirconate powder is refined by ball milling, and then granulated by molding to obtain granulated powder with an average particle size of 4 microns; Step 3: sequentially subjecting the granulated powder to cold isostatic pressing and first high-temperature sintering, and subjecting the blank after the first high-temperature sintering to a second high-temperature sintering after mechanical processing to obtain the gadolinium zirconate praseodymium ceramic target; the molding pressure of the cold isostatic pressing is 250 MPa, and the holding time is 10 min; The first high-temperature sintering is carried out by a gradient heating method, including: the high-temperature sintering under the gradient heating method is to heat to 350 °C at a heating rate of 3 °C / min in a high-temperature sintering furnace in an air or oxygen-enriched air atmosphere, and sinter for 30 min; then heat to 1300 °C at a heating rate of 10 °C / min, and sinter for 5 h; The second high temperature sintering is carried out by gradient heating method, including: The high temperature sintering under gradient temperature increase is to heat to 650 °C at a temperature increase rate of 5 °C / min in a high temperature sintering furnace in an air or oxygen-enriched air atmosphere, and sinter for 30 min; then heat to 1650 °C at a temperature increase rate of 2 °C / min, and sinter for 6 h; The thermal conductivity of the gadolinium zirconate praseodymium ceramic target prepared according to the above method at 1200 K is 1.12 W / m·K, and the thermal expansion coefficient is 11.5K -1 , fracture toughness is 1.17 MPa·m 1 / 2 .
2. The method for preparing the gadolinium-praseodymium zirconate ceramic target according to claim 1, characterized in that: In step 1, the gadolinium-praseodymium zirconate powder in the form of nanostructured aggregates is synthesized by the following steps: Step 1-1: dissolving the reaction raw materials in concentrated nitric acid to prepare a 0.4 mol / L rare earth solution; Step 1-2: adding the rare earth solution dropwise into ammonia water, controlling the pH value of the rare earth solution to 11, and obtaining a precursor precipitate after precipitation; Step 1-3: filtering, washing, and drying the precursor precipitate to obtain a precursor powder through sieving, with the drying temperature being 150 °C and the drying time being 30 h; Step 1-4: calcining the precursor powder at high temperature to generate the desired physical structure of gadolinium praseodymium zirconate. After ball milling the calcined powder, gadolinium praseodymium zirconate powder with the morphology of nanostructured agglomerates is obtained. The high-temperature calcination temperature is 900 ° C. and the time is 5 h. The desired physical structure of gadolinium praseodymium zirconate is a fluorite structure.
3. An application of a gadolinium-praseodymium zirconate ceramic target, characterized in that: The gadolinium-praseodymium zirconate ceramic target is used to prepare thermal barrier coatings for turbine blades of aircraft engines and gas turbines by electron beam physical vapor deposition. The chemical formula of gadolinium zirconate praseodymium in the gadolinium zirconate ceramic target is (Gd 1-x Pr x )2Zr2O7; wherein x=0.15, and the gadolinium-praseodymium zirconate ceramic target is prepared by the preparation method described in any one of claims 1-2.
Citation Information
Patent Citations
Dysprosium-doped gadolinium zirconate thermal barrier coating material and preparation method of coating
CN113373408A
Lanthanum-zirconium-praseodymium-oxygen thermal barrier coating material and preparation method thereof
CN115341174A
Gadolinium samarium zirconium praseodymium oxygen thermal barrier coating material and preparation method thereof
CN116676559A
A composite ceramic material having ultra high temperature stability in atmosphere and manufacturing method of the composite ceramic material
KR101722652B1
Thermal barrier coating with lower thermal conductivity