A PA6 material and preparation method thereof
By combining recycled PA6 with epoxy chain extender, mineral oil and amino-terminated hyperbranched polyamide, and performing multi-stage vacuum melt extrusion at high temperature, the problems of low viscosity of PA6 material and high caprolactam residue are solved, and high efficiency is achieved. The production process and high-quality PA6 material preparation.
Patent Information
- Application Number
- CN202410874199.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-02
Smart Images

Figure CN118406370B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of PA6 recycling, and in particular to a PA6 material and a preparation method thereof. Background Art
[0002] Nylon 6, also known as PA6 and polyamide 6, is a polymer compound. The monomer of nylon 6 is caprolactam, which is a polymer compound formed by the polymerization of caprolactam. It has excellent wear resistance and self-lubrication, high mechanical strength, good heat resistance and electrical insulation, excellent low temperature performance, self-extinguishing and good chemical resistance, especially excellent oil resistance. PA6 can be used in fiber, automobile, electronic appliances and other fields. The viscosity of PA6 has a significant impact on physical and mechanical properties. The secondary brand or unqualified products of PA6 industrial production cannot be used due to low viscosity and excessive caprolactam residue, resulting in waste and environmental pollution. The fishing nets and other silk recycled on the market have low viscosity, which makes them unable to be directly recycled.
[0003] At present, the main way to thicken PA6 industrially is to use solid-state thickening in a reactor, which has the problems of complex process and long reaction time. At the same time, there are some processes that use reactive extrusion thickening, but do not take into account the problem of caprolactam residues with certain toxicity. The recycled PA6 raw material has a high caprolactam content and low viscosity. When the commonly used twin-screw extrusion thickening is used in the prior art, the shorter screw aspect ratio, low processing temperature, no vacuum or only conventional single-stage vacuum and other processes make it difficult to remove a certain amount of residual caprolactam and obtain thickened PA6 at the same time; currently, 8-16 hours of hot water extraction are usually used in industrial production to remove residual caprolactam. This method not only wastes time, but also wastes a lot of water and energy; and although the use of reactor solid-phase thickening can reduce the amount of caprolactam residue, the process and process are relatively complex, and the reaction cycle is very long 8-24 hours, resulting in low production efficiency. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a PA6 material and a preparation method thereof which has the advantages of simple process and technology, less time consumption, reduced caprolactam residue, increased PA6 viscosity, excellent mechanical properties, etc.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] In a first aspect, the present invention provides a PA6 material comprising the following components in parts by weight:
[0007] 90~100 parts of recycled PA6, 0.3~3 parts of chain extender, 0.1~2 parts of lubricant and 0.1~1 parts of antioxidant;
[0008] The chain extender is an epoxy chain extender; the lubricant is mineral oil (white mineral oil) and / or amino-terminated hyperbranched polyamide.
[0009] The PA6 material of the present invention uses recycled PA6 as the main raw material, and is combined with an epoxy chain extender, a specific lubricant and an antioxidant to reduce the caprolactam content in the recycled PA6 while effectively increasing its relative viscosity, thereby obtaining a PA6 material with high viscosity and low caprolactam residue.
[0010] Preferably, the chain extender is an epoxy chain extender containing 9 to 12 epoxy functional groups.
[0011] Preferably, the mineral oil has a viscosity of 32-100 cts and an open flash point of 220-320°C.
[0012] Preferably, the lubricant is composed of mineral oil and amino-terminated hyperbranched polyamide in a mass ratio of 1:(0.5-5); optionally, the mass ratio of the mineral oil to amino-terminated hyperbranched polyamide can be 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, or 1:4.5.
[0013] When the lubricant is composed of mineral oil and amino-terminated hyperbranched polyamide, it can not only make the chain extender evenly adhere to the recycled material (recycled PA6) particles, while playing a lubricating and dispersing role, but the amino-terminated hyperbranched polyamide can also participate in the chain extension reaction to achieve self-plasticization and self-lubrication, thereby improving the processing performance.
[0014] Preferably, the mineral oil is paraffin oil, which makes the chain extender adhere evenly to the recycled material particles and also plays a certain lubricating and dispersing effect. Unexpectedly, it was found that when the amino-terminated hyperbranched polyamide was compounded with mineral oil as a lubricant component, the overall performance of the PA6 material was the best.
[0015] Further preferably, the antioxidant is one or more of a hindered phenol antioxidant and a phosphite antioxidant; more preferably, the antioxidant is a hindered phenol antioxidant and a phosphite antioxidant in a mass ratio of 1:(1-4).
[0016] In a second aspect, the present invention provides a method for preparing the above-mentioned PA6 material, comprising the following steps:
[0017] The recycled PA6, chain extender, lubricant and antioxidant are mixed and melt-extruded at 250-280°C to obtain the PA6 material.
[0018] The reaction time in the entire preparation process is 1 to 3 minutes, which effectively solves the defects of the existing preparation methods such as complex preparation process (more than 3 steps) and long viscosity increase time (8 to 24 hours).
[0019] The temperature of melt extrusion is a very important condition. A higher temperature can speed up the reaction extrusion rate, provide a low viscosity system, and facilitate the removal of small molecules such as caprolactam and water. However, too high a temperature will cause the chain extension reaction to be too fast, resulting in poor removal of small molecules such as caprolactam, and will also cause PA6 to degrade. Studies have found that the appropriate temperature range for melt extrusion is 250~280℃.
[0020] Preferably, an extruder is used for melt extrusion, and the screw aspect ratio of the extruder is (44-64): 1. When the screw aspect ratio of the extruder is within the above range, it can take into account the removal of low molecular weight substances, ensure as complete a reaction as possible, and ensure production timeliness.
[0021] Preferably, the melt extrusion is carried out under at least two levels of vacuum, and the vacuum degree of each level is -0.06~-0.1MPa.
[0022] Further preferably, during industrial production, secondary brand products usually contain more unremoved caprolactam, and multi-stage vacuum can make the caprolactam removal more complete. The vacuum quantity can be adjusted accordingly according to the residual caprolactam content in the raw material: when the mass content of caprolactam in the recovered PA6 is 1-20%, the melt extrusion is carried out under three-stage vacuum; when the mass content of caprolactam in the recovered PA6 is 0.6-1%, the melt extrusion is carried out under two-stage vacuum.
[0023] Preferably, the vacuum section of the extruder adopts a conveying block screw element, and the pitch of the conveying block screw element is 1.5 to 2 times the screw diameter of the extruder. The above conveying block screw element can provide a low filling degree, has good interface renewal, and can promote the removal of small molecules such as caprolactam and moisture.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The PA6 material of the present invention uses recycled PA6 as the main raw material, and is combined with an epoxy chain extender, a specific lubricant and an antioxidant to reduce the caprolactam content in the recycled PA6 while effectively increasing its relative viscosity, thereby obtaining a PA6 material with high viscosity and low caprolactam residue, thereby realizing the recycling of PA6.
[0026] Compared with the current industrial production method of removing caprolactam by hot water extraction, the preparation method of the present invention can improve production efficiency while effectively reducing water and energy waste; compared with the traditional twin-screw reactive extrusion viscosity enhancement, it not only expands the selection range of recycled PA, but also produces products with better quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1Schematic diagram of an extruder with an aspect ratio of L / D=44 in Example 4;
[0028] Figure 2 Schematic diagram of the extruder with aspect ratio L / D=64 in Example 1. DETAILED DESCRIPTION
[0029] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0030] In the following examples, the ingredients used are specifically as follows:
[0031] PA6 recycled material:
[0032] PA6 recycled material 1: relative viscosity 0.7, caprolactam residual content 9.0%;
[0033] PA6 recycled material 2: PA6 recycled material 1 was pretreated before use, i.e., hot water extraction for a certain period of time and then dried; after the treatment, PA6 recycled material 2 with a caprolactam residual content of 1 wt% was obtained.
[0034] Chain Extender:
[0035] Epoxy chain extender: The manufacturer is Nanjing Baitong New Materials Co., Ltd., brand name is BTCE-9013;
[0036] Heterocyclic chain extender: Dalian Research Institute of Chemical Industry, 1,3-bis(2-oxazoline)benzene (MPBO).
[0037] Lubricant:
[0038] Amino-terminated hyperbranched polyamide: Wuhan Hyperbranched Resin Technology Co., Ltd., brand name HyPer N10;
[0039] Mineral oil: No. 68 white oil.
[0040] Unless otherwise specified, other materials, reagents, etc. used in the examples can be obtained from commercial sources.
[0041] Example 1
[0042] A PA6 material comprises the following components in parts by weight: 97.6 parts of PA6 recycled material 1, 1 part of chain extender BCTE9013, 0.2 parts of No. 68 white oil, 0.8 parts of amino-terminated hyperbranched polyamide, 0.2 parts of antioxidant 168, and 0.2 parts of antioxidant 1010.
[0043] The preparation method of the above PA6 material comprises the following steps:
[0044] The above components were put into an extruder for melt extrusion for 2 minutes to obtain the PA6 material. The temperature (°C) of the extruder was set as:
[0045] 180 / 240 / 250 / 270 / 270 / 270 / 270 / 270 / 270 / 270 / 270 / 270 / 270 / 270 / 270 / 270 / 270 / 270; such as Figure 2 As shown, the screw length-to-diameter ratio of the extruder is L / D=64:1; three-stage vacuum is selected in the extruder, and the pitch of the screw element in the vacuum section is 2D (D is the screw diameter of the extruder).
[0046] Example 2
[0047] A PA6 material comprises the following components in parts by weight: 97.6 parts of PA6 recycled material 1, 1 part of chain extender BCTE9013, 1 part of No. 68 white oil, 0.2 parts of antioxidant 168, and 0.2 parts of antioxidant 1010.
[0048] The preparation method of the above PA6 material is the same as that in Example 1.
[0049] Example 3
[0050] A PA6 material comprises the following components in parts by weight: 97.6 parts of PA6 recycled material 1, 1 part of chain extender BCTE9013, 1 part of amino-terminated hyperbranched polyamide, 0.2 parts of antioxidant 168, and 0.2 parts of antioxidant 1010.
[0051] The preparation method of the above PA6 material is the same as that in Example 1.
[0052] Example 4
[0053] A PA6 material comprises the following components in parts by weight: 98.5 parts of PA6 recycled material 2, 0.5 parts of chain extender BCTE9013, 0.2 parts of No. 68 white oil, 0.4 parts of amino-terminated hyperbranched polyamide, 0.2 parts of antioxidant 168, and 0.2 parts of antioxidant 1010.
[0054] The preparation method of the above PA6 material comprises the following steps:
[0055] The above components were placed in an extruder for melting and homogenization for 3 minutes to obtain the PA6 material. The temperature (°C) of the extruder was set to: 180 / 240 / 250 / 270 / 270 / 270 / 270 / 270 / 270 / 270 / 270; Figure 1 As shown, the screw length-to-diameter ratio of the extruder is L / D=44:1; the extruder uses a second-level vacuum; and the pitch of the screw element in the vacuum section is 1.5D.
[0056] Example 5
[0057] The difference between Example 5 and Example 1 is that the temperatures (° C.) of the extruder of Example 5 are set to: 180 / 240 / 240 / 240 / 240 / 240 / 240 / 240 / 240 / 240 / 240 / 240 / 240 / 240 / 240 / 240 / 240.
[0058] Example 6
[0059] The difference between Example 6 and Example 1 is that the temperatures (° C.) of the extruder of Example 6 are set to: 180 / 240 / 300 / 300 / 300 / 300 / 300 / 300 / 300 / 300 / 300 / 300 / 300 / 300 / 300 / 300.
[0060] Example 7
[0061] The difference between Example 7 and Example 1 is that the screw length-to-diameter ratio L / D of the extruder of Example 7 is 32:1.
[0062] Example 8
[0063] The difference between Example 8 and Example 1 is that the vacuum level of Example 8 is 1.
[0064] Example 9
[0065] The difference between Example 9 and Example 1 is that the pitch of the vacuum section thread element of Example 9 is 1D.
[0066] Comparative Example 1
[0067] The difference between Comparative Example 1 and Example 1 is that: Comparative Example 1 uses 1 part of heterocyclic chain extender to replace the chain extender BCTE9013.
[0068] Comparative Example 2
[0069] The difference between Comparative Example 2 and Example 1 is that no lubricant component is added in Comparative Example 2.
[0070] Comparative Example 3
[0071] The difference between Comparative Example 3 and Example 1 is that Comparative Example 3 uses 1 part of liquid paraffin as the lubricant component.
[0072] The performance tests were performed on the PA6 materials prepared in the above Examples 1 to 9 and Comparative Examples 1 to 3.
[0073] The specific test method is as follows:
[0074] Relative viscosity: According to GB / T 12006.1-2009 standard, using Ubbelohde viscometer, the solvent is 96% by mass sulfuric acid, and the concentration of polyamide solution is 0.005g / ml.
[0075] Caprolactam Residue: Caprolactam residue is tested using gas chromatography.
[0076] Mechanical properties test: Tensile strength is tested at 23°C according to GB / T 1040.2-2022; Flexural properties are tested at 23°C according to GB T 9341-2008.
[0077] Table 1 Test results of each group of materials
[0078]
[0079] The present invention example 1 and comparative examples 1 to 3 verify that the selection of specific types of chain extenders and lubricants in the PA6 material formula of the present invention can effectively improve the viscosity and mechanical properties of the PA6 material and reduce the residual amount of caprolactam. At the same time, the comparison between examples 1 to 3 shows that the example 1, which uses amino-terminated hyperbranched polyamide and mineral oil as the lubricant component, has the best recovery performance.
[0080] Comparison between Examples 1 and 4 shows that the present invention is not only applicable to recycled materials with low caprolactam content, but also to recycled materials with high caprolactam content.
[0081] Comparison between Examples 1 and 5 to 9 shows that the extrusion temperature of the present invention is 250 to 280°C, the screw aspect ratio L / D=36, 2 to 3 levels of vacuum are used, and the lead of the screw element in the vacuum section of the extruder is (1.5 to 2) D. At the same time, when the extruder with a long aspect ratio adopts a high speed process, a reasonable residence time required for the extrusion reaction can be guaranteed, thereby increasing the output per unit time.
[0082] Compared with the existing scheme, the present invention has only one reaction step of extrusion, the steps are simple, and the reaction time is only 1 to 3 minutes, which greatly improves the production efficiency and gives the PA6 material excellent regeneration performance.
[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A PA6 material, characterized in that: The invention comprises the following components in parts by weight: 90 to 100 parts of recycled PA6, 0.3 to 3 parts of a chain extender, 0.1 to 2 parts of a lubricant and 0.1 to 1 parts of an antioxidant; the chain extender is an epoxy chain extender containing 9 to 12 epoxy functional groups; the lubricant is composed of mineral oil and amino-terminated hyperbranched polyamide in a mass ratio of 1:(0.5 to 5).
2. The PA6 material according to claim 1, characterized in that The mineral oil has a viscosity of 32-100 cts and an open flash point of 220-320°C.
3. The PA6 material according to claim 1 or 2, characterized in that: The antioxidant is one or more of a hindered phenol antioxidant and a phosphite antioxidant.
4. The method for preparing the PA6 material according to any one of claims 1 to 3, characterized in that: The following steps are involved: The recycled PA6, chain extender, lubricant and antioxidant are mixed and melt-extruded at 250-280°C to obtain the PA6 material.
5. The method for preparing the PA6 material according to claim 4, characterized in that: An extruder is used for melt extrusion, and the aspect ratio of the screw of the extruder is (44-64):
1.
6. The method for preparing the PA6 material according to claim 5, characterized in that: The melt extrusion is carried out under at least two levels of vacuum, and the vacuum degree of each level is -0.06~-0.1MPa.
7. The method for preparing the PA6 material according to claim 6, characterized in that: When the mass content of caprolactam in the recovered PA6 is 1-20%, the melt extrusion is performed under three-stage vacuum; when the mass content of caprolactam in the recovered PA6 is 0.6-1%, the melt extrusion is performed under two-stage vacuum.
8. The method for preparing the PA6 material according to claim 7, characterized in that: The vacuum section of the extruder adopts a conveying block thread element, and the pitch of the conveying block thread element is 1.5 to 2 times the diameter of the screw of the extruder.