A manufacturing process for a silicon carbide substrate laser heat sink substrate

By using the laser heat sink substrate process of silicon carbide substrate, the problem of thermal management of semiconductor lasers is solved, the heat dissipation capacity and reliability are improved, and it can adapt to high temperature and high pressure environments.

CN118399190BActive Publication Date: 2024-10-15江苏富乐华功率半导体研究院有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410530899.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-29
Publication Date
2024-10-15
Estimated Expiration
2044-04-29

AI Technical Summary

Technical Problem

Thermal management of existing semiconductor lasers is difficult to effectively reduce heat accumulation, resulting in temperature rise and affecting efficiency and reliability, especially under high power and miniaturized packaging structures.

Method used

Laser heat sink substrate production process using silicon carbide (SiC) substrate, through magnetron sputtering, electroplating, mask photolithography and grinding and polishing processes to optimize thermal conductivity, bending strength and surface roughness, combined with electroplating nickel The gold layer and the magnetron sputtered gold-tin solder layer ensure the performance advantages of the SiC substrate.

Benefits of technology

It improves the heat dissipation capacity of the laser, extends the service life, improves efficiency and reliability, and adapts to the laser performance in high temperature and high pressure environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118399190B_ABST
    Figure CN118399190B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of semiconductor technology, and specifically to a manufacturing process for a silicon carbide substrate laser heat sink substrate. The manufacturing process comprises the following steps: magnetron sputtering → first pattern transfer process → second pattern transfer process → grinding and polishing → degumming and stripping → nickel-gold electroplating process → third pattern transfer process → sputtering gold-tin process → slicing and forming process. The manufacturing process adopts a semi-insulating silicon carbide substrate and a negative film process. Compared with the traditional method, this process does not need to sputter an insulating layer such as tantalum nitride or titanium nitride again to block the metal layer, while ensuring the high precision of the pattern; in addition, the verticality of its side wall can reach or exceed 88°, thereby ensuring the efficient transmission of heat conduction. Since silicon carbide has excellent thermal conductivity and strength, it exhibits good performance in a high-temperature and high-pressure laser working environment. The present invention can significantly improve the heat dissipation capacity of the laser heat sink and the life and performance of the laser.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductor technology, in particular to a manufacturing process of a silicon carbide substrate laser heat sink base plate. Background Art

[0002] With the rapid development of the microelectronics packaging industry, the output power requirements of semiconductor lasers are getting higher and higher, and the additional heat is also increasing. In addition, the miniaturization and integration of the laser packaging structure also hinder the conduction of heat, which puts higher requirements on the thermal management of laser packaging. At present, the epitaxial growth technology and chip manufacturing technology of lasers are relatively mature. The improvement of packaging methods has become the focus of improving the performance of lasers. Improving the heat dissipation capacity of lasers can reduce the accumulation of heat in the active area, reduce the temperature of the active area, improve efficiency, reduce the operating current, reduce the wavelength, and improve the spot output. Among them, the transition heat sink technology can effectively reduce the thermal resistance of the laser and improve the performance of the laser.

[0003] The main heat dissipation packaging methods for high-power semiconductor lasers include natural convection heat sink cooling, microchannel, electric refrigeration and spray cooling. Among them, for single-tube semiconductor lasers, natural convection heat sink cooling is easy to process and assemble, and is the most economical and commonly used cooling method. Generally, high thermal conductivity materials are used as heat sinks to expand the natural convection heat dissipation area to increase heat dissipation and reduce the temperature of the laser chip. In order to make the active area of ​​the laser chip closer to the heat sink and reduce the heat transfer path, the flip-chip packaging form is now commonly used, and the chip is attached to the heat sink through gold-tin solder. Adding a transition heat sink with high thermal conductivity and an expansion coefficient close to the thermal expansion coefficient of the chip between the chip and the secondary heat sink can greatly improve the service life, efficiency and reliability of the laser chip.

[0004] In order to overcome the defects of the prior art, the present invention provides a process for manufacturing a silicon carbide substrate laser heat sink base plate. Summary of the invention

[0005] The purpose of the present invention is to provide a process for manufacturing a silicon carbide substrate laser heat sink base plate to solve the problems in the prior art.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A process for manufacturing a silicon carbide substrate laser heat sink substrate comprises the following steps:

[0008] S1: Magnetron sputtering: The silicon carbide substrate is first cleaned and baked, and then the metal seed layer is magnetron sputtered;

[0009] S2: First pattern transfer process: electroplating the silicon carbide substrate obtained in S1 with bottom copper, and then performing first pattern mask exposure, development, and flash etching to form a circuit pattern;

[0010] S3: Second pattern transfer process: The silicon carbide substrate obtained in S2 is subjected to a secondary pattern mask process to expose the circuit pattern to be electroplated and thickened;

[0011] S4: Grinding and polishing process: The silicon carbide substrate obtained in S3 is first subjected to heat treatment and leveling, and then subjected to double-sided rough polishing and thinning, sandblasting, and double-sided fine polishing processes;

[0012] S5: debonding and stripping: immersing the silicon carbide substrate obtained in S4 in an N-methylpyrrolidone solution, and then stripping the film;

[0013] S6: Electroplating nickel-gold layer process: the silicon carbide substrate obtained in S5 is first sandblasted and electroplated with nickel-gold, and then electroplated with gold for thickening;

[0014] S7: The third pattern transfer process: the silicon carbide substrate obtained in S6 is subjected to pretreatment, vacuum lamination and exposure and development processes in sequence to obtain a silicon carbide substrate showing a gold-tin pattern;

[0015] S8: Sputtering gold-tin process: magnetron sputtering Pt and AuSn layers on the silicon carbide substrate obtained in S7, and then performing debonding and stripping;

[0016] S9: Slicing and forming process: Slicing and forming the silicon carbide substrate obtained in S8 to obtain a finished product.

[0017] More optimally, in step S1, cleaning includes ultrasonic alkaline acid cleaning and ultrasonic pure water cleaning; the conductivity of pure water is controlled at 1-10us / cm; the alkaline washing mass concentration is 5-10%, the temperature is 50-60°C, and sodium hydroxide is used for alkaline washing; the acid washing mass concentration is 2-5%, the temperature is 30-40°C, and sulfuric acid is used for acid washing; the ultrasonic cleaning frequency is 20-40KHz; after cleaning, high temperature baking is 100-120°C, and the baking time is 60-120min.

[0018] More optimally, in step S1, the magnetron sputtering process is a titanium-copper process, first sputtering a 100-150nm titanium layer, and then sputtering a 1-2μm copper layer; wherein the sputtering pressure is 0.3-0.35Pa, the sputtering temperature is 200-300°C, the sputtering current is 10-20A, the sputtering voltage is 500-800V, and the sputtering power is 10-25KW; the magnetron sputtering magnetic field is 300-1200GS; and the power output mode is a sinusoidal wave of 40KHz or 80KHz.

[0019] More optimally, the magnetron sputtering process is medium-frequency pulse current sputtering, and the current output mode is sinusoidal wave output; the copper layer is sputtered alternately by medium and high power on the double copper targets, the sputtering power of the copper target A is 17-20KW, and the sputtering power of the copper target B is 15-17KW. The former high-power coating ensures the coating thickness, and the latter medium-to-high power sputtering compensates and fills the copper layer deposition gaps in the micropores caused by the deposition of high-power sputtering copper particles, so that the film layer is thicker and has excellent bonding strength.

[0020] More optimally, in step S2, the first pattern transfer process includes electroplating base copper, film pre-treatment, film pressing, exposure and development, and flash etching to remove the film, and the process is a negative film process.

[0021] More optimally, in step S2, a 38 μm dry film is used for lamination, and exposure and development are performed after lamination; when electroplating the base copper, the base copper thickness is 3-5 μm, and the copper layer is deposited by direct current electroplating; the flash etching is acid etching, the copper etching solution is a sulfuric acid and sodium persulfate system, the titanium etching solution is a 5-8% hydrofluoric acid solution system, and the film stripping is an alkaline solution stripping; the pattern after etching retains the electroplated leads and the dry film is stripped, leaving the pattern to be thickened.

[0022] More optimally, in step S3, the second pattern transfer process includes film pre-treatment, film pressing, exposure and development, and thick copper electroplating.

[0023] More optimally, in step S3, the electroplating process steps are: degreasing → micro-etching → pickling → water washing → copper electroplating → water washing → drying.

[0024] More optimally, in step S3, the method of electroplating thick copper is a pulse electroplating process, and the pulse electroplating process has the following characteristics: temperature of 20-26°C, cathode current density of 1.5-2.5ASD, anode current density of 1-3ASD, and jet flow rate of 0.2-2L / Min / nozzle.

[0025] More optimally, in step S3, the copper electroplating solution of the pulse electroplating is an acidic copper sulfate solution electroplating system: copper sulfate pentahydrate is 200-260g / L; sulfuric acid is 40-90g / L; chloride ions are 40-70ppm; wetting agent is 8-15ml / L; copper plating brightener is 0.6-1.4ml / L; leveling agent is 25-35ml / L.

[0026] More optimally, in step S3, the formula for the coating thickness δ is δ=(K*J K *t*η) / ρ; K: electrochemical equivalent (g / C), J K :Cathode current density (A / dm 2 ), t: copper plating time (s), η: cathode current efficiency, ρ: density of plated metal; the formula for current density J is J = I / S, where the unit is A / dm 2, I: current size, S: plated area.

[0027] More optimally, in step S4, a polyurethane pad and a 3-5 μm abrasive are used for rough polishing and thinning, and the abrasive is prepared by aluminum oxide micropowder; 300-500 mesh corundum is used for sandblasting; and a black velvet pad and polishing liquid are used for fine polishing for 30-60 minutes, and the surface roughness is 30-50 nm.

[0028] More optimally, in step S5, the degumming and stripping includes soaking in N-methylpyrrolidone solution and film removal; the soaking in N-methylpyrrolidone solution is under ultrasonic conditions at a temperature of 80-110°C; the film removal is spraying N-methylpyrrolidone solution at 5-10MPa for 30-50s under the conditions of a temperature of 50-60°C and a rotation speed of 800-1000rpm; after completion, IPA spray rinsing and N2 purging are performed.

[0029] More optimally, in step S6, the nickel-gold electroplating process includes sandblasting, nickel-gold electroplating and gold electroplating thickening, the nickel layer thickness of the nickel-gold electroplating is 3-5 μm, and the gold electroplating is thickened to 1-1.5 μm.

[0030] More optimally, in step S7, the silicon carbide substrate obtained in step S6 is subjected to pre-film lamination treatment, vertical line cleaning, pickling, water washing, and drying.

[0031] More optimally, in step S7, vacuum lamination is performed by using a dry film with a thickness of 100-150 μm and a cutting size slightly smaller than the substrate by 1-2 mm. A vacuum laminator is used with a vacuum degree of 300-400 Pa, upper and lower layer temperatures of 75-80°C, a vacuum delay of 15-20 s, and a holding time of 20-30 s. A photolithography machine is then used in conjunction with a mask plate to perform photolithography patterning and development.

[0032] More optimally, in step S8, magnetron sputtering uses vacuum low-temperature eutectic sputtering with a vacuum pressure of 0.3-0.4 Pa and a temperature of 50-60°C; the magnetron sputtering process is plasma cleaning → sputtering Pt barrier layer → sputtering AuSn solder layer → sputtering Au protective layer. Since Sn metal is relatively active, pre-glow sputtering is required to remove the surface oxide layer before work.

[0033] More optimally, in step S8, the silicon carbide substrate after magnetron sputtering is immersed in N-methylpyrrolidone at 80-90° C. for 5-10 min, and then N-methylpyrrolidone, isopropanol and nitrogen are sprayed at 5-10 MPa for debonding and stripping.

[0034] More optimally, in step S9, the dicing process includes back-side UV film sticking, dicing, debonding and film expansion processes; a metal resin knife is used in the dicing process with a rotation speed of 25,000-30,000 rpm and a speed of 3-6 mm / s; after dicing, ultraviolet light is used to debond → blue film is inverted → film expansion is performed.

[0035] Beneficial effects of the present invention:

[0036] Compared with the conventional heat sink substrate manufacturing process, the present invention replaces the substrate with SiC, which is different from conventional metal heat sinks and ceramic heat sinks. SiC substrates have better thermal conductivity, bending strength and surface roughness. In order to ensure the verticality level within the unit, a double-sided polished SiC substrate is selected and combined with an electroplating thickening process. In surface treatment, a double-sided plane grinding and polishing method is adopted to meet the surface roughness requirements. The advantage of using pulse electroplating thickening in the second graphic process is to improve the coating structure, make the grains smaller, and obtain a denser coating; at the same time, reduce the porosity and internal stress of the coating. In the electroplating nickel-gold layer process, the electroplating nickel-gold has excellent bonding strength, the internal stress is small, and the coating crystallization is denser. The third graphic process adopts a vacuum film pressing process to avoid infiltration plating. Finally, the gold-tin solder layer is sputtered by magnetron sputtering. The order of these process steps helps to ensure that the performance advantages of the SiC substrate are fully utilized and improve the quality and reliability of the heat sink substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0038] Figure 1 is a process flow chart of the present invention;

[0039] Figure 2 is a schematic diagram of Example 1 of the present invention after the first pattern transfer process;

[0040] Figure 3 This is a finished product diagram of Example 1 of the present invention. DETAILED DESCRIPTION

[0041] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Source of raw materials:

[0043] Silicon carbide substrate, thickness 0.35mm, size 100.5×0.37mm, thermal conductivity >300W / (m·K).

[0044] Embodiment 1: S1: magnetron sputtering: the silicon carbide substrate is first cleaned and baked, and then the metal seed layer is magnetron sputtered; the cleaning includes ultrasonic alkaline acid cleaning and ultrasonic pure water cleaning; the conductivity of pure water is controlled at 5us / cm; the alkaline washing mass concentration is 6%, the temperature is 55°C, and sodium hydroxide is used for alkaline washing; the acid washing mass concentration is 3%, the temperature is 35°C, and sulfuric acid is used for acid washing; the ultrasonic cleaning frequency is 25KHz; after cleaning, it is baked at a high temperature of 100°C for 80 minutes;

[0045] The magnetron sputtering process is to first sputter a 110nm titanium layer and then sputter a 1.5μm copper layer; the sputtering pressure is 0.3Pa, the sputtering temperature is 230℃, the sputtering current is 15A, the sputtering voltage is 600V, and the sputtering power is 20KW; the magnetron sputtering magnetic field is 500GS; the power output mode is a sine wave of 80KHz;

[0046] S2: First pattern transfer process: electroplating the silicon carbide substrate obtained in S1 with base copper, then performing the first pattern mask exposure, development, and flash etching to form a circuit pattern; using a 38μm dry film for lamination, and then performing exposure and development after lamination; when electroplating the base copper, the base copper thickness is 4μm; the flash etching is acid etching, the copper etching solution is a sulfuric acid and sodium persulfate system, the titanium etching solution is a 7% hydrofluoric acid solution system, and the film stripping is an alkaline solution stripping; after etching, the pattern retains the electroplated leads and the dry film is stripped, leaving the pattern to be thickened;

[0047] S3: Second pattern transfer process: The silicon carbide substrate obtained in S2 is subjected to a secondary pattern mask process to expose the circuit pattern to be electroplated and thickened; the second pattern transfer process includes film pre-treatment, lamination, exposure and development, and thick copper electroplating; the secondary pattern transfer uses a 100μm dry film, and the Mark point recognition is used on the primary pattern for precise alignment to expose the secondary pattern; the electroplating process is as follows: degreasing → micro-etching → pickling → water washing → electroplating copper → water washing → drying; the copper layer is thickened by pulse electroplating, and pulse electroplating is performed in square wave form; the electroplating copper solution is prepared as an acidic copper sulfate solution electroplating system: copper sulfate pentahydrate is 230g / L; sulfuric acid is 50g / L; chloride ions are 50ppm; wetting agent is 12ml / L; copper plating brightener is 1ml / L; leveling agent is 30ml / L;

[0048] S4: Grinding and polishing process: The silicon carbide substrate obtained in S3 is first heat-treated and leveled, and then subjected to double-sided rough polishing, sandblasting, and double-sided fine polishing. The rough polishing uses a polyurethane pad and a 3μm abrasive with alumina micropowder. The sandblasting uses 300-mesh corundum. The fine polishing uses a black velvet pad and polishing liquid to polish the surface for 40 minutes, and the surface roughness is 30nm.

[0049] S5: debonding and stripping: soak the silicon carbide substrate obtained in S4 in N-methylpyrrolidone solution, and then remove the film; soaking in N-methylpyrrolidone solution is done under ultrasonic conditions, at 10MPa and 90°C for 5min; when removing the film, spray N-methylpyrrolidone solution at a temperature of 50°C and a rotation speed of 800rpm for 30s; after completion, perform IPA spray rinsing and N2 purging;

[0050] S6: Electroplating nickel-gold layer process: the silicon carbide substrate obtained in S5 is first sandblasted and electroplated with nickel-gold, and then electroplated with gold for thickening; the electroplating nickel-gold process includes electroplating nickel-gold and electroplating with gold for thickening, the thickness of the nickel layer of the electroplated nickel-gold is 3 μm, and the electroplated gold is thickened to 1 μm;

[0051] S7: The third pattern transfer process: the silicon carbide substrate obtained in S6 is subjected to film pre-treatment, vertical line cleaning, pickling, water washing, and drying; then a 100μm dry film is used for vacuum lamination and the cutting size is 1mm larger than the substrate, a vacuum laminator is used, the vacuum degree is 300Pa, the upper and lower layer temperatures are 77°C, the vacuum is delayed for 15s, and the pressure holding time is 20s; then a photolithography machine is used in conjunction with a mask plate to perform photolithography and development, and a silicon carbide substrate showing a gold-tin pattern is obtained;

[0052] S8: Sputtering gold-tin process: magnetron sputter Pt and AuSn layers on the silicon carbide substrate obtained in S7. The magnetron sputtering uses vacuum low-temperature eutectic sputtering with a vacuum pressure of 0.35 Pa and a temperature of 55°C. The magnetron sputtering process is plasma cleaning → sputtering Pt barrier layer → sputtering AuSn solder layer → sputtering Au protective layer. Since Sn metal is relatively active, pre-glow sputtering is required before work to remove the surface oxide layer. After completion, the silicon carbide substrate after magnetron sputtering is immersed in N-methylpyrrolidone at 10 MPa and 90°C for 7 minutes, and then sprayed with N-methylpyrrolidone, isopropyl alcohol, and nitrogen for debonding and stripping.

[0053] S9: Slicing and forming process: The silicon carbide substrate obtained in S8 is sliced ​​and formed. The slicing and forming process includes UV film sticking on the back, slicing, debonding and film expansion. A metal resin knife is used in the slicing process with a rotation speed of 28,000 rpm and a speed of 3 mm / s. After slicing, ultraviolet light is used to debond → blue film is inverted → film expansion is performed to prepare the finished product.

[0054] Comparative Example 1: The pulse plating process in S3: the second pattern transfer process step is changed to a DC plating process, and the rest is the same as Example 1, and the specific steps are as follows: S1: magnetron sputtering: the silicon carbide substrate is first cleaned and baked, and then the metal seed layer is magnetron sputtered; the cleaning includes ultrasonic alkaline acid cleaning and ultrasonic pure water cleaning; the conductivity of pure water is controlled at 5us / cm; the alkaline washing mass concentration is 6%, the temperature is 55°C, and sodium hydroxide is used for alkaline washing; the acid washing mass concentration is 3%, the temperature is 35°C, and sulfuric acid is used for acid washing; the ultrasonic cleaning frequency is 25KHz; after cleaning, it is baked at a high temperature of 100°C for 80min;

[0055] The magnetron sputtering process is to first sputter a 110nm titanium layer and then sputter a 1.5μm copper layer; the sputtering pressure is 0.3Pa, the sputtering temperature is 230℃, the sputtering current is 15A, the sputtering voltage is 600V, and the sputtering power is 20KW; the magnetron sputtering magnetic field is 500GS; the power output mode is a sine wave of 80KHz;

[0056] S2: First pattern transfer process: electroplating the silicon carbide substrate obtained in S1 with base copper, then performing the first pattern mask exposure, development, and flash etching to form a circuit pattern; using a 38μm dry film for lamination, and then performing exposure and development after lamination; when electroplating the base copper, the base copper thickness is 4μm; the flash etching is acid etching, the copper etching solution is a sulfuric acid and sodium persulfate system, the titanium etching solution is a 7% hydrofluoric acid solution system, and the film stripping is an alkaline solution stripping; after etching, the pattern retains the electroplated leads and the dry film is stripped, leaving the pattern to be thickened;

[0057] S3: Second pattern transfer process: The silicon carbide substrate obtained in S2 is subjected to a secondary pattern mask process to expose the circuit pattern to be electroplated and thickened; the second pattern transfer process includes film pre-treatment, lamination, exposure and development, and electroplating of thick copper; the secondary pattern transfer uses a 100μm dry film, and the Mark point recognition is used on the primary pattern for precise alignment to expose the secondary pattern; the electroplating process is as follows: degreasing → micro-etching → pickling → water washing → electroplating copper → water washing → drying; the copper layer is thickened by direct current electroplating; the electroplating copper solution is prepared as an acidic copper sulfate solution electroplating system: copper sulfate pentahydrate is 20g / L; the mass concentration of sulfuric acid is 10%; the chloride ion is 70ppm; the wetting agent is 8ml / L; the copper plating brightener is 0.07ml / L;

[0058] S4: Grinding and polishing process: The silicon carbide substrate obtained in S3 is first heat-treated and leveled, and then subjected to double-sided rough polishing, sandblasting, and double-sided fine polishing. The rough polishing uses a polyurethane pad and a 3μm abrasive with alumina micropowder. The sandblasting uses 300-mesh corundum. The fine polishing uses a black velvet pad and polishing liquid to polish the surface for 40 minutes, and the surface roughness is 30nm.

[0059] S5: debonding and stripping: soak the silicon carbide substrate obtained in S4 in N-methylpyrrolidone solution, and then remove the film; soaking in N-methylpyrrolidone solution is done under ultrasonic conditions, at 10MPa and 90°C for 5min; when removing the film, spray N-methylpyrrolidone solution at a temperature of 50°C and a rotation speed of 800rpm for 30s; after completion, perform IPA spray rinsing and N2 purging;

[0060] S6: Electroplating nickel-gold layer process: the silicon carbide substrate obtained in S5 is first sandblasted and electroplated with nickel-gold, and then electroplated with gold for thickening; the electroplating nickel-gold process includes electroplating nickel-gold and electroplating with gold for thickening, the thickness of the nickel layer of the electroplated nickel-gold is 3 μm, and the electroplated gold is thickened to 1 μm;

[0061] S7: The third pattern transfer process: the silicon carbide substrate obtained in S6 is subjected to film pre-treatment, vertical line cleaning, pickling, water washing, and drying; then a 100μm dry film is used for vacuum lamination and the cutting size is 1mm larger than the substrate, a vacuum laminator is used, the vacuum degree is 300Pa, the upper and lower layer temperatures are 77°C, the vacuum is delayed for 15s, and the pressure holding time is 20s; then a photolithography machine is used in conjunction with a mask plate to perform photolithography and development, and a silicon carbide substrate showing a gold-tin pattern is obtained;

[0062] S8: Sputtering gold-tin process: magnetron sputter Pt and AuSn layers on the silicon carbide substrate obtained in S7. The magnetron sputtering uses vacuum low-temperature eutectic sputtering with a vacuum pressure of 0.35 Pa and a temperature of 55°C. The magnetron sputtering process is plasma cleaning → sputtering Pt barrier layer → sputtering AuSn solder layer → sputtering Au protective layer. Since Sn metal is relatively active, pre-glow sputtering is required before work to remove the surface oxide layer. After completion, the silicon carbide substrate after magnetron sputtering is immersed in N-methylpyrrolidone at 10 MPa and 90°C for 7 minutes, and then sprayed with N-methylpyrrolidone, isopropyl alcohol, and nitrogen for debonding and stripping.

[0063] S9: Slicing and forming process: The silicon carbide substrate obtained in S8 is sliced ​​and formed. The slicing and forming process includes UV film sticking on the back, slicing, debonding and film expansion. A metal resin knife is used in the slicing process with a rotation speed of 28,000 rpm and a speed of 3 mm / s. After slicing, ultraviolet light is used to debond → blue film is inverted → film expansion is performed to prepare the finished product.

[0064] Comparative Example 2: S6: nickel-gold plating process is changed from electroplating to chemical plating, and the rest is the same as Example 1, and the specific steps are as follows: S1: magnetron sputtering: the silicon carbide substrate is first cleaned and baked, and then the metal seed layer is magnetron sputtered; the cleaning includes ultrasonic alkaline acid cleaning and ultrasonic pure water cleaning; the conductivity of pure water is controlled at 5us / cm; the alkaline washing mass concentration is 6%, the temperature is 55°C, and sodium hydroxide is used for alkaline washing; the acid washing mass concentration is 3%, the temperature is 35°C, and sulfuric acid is used for acid washing; the ultrasonic cleaning frequency is 25KHz; after cleaning, it is baked at a high temperature of 100°C for 80min;

[0065] The magnetron sputtering process is to first sputter a 110nm titanium layer and then sputter a 1.5μm copper layer; the sputtering pressure is 0.3Pa, the sputtering temperature is 230℃, the sputtering current is 15A, the sputtering voltage is 600V, and the sputtering power is 20KW; the magnetron sputtering magnetic field is 500GS; the power output mode is a sine wave of 80KHz;

[0066] S2: First pattern transfer process: electroplating the silicon carbide substrate obtained in S1 with base copper, then performing the first pattern mask exposure, development, and flash etching to form a circuit pattern; using a 38μm dry film for lamination, and then performing exposure and development after lamination; when electroplating the base copper, the base copper thickness is 4μm; the flash etching is acid etching, the copper etching solution is a sulfuric acid and sodium persulfate system, the titanium etching solution is a 7% hydrofluoric acid solution system, and the film stripping is an alkaline solution stripping; after etching, the pattern retains the electroplated leads and the dry film is stripped, leaving the pattern to be thickened;

[0067] S3: Second pattern transfer process: The silicon carbide substrate obtained in S2 is subjected to a secondary pattern mask process to expose the circuit pattern to be electroplated and thickened; the second pattern transfer process includes film pre-treatment, lamination, exposure and development, and thick copper electroplating; the secondary pattern transfer uses a 100μm dry film, and the Mark point recognition is used on the primary pattern for precise alignment to expose the secondary pattern; the electroplating process is as follows: degreasing → micro-etching → pickling → water washing → electroplating copper → water washing → drying; the copper layer is thickened by pulse electroplating, and pulse electroplating is performed in square wave form; the electroplating copper solution is prepared as an acidic copper sulfate solution electroplating system: copper sulfate pentahydrate is 230g / L; sulfuric acid is 50g / L; chloride ions are 50ppm; wetting agent is 12ml / L; copper plating brightener is 1ml / L; leveling agent is 30ml / L;

[0068] S4: Grinding and polishing process: The silicon carbide substrate obtained in S3 is first heat-treated and leveled, and then subjected to double-sided rough polishing, sandblasting, and double-sided fine polishing. The rough polishing uses a polyurethane pad and a 3μm abrasive with alumina micropowder. The sandblasting uses 300-mesh corundum. The fine polishing uses a black velvet pad and polishing liquid to polish the surface for 40 minutes, and the surface roughness is 30nm.

[0069] S5: debonding and stripping: soak the silicon carbide substrate obtained in S4 in N-methylpyrrolidone solution, and then remove the film; soaking in N-methylpyrrolidone solution is done under ultrasonic conditions, at 10MPa and 90°C for 5min; when removing the film, spray N-methylpyrrolidone solution at a temperature of 50°C and a rotation speed of 800rpm for 30s; after completion, perform IPA spray rinsing and N2 purging;

[0070] S6: Chemical nickel-gold plating process: the silicon carbide substrate obtained in S5 is first sandblasted and chemically nickel-gold plated, and then electroplated with gold for thickening; the electroplated nickel-gold process includes electroplating nickel-gold and electroplating with gold for thickening, the thickness of the nickel layer of the electroplated nickel-gold is 3 μm, and the electroplated gold is thickened to 1 μm;

[0071] S7: The third pattern transfer process: the silicon carbide substrate obtained in S6 is subjected to film pre-treatment, vertical line cleaning, pickling, water washing, and drying; then a 100μm dry film is used for vacuum lamination and the cutting size is 1mm larger than the substrate, a vacuum laminator is used, the vacuum degree is 300Pa, the upper and lower layer temperatures are 77°C, the vacuum is delayed for 15s, and the pressure holding time is 20s; then a photolithography machine is used in conjunction with a mask plate to perform photolithography and development, and a silicon carbide substrate showing a gold-tin pattern is obtained;

[0072] S8: Sputtering gold-tin process: magnetron sputter Pt and AuSn layers on the silicon carbide substrate obtained in S7. The magnetron sputtering uses vacuum low-temperature eutectic sputtering with a vacuum pressure of 0.35 Pa and a temperature of 55°C. The magnetron sputtering process is plasma cleaning → sputtering Pt barrier layer → sputtering AuSn solder layer → sputtering Au protective layer. Since Sn metal is relatively active, pre-glow sputtering is required before work to remove the surface oxide layer. After completion, the silicon carbide substrate after magnetron sputtering is immersed in N-methylpyrrolidone at 10 MPa and 90°C for 7 minutes, and then sprayed with N-methylpyrrolidone, isopropyl alcohol, and nitrogen for debonding and stripping.

[0073] S9: Slicing and forming process: The silicon carbide substrate obtained in S8 is sliced ​​and formed. The slicing and forming process includes UV film sticking on the back, slicing, debonding and film expansion. A metal resin knife is used in the slicing process with a rotation speed of 28,000 rpm and a speed of 3 mm / s. After slicing, ultraviolet light is used to debond → blue film is inverted → film expansion is performed to prepare the finished product.

[0074] Detection test:

[0075] Thermal shock test: The finished product prepared by the present invention is placed on a heating platform and maintained at 350°C for 5 minutes to observe whether it has blistering or other poor bonding phenomena. The results are shown in the following table:

[0076]

[0077]

[0078] Conclusion: The present invention discloses a manufacturing process for a silicon carbide substrate laser heat sink substrate. The process design is reasonable. The SiC wafer is manufactured through magnetron sputtering, electroplating, mask lithography, grinding and polishing, etc. It has excellent roughness, verticality, appearance and yield rate, and has high practicality. Encapsulation in the laser will greatly improve the life and efficiency of the laser, and it also shows good performance in dealing with the high temperature and high pressure under the operation of the laser.

[0079] After testing in Example 1, the copper thickness, roughness, and gold-tin sputtering effect of the process all met the requirements.

[0080] Comparative Example 1: The pulse plating process in S3: the second pattern transfer process step is changed to a DC plating process, and the rest is the same as Example 1. After comparative analysis, the copper thickness under this process is abnormal, and there are many abnormalities in uniformity, resulting in poor grinding and polishing effects, and the specified roughness cannot be achieved as required.

[0081] Comparative Example 2: S6: The nickel-gold plating process is changed from electroplating to chemical plating, and the rest is the same as Example 1. After comparative testing, this process has the problems of low power of the overall heat sink and poor gold-tin melting effect.

[0082] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0083] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A process for manufacturing a silicon carbide substrate laser heat sink substrate, characterized in that: The following steps are involved: S1: Magnetron sputtering: The silicon carbide substrate is first cleaned and baked, and then the metal seed layer is magnetron sputtered; S2: First pattern transfer process: electroplating the silicon carbide substrate obtained in S1 with bottom copper, and then performing first pattern mask exposure, development, and flash etching to form a circuit pattern; S3: Second pattern transfer process: The silicon carbide substrate obtained in S2 is subjected to a secondary pattern mask process to expose the circuit pattern to be electroplated and thickened; The second pattern transfer process includes film pre-treatment, lamination, exposure and development, and thick copper electroplating; the thickening is carried out by pulse electroplating; S4: Grinding and polishing process: The silicon carbide substrate obtained in S3 is first subjected to heat treatment and leveling, and then subjected to double-sided rough polishing and thinning, sandblasting, and double-sided fine polishing processes; S5: debonding and stripping: immersing the silicon carbide substrate obtained in S4 in an N-methylpyrrolidone solution, and then stripping the film; S6: Electroplating nickel-gold layer process: the silicon carbide substrate obtained in S5 is first sandblasted and electroplated with nickel-gold, and then electroplated with gold for thickening; S7: The third pattern transfer process: the silicon carbide substrate obtained in S6 is subjected to pretreatment, vacuum lamination and exposure and development processes in sequence to obtain a silicon carbide substrate showing a gold-tin pattern; S8: Sputtering gold-tin process: magnetron sputtering Pt and AuSn layers on the silicon carbide substrate obtained in S7, and then performing debonding and stripping; S9: Slicing and forming process: Slicing and forming the silicon carbide substrate obtained in S8 to obtain a finished product.

2. The process for manufacturing a silicon carbide laser heat sink substrate according to claim 1, characterized in that: In step S1, cleaning includes ultrasonic alkaline acid cleaning and ultrasonic pure water cleaning; the conductivity of pure water is controlled at 1-10us / cm; the alkaline cleaning mass concentration is 5-10%, the temperature is 50-60°C, and sodium hydroxide is used for alkaline cleaning; the acid cleaning mass concentration is 2-5%, the temperature is 30-40°C, and sulfuric acid is used for acid cleaning; the ultrasonic cleaning frequency is 20-40KHz; after cleaning, the high temperature baking is 100-120°C, and the baking time is 60-120min.

3. The process for manufacturing a silicon carbide laser heat sink substrate according to claim 1, characterized in that: In step S1, the magnetron sputtering process is a titanium-copper process, first sputtering a 100-150nm titanium layer, and then sputtering a 1-2μm copper layer; the sputtering pressure is 0.3-0.35Pa, the sputtering temperature is 200-250℃, the sputtering current is 10-20A, the sputtering voltage is 500-800V, and the sputtering power is 10-25KW; the magnetron sputtering magnetic field is 300-1200GS; the power output mode is a sinusoidal wave of 40KHz or 80KHz.

4. The process for manufacturing a silicon carbide laser heat sink substrate according to claim 1, characterized in that: In step S2, a 38 μm dry film is used for lamination, and exposure and development are performed after lamination; when electroplating the base copper, the base copper thickness is 3-5 μm; the flash etching is acid etching, the copper etching solution is a sulfuric acid and sodium persulfate system, the titanium etching solution is a 5-8% hydrofluoric acid solution system, and the film stripping is an alkaline solution stripping; the pattern after etching retains the electroplated leads and the dry film is stripped, leaving the pattern to be thickened.

5. The process for manufacturing a silicon carbide laser heat sink substrate according to claim 1, characterized in that: In step S4, a polyurethane pad and a 3-5 μm abrasive are used for rough polishing and thinning; 300-500 mesh corundum is used for sand blasting; and a black velvet pad and polishing liquid are used for fine polishing to polish the surface.

6. The process for manufacturing a silicon carbide laser heat sink substrate according to claim 1, characterized in that: In step S6, the nickel-gold electroplating process includes nickel-gold electroplating and gold-thickening electroplating, the nickel layer thickness of the nickel-gold electroplating is 3-5 μm, and the gold-thickening electroplating is 1-1.5 μm.

7. The process for manufacturing a silicon carbide laser heat sink substrate according to claim 1, characterized in that: In step S7, vacuum lamination, exposure and development are performed by using a 100-150 μm dry film.

8. The process for manufacturing a silicon carbide laser heat sink substrate according to claim 1, characterized in that: In step S8, the silicon carbide substrate after magnetron sputtering is immersed in N-methylpyrrolidone at 80-90°C for 5-10 minutes, and then N-methylpyrrolidone, isopropyl alcohol and nitrogen are sprayed at 5-10 MPa for debonding and peeling.

9. The process for manufacturing a silicon carbide laser heat sink substrate according to claim 1, characterized in that: In step S9, the dicing process includes back-side UV film application, dicing, debonding and film expansion processes; a metal resin knife is used in the dicing process, with a rotation speed of 25,000-30,000 rpm and a speed of 3-6 mm / s.