A method for preparing wear-resistant self-lubricating coating for inner hole of aircraft landing gear

Through hollow cathode discharge plasma-assisted chemical vapor deposition technology, the equipment limitation and high temperature problems of wear-resistant self-lubricating coating on the inner surface of the aircraft landing gear are solved, and an efficient and environmentally friendly wear-resistant coating is achieved to ensure landing gear strength and reduce subsequent results Processing risks.

CN118407020BActive Publication Date: 2024-11-15CHENGDU ZHONGYUN CENTURY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410874730.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-15
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

The prior art has many shortcomings in the wear-resistant self-lubricating coating on the surface of aircraft landing gear, including the toxicity of electroplating hard chromium, the equipment limitation of supersonic flame spraying tungsten carbide, and the difficulty of uniform deposition in the inner holes in physical vapor deposition. Moreover, high temperature during processing will affect the strength of the landing gear.

Method used

The plasma-assisted chemical vapor deposition technology is used to generate hollow cathode discharge, which improves the film binding force through in-situ nitriding process and reduces the deposition temperature to achieve a one-step inner surface coating to avoid the impact on the landing gear strength.

Benefits of technology

An efficient and environmentally friendly wear-resistant self-lubricating coating is achieved, with increased film bonding force and low deposition temperature, which does not affect the strength of the landing gear, avoids breathing and liquid leakage problems, and does not require further processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118407020B_ABST
    Figure CN118407020B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear, the steps of which include: grinding and polishing the inner surface of the landing gear until the roughness reaches a preset standard, then removing oil and cleaning; placing the landing gear in a vacuum device, connecting the landing gear to the negative electrode of a power supply, connecting the vacuum chamber to the positive electrode of a power supply, and evacuating to 5.0×10 ‑3 Pa or less; introduce argon gas to perform argon plasma cleaning on the inner surface of the landing gear; after the argon plasma cleaning is completed, gradually introduce a mixed gas of nitrogen and hydrogen or ammonia to nitride the inner surface of the landing gear; gradually introduce a carbon-containing gas source, adjust the bias voltage and the gas flow rate of each gas to perform carbonitriding treatment and amorphous carbon film deposition; gradually reduce until the nitrogen-containing gas source flow rate is closed, maintain the inner hole hollow cathode discharge to deposit the carbon film, and take it out of the furnace after the coating is completed. It can achieve inner surface coating in one step, and the combination of infiltration and deposition can greatly improve the bonding strength of the film layer. The deposition temperature is low and will not affect the strength of the landing gear.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aviation manufacturing, and in particular relates to a method for preparing a wear-resistant self-lubricating coating for an inner hole of an aircraft landing gear. Background Art

[0002] Aircraft landing gear is a core component of aircraft and is directly related to the safety of aircraft service. The inner surface of the outer tube of the aircraft landing gear needs to withstand harsh friction environment during service, so its surface needs to be treated for wear resistance. The material of aircraft landing gear is mainly high-strength steel, and the landing gear material of some small drones is aluminum alloy. At present, the surface of high-strength steel is mainly treated with electroplating hard chrome, and aluminum alloy is treated with hard anodizing. Electroplating hard chrome and hard anodizing will bring the risk of leakage and panting, which will have an adverse effect on the normal service of the aircraft. Electroplating hard chrome uses hexavalent chromium as raw material. Hexavalent chromium is a strong carcinogen. Chromium mist will be generated during the electroplating process, which will seriously damage the operator's body. In addition, its wastewater treatment is more difficult and may cause greater pollution to the water body.

[0003] At present, the industry has also conducted a lot of research and application attempts on the wear-resistant protective coating on the inner surface of the outer tube of the landing gear, including supersonic flame spraying of tungsten carbide, physical vapor deposition hard coating, chemical vapor deposition hard coating, etc. Supersonic flame spraying of tungsten carbide is difficult to achieve inner hole spraying due to equipment limitations. After spraying, secondary processing such as grinding and polishing is required. The processing is difficult, and the high temperature during the processing will affect the tensile strength and fatigue strength of the landing gear. Physical vapor deposition technology is a green and environmentally friendly surface treatment technology that can deposit high-performance wear-resistant hard film layers, but due to the principles of this technology, physical vapor deposition is difficult to uniformly deposit film layers on inner holes or complex landing gear surfaces. Chemical vapor deposition can also obtain high-performance hard films, but the deposition temperature is too high and the film layer has poor bonding strength. Therefore, the industry is still researching the next generation of wear-resistant self-lubricating coatings for aircraft landing gear.

[0004] The present invention adopts hollow cathode discharge to generate plasma to assist chemical vapor deposition, on the one hand, through in-situ nitriding

[0005] The process increases the bonding strength of the film layer. On the other hand, the deposition temperature is reduced by plasma-assisted chemical vapor deposition to avoid thermal effects on the landing gear. Summary of the invention

[0006] In order to overcome the above-mentioned shortcomings, the inventors of the present invention have continuously reformed and innovated through long-term exploration and attempts, multiple experiments and efforts, and proposed a method for preparing a wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear. The method can achieve inner surface coating in one step, and the bonding strength of the film layer is greatly improved by combining infiltration and deposition. The deposition temperature is low, which is the same as the tempering temperature of most metals, and will not affect the strength of the landing gear.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is to provide a method for preparing a wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear. The steps include:

[0008] 1) Grind and polish the inner surface of the landing gear until the roughness reaches the preset standard;

[0009] 2) Degrease and clean the landing gear until the water film is continuous;

[0010] 3) Place the landing gear in the vacuum equipment, connect the landing gear to the negative pole of the power supply, connect the vacuum chamber to the positive pole of the power supply, and evacuate the vacuum chamber to 5.0×10 -3 Below Pa;

[0011] 4) Introduce argon gas, control the pressure in the vacuum chamber to 1 Pa-30 Pa, turn on the heating switch to raise the temperature in the furnace to the set temperature, then turn on the power switch, adjust the power bias, pulse frequency, and pulse width, so that the inner hole of the landing gear undergoes hollow cathode discharge to generate argon plasma to perform argon plasma cleaning on the inner surface of the landing gear;

[0012] 5) After the argon plasma cleaning is completed, a mixed gas of nitrogen and hydrogen or ammonia is gradually introduced, and the gas pressure, power bias, pulse frequency, pulse width and temperature are adjusted to perform nitriding treatment on the inner surface of the landing gear;

[0013] 6) Gradually introduce a carbon-containing gas source to carry out nitrogen carbonization treatment;

[0014] 7) Gradually reduce until the nitrogen-containing gas source flow is shut down, and the inner hole hollow cathode discharge is maintained for carbon film deposition;

[0015] 8) Turn off the power, close the gas valve, open the vacuum chamber vent valve, and take the furnace out after the furnace temperature drops.

[0016] According to the method for preparing a wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear of the present invention, a further preferred technical solution is: in step 1), the roughness needs to reach Ra0.2 μm or less.

[0017] According to the method for preparing a wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear described in the present invention, a further preferred technical solution is: in step 2), the degreasing cleaning includes preliminary cleaning and rinsing, the preliminary cleaning adopts detergent assisted by ultrasonic cleaning, and after the preliminary cleaning is completed, it is rinsed in pure water, and the rinsing time is not less than 1 minute. If the cleaning standard cannot be met, the preliminary cleaning and rinsing steps are repeated until the standard is met.

[0018] According to the method for preparing the wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear of the present invention, a further preferred technical solution is: after the cleaning in step 2) is completed, the non-coating area of ​​the landing gear is selectively masked.

[0019] According to the method for preparing a wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear described in the present invention, a further preferred technical solution is: in step 4), the temperature is set to 200°C~300°C; the power bias is -1000V~-4000V; the pulse frequency is 300Hz~1500Hz; and the pulse width is 5μs~30μs.

[0020] According to the method for preparing the wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear of the present invention, a further preferred technical solution is: in step 4), the argon plasma cleaning time is not less than 10 minutes.

[0021] According to the method for preparing a wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear described in the present invention, a further preferred technical solution is: in step 5), the pulse frequency is 300Hz~1500Hz, the power bias is -2000V~-4000V, the pulse width is 5μs~30μs, and the temperature is 200℃~500℃.

[0022] According to the method for preparing a wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear described in the present invention, a further preferred technical scheme is: in step 6), the carbon-containing gas source is any one or a mixed gas of any of the following: methane, ethane, propane, butane, ethylene, propylene, butene, acetylene, propyne, butyne, tetramethylsilane, hexamethyldisiloxane, and carbon tetrafluoride.

[0023] Compared with the prior art, the technical solution of the present invention has the following advantages / benefits:

[0024] 1. Compared with electroplated chrome on landing gear, vacuum vapor deposition carbon-based film has a dense structure, good corrosion resistance and air tightness, and can effectively prevent the problems of gasping and leakage during the service of landing gear. The film layer prepared by this method has a smooth surface and does not require further processing, which can effectively reduce the quality risk brought by post-processing, reduce the coating temperature, and can be coated at about 200°C to ensure the strength of the landing gear. This method does not produce toxic and harmful substances. Compared with electroplated chrome, it is a green and environmentally friendly surface treatment method.

[0025] 2. Compared with the existing physical vapor deposition carbon film technology, physical vapor deposition technology is difficult to achieve inner surface coating, and this method can achieve inner surface coating in one step.

[0026] 3. This method combines infiltration and deposition. Compared with general chemical vapor deposition, this method greatly improves the bonding strength of the film layer. In addition, the deposition temperature of this method is lower than the tempering temperature of most metals and will not affect the strength of the landing gear.

[0027] 4. The inner wall nitriding technology is combined with the hollow cathode discharge deposition of carbon-based film to increase the substrate hardness and reduce the surface friction coefficient. Through nitriding, carbonitriding treatment and in-situ carbon-based film deposition, a gradual transition layer by layer is achieved to improve the bonding strength of the film layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 The present invention is a flow chart of a method for preparing a wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. Therefore, the detailed description of the embodiments of the present invention provided below is not intended to limit the scope of the claimed invention, but merely represents the selected embodiments of the present invention.

[0031] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and thus, once an item is defined in one drawing, it may not be further defined or explained in the subsequent drawings.

[0032] Embodiment 1:

[0033] A method for preparing a wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear. The steps include:

[0034] 1) Grind and polish the inner surface of the landing gear to a roughness of Ra0.2μm or less;

[0035] 2) Degreasing and cleaning the landing gear until the water film is continuous. Degreasing and cleaning include preliminary cleaning and rinsing. The preliminary cleaning uses detergent and ultrasonic cleaning. After the preliminary cleaning, rinse in pure water for 3 minutes. If the cleaning standard cannot be met, repeat the preliminary cleaning and rinsing steps until the standard is met. After the cleaning is completed, the non-coated area of ​​the landing gear is selectively masked;

[0036] 3) Place the landing gear in the vacuum equipment, connect the landing gear to the negative pole of the power supply, connect the vacuum chamber to the positive pole of the power supply, and evacuate the vacuum chamber to 5.0×10 -3 Below Pa;

[0037] 4) Introduce argon gas, control the pressure in the vacuum chamber to 1Pa-30Pa, turn on the heating switch to raise the temperature in the furnace to the set temperature, then turn on the power switch, adjust the power bias, pulse frequency, and pulse width, so that the inner hole of the landing gear undergoes hollow cathode discharge to generate argon plasma to perform argon plasma cleaning on the inner surface of the landing gear. The set temperature is 200℃~300℃; the power bias is -1000V~-4000V; the pulse frequency is 300Hz~1500Hz; the pulse width is 5μs~30μs, and the argon plasma cleaning time is not less than 10 min; of course, this parameter is only a reasonable parameter range and can be adjusted according to usage requirements.

[0038] 5) After the argon plasma cleaning is completed, a mixed gas of nitrogen and hydrogen or ammonia is gradually introduced, and the gas pressure, power bias, pulse frequency, pulse width and temperature are adjusted to perform nitriding treatment on the inner surface of the landing gear. In this step, the pulse DC power frequency is 300Hz~1500Hz, the voltage value is 2000V~4000V, the pulse width is 20μs, and the temperature is 200℃~500℃. The power supply can be adjusted according to the actual situation. Generally speaking, the higher the temperature, the better the effect, but it will also affect the strength of some metal substrates such as aluminum alloy and alloy steel. The requirements for aviation landing gear are that aluminum alloy does not exceed 200℃, alloy steel does not exceed 300℃, and titanium alloy does not exceed 500℃. The advantage of this process is that the temperature can be reduced, and coating can be achieved at about 200℃ to ensure the strength of the landing gear;

[0039] 6) gradually introducing a carbon-containing gas source for nitrogen carbonization treatment, wherein the carbon-containing gas source is any one or a mixture of any of the following gases: methane, ethane, propane, butane, ethylene, propylene, butene, acetylene, propyne, butyne, tetramethylsilane, hexamethyldisiloxane, and carbon tetrafluoride. Of course, these are only some existing carbon-containing gases, and existing gases or other possible synthetic gases may also be applicable to the present invention;

[0040] 7) Gradually reduce until the nitrogen-containing gas source flow is shut down, maintain the inner hole hollow cathode discharge for carbon film deposition, so that the inner hole can continue to deposit carbon film to increase the thickness of the carbon film and avoid the existence of uncoated areas or thin thickness;

[0041] 8) Turn off the power, close the gas valve, open the vacuum chamber vent valve, and take the furnace out after the furnace temperature drops.

[0042] Embodiment 2:

[0043] In this example, an aluminum alloy landing gear outer tube is taken as an example to prepare a wear-resistant self-lubricating coating on the inner surface of the landing gear outer tube.

[0044] (1) Use a special grinding tool to grind and polish the inner hole of the aluminum alloy landing gear, and use a handheld roughness tester to test the roughness of the inner hole until the roughness drops below Ra0.1μm.

[0045] (2) Soak the landing gear in an aluminum alloy cleaning solution for 20 minutes for ultrasonic cleaning to remove oil, then rinse it in pure water for 3 minutes and observe the state of the water film on the landing gear surface. If the water film cannot be continuous, return it to the aluminum alloy cleaning solution for cleaning again.

[0046] (3) Use special tooling to mask the non-coating area, place the landing gear in the vacuum coating machine, connect the landing gear to the negative pole of the power supply (the connection method can achieve hollow cathode discharge in the inner hole), and connect the vacuum chamber to the positive pole of the power supply.

[0047] (4) Introduce argon gas at a flow rate of 200 sccm, adjust the vacuum valve, control the pressure in the vacuum chamber to 10 Pa, turn on the heating switch, and set the heating temperature to 200°C. After the temperature reaches the set temperature, turn on the power switch, set the power bias to -1000V, the pulse frequency to 500Hz, and the pulse width to 20 μs, so that the inner hole of the landing gear undergoes hollow cathode discharge to generate argon plasma to perform argon plasma cleaning on the inner surface of the landing gear for 15 minutes.

[0048] (5) Open the nitrogen and hydrogen valves, introduce nitrogen and hydrogen, set the nitrogen flow rate to 90 sccm, the hydrogen flow rate to 30 sccm, reduce the argon flow rate to 100 sccm, adjust the vacuum valve, control the pressure in the vacuum chamber to 10 Pa, adjust the bias voltage to -2500 V, and continue for 2 hours.

[0049] (6) Open the tetramethylsilane valve and control the tetramethylsilane flow rate to slowly increase to 16 sccm within 10 minutes. At the same time, slowly reduce the nitrogen and hydrogen flow rates until they are closed, and slowly increase the argon flow rate to 160 sccm. Adjust the pressure in the vacuum chamber to 10 Pa and the bias voltage to -1000 V for 10 minutes.

[0050] (7) Open the acetylene valve, set the acetylene flow rate to 60 sccm, reduce the argon flow rate to 100 sccm, and adjust the air pressure in the vacuum chamber to 10 Pa for 30 minutes.

[0051] (8) Turn off the power supply, close the gas valve, open the vacuum chamber vent valve, and wait until the furnace temperature drops below 100°C before taking the furnace out.

[0052] Embodiment 3:

[0053] In this embodiment, an aluminum-titanium alloy landing gear outer tube is taken as an example to prepare a wear-resistant self-lubricating coating on the inner surface of the landing gear outer tube.

[0054] (1) Use a special grinding tool to grind and polish the inner hole of the aluminum alloy landing gear, and use a handheld roughness tester to test the roughness of the inner hole until the roughness drops below Ra0.1μm.

[0055] (2) Soak the landing gear in a degreasing cleaning agent and perform ultrasonic cleaning for 20 minutes, then rinse it in pure water for 1 to 3 minutes and observe the state of the water film on the landing gear surface. If a continuous water film cannot be achieved, return it to the degreasing cleaning agent for further cleaning.

[0056] (3) Use special tooling to mask the non-coating area, place the landing gear in the vacuum coating machine, connect the landing gear to the negative pole of the power supply, and connect the vacuum chamber to the positive pole of the power supply.

[0057] (4) Introduce argon gas at a flow rate of 200 sccm, adjust the vacuum valve, control the pressure in the vacuum chamber to 8 Pa, turn on the heating switch, and set the heating temperature to 300°C. After the temperature reaches the set temperature, turn on the power switch, set the bias voltage to -1000V, the pulse frequency to 500Hz, and the pulse width to 20μs, so that the inner hole of the landing gear undergoes hollow cathode discharge to generate argon plasma to perform argon plasma cleaning on the inner surface of the landing gear for 15 minutes.

[0058] (5) Open the nitrogen and hydrogen valves, introduce nitrogen and hydrogen, set the nitrogen flow rate to 100 sccm, the hydrogen flow rate to 50 sccm, reduce the argon flow rate to 80 sccm, adjust the vacuum valve, control the pressure in the vacuum chamber to 8 Pa, adjust the bias voltage to -3000 V, and continue for 2 h.

[0059] (6) Open the acetylene valve and control the acetylene flow rate to slowly increase to 80 sccm within 10 minutes. At the same time, slowly reduce the nitrogen and hydrogen flow rates until they are closed, and slowly increase the argon flow rate to 160 sccm. Adjust the pressure in the vacuum chamber to 10 Pa and the bias voltage to -1000 V for 10 minutes.

[0060] (7) Open the tetramethylsilane valve, control the tetramethylsilane flow rate to 8 sccm, maintain the acetylene flow rate to 80 sccm, and the argon flow rate to 160 sccm for 7 minutes.

[0061] (8) Close the tetramethylsilane valve, maintain the acetylene flow rate at 80 sccm and the argon flow rate at 160 sccm for 10 min.

[0062] (9) Turn off the power, close the gas valve, open the vacuum chamber vent valve, and wait until the furnace temperature drops below 100°C before taking the furnace out.

[0063] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0064] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0065] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear. It is characterized in that The steps include: 1) grinding and polishing the inner surface of the landing gear until the roughness reaches the preset standard; 2) Degrease and clean the landing gear until the water film is continuous; 3) Place the landing gear in the vacuum equipment, connect it to the negative pole of the power supply, connect the vacuum chamber to the positive pole of the power supply, and evacuate to 5.0×10 -3 Pa or less; 4) Introduce argon gas, control the pressure in the vacuum chamber to 1 Pa-30 Pa, turn on the heating switch to raise the temperature in the furnace to the set temperature, then turn on the power switch, adjust the power bias, pulse frequency, and pulse width, so that the inner hole of the landing gear undergoes hollow cathode discharge to generate argon plasma to perform argon plasma cleaning on the inner surface of the landing gear; 5) After the argon plasma cleaning is completed, a mixed gas of nitrogen and hydrogen or ammonia is gradually introduced, and the gas pressure, power bias, pulse frequency, pulse width and temperature are adjusted to perform nitriding treatment on the inner surface of the landing gear, and the power bias is -2000V~-4000V; 6) A carbon-containing gas source is gradually introduced to perform nitrogen carbonization treatment; 7) Gradually reduce until the nitrogen-containing gas source flow is shut down, and the inner hole hollow cathode discharge is maintained for carbon film deposition; 8) Turn off the power, close the gas valve, open the vacuum chamber vent valve, and take the furnace out after the furnace temperature drops.

2. A method for preparing a wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear according to claim 1, It is characterized in that In step 1), the roughness needs to be less than Ra0.2μm.

3. The method for preparing the wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear according to claim 1, It is characterized in that In step 2), the degreasing cleaning includes preliminary cleaning and rinsing. The preliminary cleaning adopts detergent assisted by ultrasonic cleaning. After the preliminary cleaning is completed, it is rinsed in pure water. The rinsing time is not less than 1 minute. If the cleaning standard cannot be met, the preliminary cleaning and rinsing steps are repeated until the standard is met.

4. The method for preparing the wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear according to claim 1, It is characterized in that After step 2) cleaning is completed, the non-coated area of ​​the landing gear is selectively masked.

5. The method for preparing the wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear according to claim 1, It is characterized in that In step 4), the temperature is set to 200°C~300°C; the power bias is -1000V~-4000V; the pulse frequency is 300Hz~1500Hz; and the pulse width is 5μs~30μs.

6. The method for preparing the wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear according to claim 1, It is characterized in that In step 4), the argon plasma cleaning time lasts for 10 minutes to 30 minutes.

7. The method for preparing the wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear according to claim 1, It is characterized in that In step 5), the pulse DC power supply frequency is 300 Hz to 1500 Hz, the pulse width is 5 to 30 μs, and the temperature is 200° C. to 500° C.

8. The method for preparing the wear-resistant self-lubricating coating for the inner hole of an aircraft landing gear according to claim 1, It is characterized in that In step 6), the carbon-containing gas source is any one or a mixed gas of the following: methane, ethane, propane, butane, ethylene, propylene, butene, acetylene, propyne, butyne, tetramethylsilane, hexamethyldisiloxane, and carbon tetrafluoride.