Neutron in-situ diagnostic system and method for directional solidification of single crystal high-temperature alloys

Through the combination of neutron scattering technology and vacuum environment system, in-situ diagnosis of the directional solidification process of single crystal high-temperature alloys is achieved, which solves the problem of the inability of existing technology to monitor and improve blade quality in real time, and provides efficient process optimization and quality improvement. means of control.

CN118425208BActive Publication Date: 2024-10-01NORTHEASTERN UNIV CHINA
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN202410879082.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-01
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

The existing technology cannot directly observe the formation of solid-liquid interface or growth defects during the directional solidification process of single crystal superalloys in situ, and cannot diagnose and improve the microscopic mechanism of blade quality in real time, especially in controlling the microstructure of single crystal superalloys in industrial production. and defect formation mechanisms.

Method used

Using neutron scattering technology combined with the vacuum environment system and comprehensive control system, neutron in-situ diffraction is performed in the vacuum chamber through the neutron incident window, diffraction window and transmission window, and the orientation deviation and orientation deviation during the directional solidification process of single crystal high-temperature alloys are diagnosed in real time. Defects such as crystalline integrity and striped crystals.

Benefits of technology

It achieves in-situ and real-time diagnosis of the directional solidification process of single crystal superalloys, can monitor and analyze defects such as orientation deviation, plastic deformation and recrystallization of columnar dendrites in real time, and provide technical data for process optimization and quality control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118425208B_ABST
    Figure CN118425208B_ABST
Patent Text Reader

Abstract

The present invention relates to a neutron in-situ diagnostic system and method for the directional solidification process of a single crystal high-temperature alloy, belonging to the technical field of high-temperature alloy manufacturing, and includes a vacuum environment system suitable for carrying out time-of-flight neutron in-situ diffraction, a single crystal growth system, and a comprehensive control system for controlling the vacuum environment system and the single crystal growth system. The present invention can realize in-situ and minute-level real-time diagnosis of the directional solidification process of a single crystal high-temperature alloy, and make continuous analysis for analyzing the conditions for the occurrence and duration of defects, thereby providing technical data for the optimization and innovative design of processes in industrial production. The method is not limited to the directional solidification process of single crystal high-temperature alloys, but can also be applied to the diagnosis of the heat treatment process of high-temperature alloys or the solidification and heat treatment process of other medium- and high-melting-point metals or alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of high-temperature alloy manufacturing, and in particular relates to a neutron in-situ diagnosis system and method for a single crystal high-temperature alloy directional solidification process. Background Art

[0002] High-temperature alloys are key materials for making hot-end components of aircraft engines and gas turbines in power plants. They are usually made of nickel as the main alloying element, with the addition of medium- and low-melting-point metals such as Al, Co, Cr, and Ti, as well as high-melting-point metal elements such as Nb, Mo, Hf, W, Re, Ta, and Ru. The liquidus temperature (complete melting temperature) of the alloy is usually between 1300°C and 1500°C. According to its composition and grade, it can be divided into single-crystal high-temperature alloys and polycrystalline high-temperature alloys. Among them, the development of single-crystal high-temperature alloys has received great attention from domestic and foreign research and development institutions because of its important applications in key fields.

[0003] The manufacturing process of single crystal high temperature alloy is mainly directional solidification technology, whose main feature is that after melting the alloy raw material, the melt is introduced into an alumina ceramic membrane shell with a specific directional temperature gradient G, and then the directional solidification is achieved and controlled by controlling the temperature gradient G and the pulling rate V of the container from the hot end to the cold end. Its main microstructural feature is that the columnar dendrites are directional and arranged along the thermal gradient direction (i.e., growth direction) of directional solidification. Single crystal blades made in this way are relatively expensive and are generally used in advanced aircraft engines and gas turbines in power plants. Therefore, how to reduce the scrap rate in the production process is an important means to reduce costs.

[0004] A Chinese patent (publication number: CN219703470U, publication date: September 19, 2023) discloses a directional solidification device for high-speed solidification, which improves the yield of directionally solidified single-crystal high-temperature alloy blades for aero-engines by solving the problems of uneven temperature fields inside and outside the casting, reduced temperature gradients on the inside, and unsatisfactory unidirectional heat flow conditions.

[0005] A Chinese patent (publication number: CN116689741A, publication date: September 5, 2023) discloses a method for adjusting the directional solidification temperature field and optimizing the stray crystals of castings by partially packing cotton in the mold shell. This method adjusts the temperature field distribution during the directional solidification of single crystal high-temperature alloy castings by partially packing cotton in the single crystal casting shell, thereby achieving the purpose of eliminating stray crystal defects in single crystal high-temperature alloy castings. The invention can effectively reduce the generation of stray crystals in directional solidification castings, has a simple operation process and low cost, and is suitable for mass production of engineered single crystal high-temperature alloy castings.

[0006] A Chinese patent (publication number: CN219541677U, publication date: August 18, 2023) discloses a device that can control the flatness of the solid-liquid interface during the cooling and directional solidification of liquid metal. The device can maintain the liquid metal level in the cooling tank always flush with the tank mouth during the directional pulling of membrane shells with different cross-sections, so that the radial temperature field of the solidified material is stable during the directional solidification process, ensuring growth in a flat interface manner, thereby improving the mechanical properties of the directional solidification casting while reducing the generation of defects.

[0007] A Chinese patent (publication number: CN115625291A, publication date: January 20, 2023) discloses a device and method for eliminating zebra crystals (also known as stripe crystals) on nickel-based single crystal high-temperature alloy blades. The device includes a wax mold and a wax block for a nickel-based single crystal high-temperature alloy blade. During the wax mold making stage, the wax block is set at a position where zebra crystals are prone to appear on the edge plate of the single crystal high-temperature alloy blade. The temperature field at the position where zebra crystals are generated on the edge plate of the original single crystal high-temperature alloy blade can be changed during the directional solidification process, thereby completely eliminating the zebra crystals of the single crystal high-temperature alloy blade.

[0008] The Chinese patent (publication number: CN116906126A, publication date: October 20, 2023) discloses a multi-unit guide vane of ceramic-based composite materials and single-crystal high-temperature alloys and a preparation method. The invention solves the problem of mismatch in thermal expansion coefficients between ceramic-based materials and high-temperature alloys at high temperatures by integrally forming heterogeneous blades of single-crystal high-temperature alloys and ceramic-based composite materials.

[0009] The above five patents respectively adopt the method of changing the process parameters or changing the structure of the directional solidification device (increasing the pulling rate V, using asbestos to wrap the shell, using liquid metal to enhance cooling at the cold end, adding wax blocks at specific ends of the blade, and integrated molding) to improve the yield of single crystal high-temperature alloy blades, but it is impossible to directly observe in situ the formation process of the solid-liquid interface or growth defects during the directional solidification of the single crystal blade, and it is impossible to determine the microscopic mechanism of improving the blade quality after taking measures.

[0010] Like other high-temperature structural materials, controlling the microstructure of single-crystal high-temperature alloy blades is an important means to obtain high-temperature mechanical properties. In industrial production, orientation deviation, recrystallization caused by plastic deformation, and streak crystals appearing locally on blades are the main defects that limit the stability of batch production of high-performance high-temperature alloy single-crystal blades. Therefore, whether from the perspective of single-crystal blade quality control or the development of scientific instruments, it is necessary to develop diagnostic systems and methods that can directly analyze the microstructure evolution, especially the defect formation mechanism, during the manufacturing process of high-temperature alloy single-crystal blades in situ.

[0011] A Chinese patent (publication number: CN104345071A, publication date: February 11, 2015) discloses a method for characterizing the lattice mismatch of the γ / γ' phase in a nickel-based high-temperature alloy using X-ray diffraction phenomena. This characterization method can achieve in-situ measurement of bulk solids. The operation of this characterization method is simple and convenient, and the requirements for equipment are not high. However, this characterization is only applied at room temperature, and due to the limitation of the penetration depth of X-rays, it can only detect the lattice mismatch near the surface position without covering, and the scope of application is limited.

[0012] A Chinese patent (publication number: CN117664992A, publication date: March 8, 2024) discloses a method for observing streak crystal defects in single crystal high-temperature alloy castings using a laser confocal microscope and a scanning electron microscope. This method analyzes the chemical composition factors and crystal orientation that produce streak crystals, and is used to infer the mechanism that causes streak crystal defects. It has reference value for formulating measures to control streak crystal defects in industrial production. However, this invention belongs to a post-analysis method, not an in-situ diagnostic analysis.

[0013] A Chinese patent (publication number: CN115586317A, publication date: January 10, 2023) discloses a method for evaluating the tendency of single crystal high temperature alloy to form freckles. This evaluation method can evaluate the tendency of freckle formation after the cast sample is obtained after pouring. It does not require heat treatment and other detection methods. The operation is simple, fast and efficient, and can save time and cost. However, this method is a post-analysis, not an in-situ diagnostic analysis, and has certain requirements on the shape and size of the sample.

[0014] In the 1970s and 1980s, domestic and foreign research institutions and production enterprises usually used post-test methods such as metallographic microscopes, scanning electron microscopes and transmission electron microscopes to determine the crystal quality of single crystal high-temperature alloys and blades after directional solidification. The characteristic of this method is that it can reveal the morphology and crystallographic characteristics of dendrites. However, this detection method is a destructive detection method, which not only has a long cycle, but also belongs to post-test and is usually carried out at room temperature.

[0015] In recent years, researchers from some domestic institutions have set up mechanical and high-temperature platforms, combined them with scanning electron microscopy and transmission electron microscopy techniques, and used backscattered electron diffraction or electron diffraction techniques to carry out real-time and in-situ observations of the microstructural evolution of polycrystalline and single-crystal superalloys under mechanical loading and high temperature conditions. Some researchers have used transmission electron microscopy and scanning transmission electron microscopy to study the rapid solidification process of aluminum alloys. However, due to the penetration ability of the electron beam (less than 0.001 mm) and the space limitations in the microscope, the use of diffraction technology in electron microscopy to carry out real-time and in-situ diagnosis of the directional solidification process of single-crystal superalloys or blades faces many challenges. There are no reports of such research in the current public literature.

[0016] Synchrotron radiation technology is a large scientific device technology established in the 1940s. It was first used to study the structural evolution of liquid metals during solidification in the 1990s. At that time, European researchers used high-brightness synchrotron radiation X-ray sources to conduct in-situ diagnosis of the structural evolution of low-melting-point liquid metals such as lead and tin during solidification. The establishment of this advanced technology provides researchers and technicians with a new way to understand the real structural evolution information during the solidification of liquid metals.

[0017] Since 2010, scientists and researchers in Europe and the United States have used synchrotron radiation X-ray two-dimensional imaging technology to observe the microstructural evolution information during fatigue, creep and heat treatment of single crystals. Around 2020, researchers carried out structural evolution characteristics of high-temperature alloys during directional solidification at synchrotron radiation light sources. Since then, researchers at home and abroad have conducted computer simulations of experimental phenomena. These practices have shown that synchrotron radiation imaging technology does provide researchers with a powerful real-time and in-situ diagnostic method to understand the morphological evolution of dendrites during directional solidification of single-crystal high-temperature alloys. However, in-situ and real-time diagnosis based on synchrotron radiation imaging has two limitations. On the one hand, high-temperature alloys contain heavy elements such as Hf, W, Re, Ta, and Ru, which have particularly significant absorption of X-rays. In order to meet the penetration requirements, the single crystal high temperature alloy used must be very thin, with a thickness of only 0.05mm-0.2mm, which is 2 to 3 orders of magnitude different from the actual single crystal high temperature alloy blade thickness of centimeters. Therefore, the observed morphological evolution information cannot fully reflect the microstructural evolution law of the single crystal high temperature alloy blade during the directional solidification process. On the other hand, its working principle is to obtain the morphological evolution information of dendrites based on the difference in X-ray absorption caused by the difference in liquid and solid phase density. Therefore, it is impossible to determine the crystallographic direction difference of columnar dendrites, especially the deviation of the crystallographic axis relative to the blade geometry (orientation deviation), plastic deformation and dynamic recrystallization and other microstructural information related to crystallographic characteristics.

[0018] The Chinese patent (publication number: CN117092142A, publication date: November 21, 2023) discloses a method, system and equipment for detecting hollow turbine blades. The invention also involves the field of X-ray detection technology. It mainly uses industrial CT in electronic computer tomography equipment to complete the full-process dimensional detection and dimensional error analysis of the blade investment casting process. This detection method improves the accuracy of the full-process detection of hollow turbine blades. However, the detection is a post-detection and is carried out at room temperature. Because the ray source used is X-ray, the thickness of the blade that can be penetrated is limited.

[0019] A Chinese patent (publication number: CN110715946A, publication date: January 21, 2020) discloses a single crystal stress tensor measurement method based on monochromatic X-ray diffraction. The invention uses X-ray diffraction results to calculate the residual strain tensor of single crystal materials, and provides a data processing method for the widely used and equipped X-ray diffraction / stress instrument to measure the residual strain of single crystal materials. It can be achieved using a personal computer or a computing platform with similar performance, simplifying the measurement and calculation requirements. However, the detection is a post-detection and is carried out at room temperature, and the thickness of the material sample that can be measured is also limited.

[0020] In short, neither traditional nor modern two-dimensional imaging methods using physical means such as visible light, electron beam or X-ray can diagnose in situ the microstructural evolution, especially the defect formation mechanism, during the directional solidification of centimeter-scale single-crystal high-temperature alloy samples that are close to industrial production practice.

[0021] In principle, the crystallographic structural information in the microstructure of single-crystal superalloys can be obtained by using synchrotron X-ray diffraction technology. Superalloys contain more heavy elements, so the absorption is also stronger. This means that the depth of the sample that can be penetrated is also limited. If in-situ diffraction diagnosis of the directional solidification process of single-crystal superalloys is to be carried out, a ceramic membrane shell must be placed on its periphery, which will further reduce the intensity of the X-ray signal, so it still faces difficulties in practical application. At present, the only public information at home and abroad is about synchrotron radiation research on the microstructural evolution of single-crystal superalloys during heat treatment and in the additive manufacturing of polycrystalline superalloys. There are no cases of using synchrotron X-ray in-situ diffraction technology for in-situ diagnosis of microstructural evolution during directional solidification of single-crystal superalloys.

[0022] Unlike X-rays, neutrons interact with the nucleus itself rather than the electrons outside the nucleus. Moreover, the intensity of their interaction with the nucleus is not directly related to the atomic number, which makes it easier to distinguish neighboring elements and analyze alloy materials containing heavy elements. Like X-rays, neutrons also undergo elastic and inelastic scattering with atoms in materials. Among them, the elastic coherent scattering of neutrons and orderly arrangements in crystalline materials is called diffraction. Based on the strong penetrating power of neutrons, neutron diffraction technology can, in principle, be used for in-situ and real-time diagnosis of the structural evolution of single-crystal high-temperature alloys with thicknesses of millimeters to centimeters at high temperatures.

[0023] Reactor neutron sources and spallation neutron sources were built in Europe, America, Japan and other countries in the last century. my country built advanced reactor neutron sources and spallation neutron sources for materials science research around 2010. So far, there are reports in domestic and foreign public literature on the use of neutron scattering technology to study the structural evolution of solidified single crystal superalloys at room temperature or during heat treatment at temperatures not higher than 1300°C. For example, researchers in the UK used the Bragg edge imaging technology of neutron scattering technology to study the orientation difference distribution in the directionally solidified CMSX series single crystal superalloys, and domestic researchers used neutron diffraction technology to study the crystallographic structure information of single crystal superalloys at room temperature under cast and different heat treatment industrial conditions.

[0024] At present, there are no systematic and methodological cases of using neutron scattering technology for in-situ and real-time diagnosis of the structural evolution of single crystal high-temperature alloys during directional solidification in public literature reports at home and abroad. Summary of the invention

[0025] In view of the deficiencies in the prior art, based on the strong penetration capability of neutron scattering and the increasingly perfect construction of neutron sources, the present invention provides a neutron in-situ diagnostic system and method for the directional solidification process of single crystal high-temperature alloys.

[0026] A neutron in-situ diagnostic system for a single crystal high temperature alloy directional solidification process, characterized in that it comprises a vacuum environment system suitable for carrying out time-of-flight neutron in-situ diffraction, a single crystal growth system and a comprehensive control system for controlling the vacuum environment system and the single crystal growth system.

[0027] The vacuum environment system includes a vacuum chamber, a vacuum unit and a vacuum measurement system for evacuating the vacuum chamber, a neutron passage, and a cooling water subsystem for cooling, wherein the neutron passage is arranged on the cavity of the vacuum chamber;

[0028] The neutron passage comprises a neutron incident window, a neutron diffraction window and a neutron transmission window. The neutron incident window is made of a vanadium-nickel alloy transparent to neutrons, has a circular shape, and is arranged at the position where the neutron beam enters the vacuum chamber; the neutron diffraction window is made of an aluminum alloy with low neutron absorption, has a square shape, and is arranged on the side wall of the vacuum chamber at a direction of 90° to the incident neutron beam. There are two of them, which are arranged oppositely, and are the left neutron diffraction window and the right neutron diffraction window respectively; the neutron transmission window is made of a vanadium-nickel alloy transparent to neutrons, has a square shape, and is arranged on the side wall of the vacuum chamber directly facing the neutron incident window;

[0029] A loading port is provided at the upper part of the vacuum chamber;

[0030] A thermocouple insertion port is provided on the side wall of the vacuum chamber, and a temperature-controlling thermocouple and a temperature-measuring thermocouple are installed thereon, which are electrically connected to a heating power supply control cabinet, and the heating power supply control cabinet is electrically connected to an integrated control system.

[0031] The vacuum chamber is a stainless steel cylindrical vacuum chamber with a water-cooled double-layer structure, which is fixed on a vacuum chamber bracket. A vacuum chamber support rod is connected to the bottom of the vacuum chamber bottom plate, and the vacuum chamber support rod is connected and fixed to the vacuum chamber bracket; the top of the vacuum chamber is a movable vacuum chamber top cover, which is connected and fixed by the movable vacuum chamber top cover fixing screws.

[0032] The vacuum unit includes a rotary vane vacuum pump fixed by a pump body bracket, an electromagnetic valve is installed between the rotary vane vacuum pump and the turbomolecular pump, the turbomolecular pump is connected to the connecting pipe welded on the vacuum chamber through a large-diameter bellows, and is communicated with the interior of the vacuum chamber, and an ionization vacuum gauge, a resistance vacuum gauge and a venting valve are arranged on the connecting pipe; a bellows horizontal support frame and a bellows vertical support frame are arranged outside the large-diameter bellows; a bypass is arranged between the electromagnetic valve and the turbomolecular pump, and a vacuum gate valve is arranged on the turbomolecular pump; a temperature sensor is arranged inside the vacuum chamber.

[0033] The cooling water subsystem includes a chiller, which is connected to the middle cavity of the double wall of the vacuum chamber, the flange at the temperature measuring thermocouple insertion port, the flange at the upper heating element electrode and the lower heating element electrode, the turbomolecular pump, and the movable vacuum chamber top cover through a cooling water row and a cooling water pipe, so as to cool the neutron incident window, the left neutron diffraction window, the right neutron diffraction window, the neutron transmission window, the middle cavity of the vacuum chamber and the turbomolecular pump; the cooling water circulates in the middle cavity of the double wall of the vacuum chamber to achieve the purpose of cooling.

[0034] The single crystal growth system is provided with a heating element and a heat preservation layer, a funnel-shaped chemical material pool, a sample rotating mechanism, a sample upper and lower pulling mechanism and a liquid metal cooling tank, wherein the heating element, the heat preservation layer and the funnel-shaped chemical material pool are placed in a vacuum chamber, and the sample rotating mechanism, the sample upper and lower pulling mechanism and the liquid metal cooling tank are placed outside the vacuum chamber; the liquid metal cooling tank is a 304 stainless steel tank containing liquid metal.

[0035] The heating element in the single crystal growth system comprises an upper heating element, an upper thermal insulation layer, a lower heating element and a lower thermal insulation layer, the upper heating element and the lower heating element are coaxially arranged, and the upper thermal insulation layer and the lower thermal insulation layer are coaxially arranged;

[0036] It also includes a heating element support frame fixed on the bottom plate of the vacuum chamber and a circular alumina ceramic insulation baffle with a central opening and coaxial with the heating element and the insulation layer, the lower heating element is arranged on the heating element support frame, the circular alumina ceramic insulation baffle is placed on the top of the lower heating element, and the upper heating element and the upper insulation layer are placed on the circular alumina ceramic insulation baffle; the upper insulation layer and the upper heating element are composed of a combination of seven layers of cylinders with different diameters, the innermost layer is the upper heating element heating cylinder, and the remaining six layers are the upper insulation layer, and the adjacent layers have a spacing of 2mm-5mm; the lower insulation layer and the lower heating element are composed of a combination of seven layers of cylinders with different diameters, the innermost layer is the lower heating element heating cylinder, and the remaining six layers are the lower insulation layer, and the adjacent layers have a spacing of 2mm-5mm;

[0037] The top of the upper heating element heating cylinder is the top of the insulation layer, which is a six-layer parallel insulation top cover corresponding to the six insulation layers respectively, and the six-layer parallel insulation top cover is provided with an insulation layer top cover support rod for support and fixation, and the top insulation board is provided with an upper top handle; the bottom of the lower heating element heating cylinder is provided with six layers of parallel insulation bottom plates corresponding to the six insulation layers respectively, and the six layers of parallel insulation bottom plates are provided with insulation layer bottom plate support rods for support and fixation; a lower heating element insulation bottom plate is provided between the bottom of the six layers of parallel insulation bottom plates and the heating element support frame;

[0038] The lower part of the lower insulation layer outside the lower heating element is provided with through holes for neutron incidence, transmission and two-way diffraction, as well as thermocouple installation channels and electrode connection channels. The bottom of the heating tube of the lower heating element is not provided with holes. The sizes of the through holes increase proportionally from the innermost layer to the outermost layer, thereby forming a conical through hole from the inside to the outside.

[0039] The side wall of the upper heating body heating cylinder is provided with a plurality of upper heating body thermocouple insertion ports, and the upper heating body heating cylinder is provided with an upper heating body electrode I and an upper heating body electrode II, wherein the upper heating body electrode I is the access end, and the upper heating body electrode II is the access end; the upper heating body electrode I is externally sleeved with an upper heating body introduction electrode insulating sleeve, and the upper heating body electrode II is externally sleeved with an upper heating body lead-out electrode insulating sleeve; the side wall of the lower heating body heating cylinder is provided with a plurality of lower heating body thermocouple insertion ports, and the lower heating body heating cylinder is provided with a lower heating body electrode I and a lower heating body electrode II, wherein the lower heating body electrode I is the access end, and the lower heating body electrode II is the access end; the lower heating body electrode I is externally sleeved with a lower heating body introduction electrode insulating sleeve, and the lower heating body electrode II is externally sleeved with a lower heating body lead-out electrode insulating sleeve; the upper heating body electrode I, the lower heating body electrode I, the upper heating body electrode II and the lower heating body electrode II extend outwardly to the side wall of the vacuum chamber and are electrically connected to the heating power supply control cabinet.

[0040] A coaxial ceramic crucible is arranged inside the lower heating element heating cylinder, and the top of the ceramic crucible is arranged opposite to the funnel-shaped chemical pool in the upper heating element heating cylinder; a pneumatic plugging rod for melt pouring is arranged on the top of the vacuum chamber, which penetrates from the outside into the bottom of the funnel-shaped chemical pool in the upper heating element heating cylinder, and is used for sealing between the funnel-shaped chemical pool and the ceramic crucible;

[0041] The sample up and down pulling mechanism includes a pulling rod, the top of the pulling rod passes through the liquid metal cooling tank and is connected to the ceramic crucible through a molybdenum joint, one end of the molybdenum joint is inserted into the ceramic crucible, and the other end is inserted into the pulling rod; the bottom of the pulling rod is connected to the slide seat, the slide seat moves up and down on the pulling rod guide rail, the pulling rod guide rail is connected to the pulling rod drive motor, and the pulling rod guide rail is fixed to the vacuum chamber bracket through the pulling rod guide rail bracket;

[0042] A sample rotating mechanism is provided at the end of the pulling rod, and the sample rotating mechanism includes a motor. The pulling rod is connected to the output end of the motor, and the pulling rod can rotate around its own axis.

[0043] The integrated control system comprises a programmable logic controller, which serves as a main console. An interactive human-machine control interface, namely a touch control screen, is installed on the top of the cabinet.

[0044] A neutron in-situ diagnosis method for a single crystal high temperature alloy directional solidification process, using the above-mentioned neutron in-situ diagnosis system for a single crystal high temperature alloy directional solidification process, specifically comprises the following steps:

[0045] Step 1: Prepare materials: put the raw materials into the funnel-shaped material pool according to the proportion;

[0046] Step 2: Vacuuming: Using the integrated control system, start the vacuum unit consisting of a rotary vane vacuum pump and a turbomolecular pump to evacuate the vacuum chamber of the vacuum system for neutron diffraction until the pressure in the vacuum chamber is lower than the specified value;

[0047] Step 3: Melting: With the help of the integrated control system, the heating element in the single crystal growth system is powered, and the raw materials in the funnel-shaped material pool are heated and melted into alloy liquid according to the preset heating program and steps;

[0048] Step 4: Pouring and temperature gradient control: With the help of the integrated control system, the pneumatic plug rod for melt pouring is lifted, and the melt is passed through the funnel-shaped material pool into the ceramic crucible, which is the alumina membrane shell used to grow high-temperature alloy single crystals. The integrated control system remotely controls the heating power supply control cabinet to adjust the temperature and temperature gradient of the upper and lower heating elements. The temperature of the lower heating element area is controlled by the liquid metal in the liquid metal cooling tank. Keep warm for 5 minutes to 10 minutes until the temperature is stable.

[0049] Step 5: Directional solidification: With the help of the integrated control system, the pull rod of the single crystal growth system is started, and the alumina film shell containing the single crystal high-temperature alloy melt is pulled down at a uniform or variable speed according to the preset program to make the alloy melt directionally solidified;

[0050] Step six: During the directional solidification process, a neutron beam is introduced through the incident window, passes through the heating element, and then irradiates the alumina membrane shell and the high-temperature alloy in the solidification stage. The neutron diffraction signal generated in the 90° direction passes through the heating element, and then is emitted from the left neutron diffraction window and the right neutron diffraction window and reaches the mid-angle detectors on both sides. By analyzing the flight time, wavelength, intensity and position information of the neutron signal received on the detector, the deviation of the single crystal orientation, the decrease in the crystallization integrity of the single crystal, and the occurrence of defects such as streak crystals and recrystallization that occur during the directional solidification of the single crystal high-temperature alloy are diagnosed in real time.

[0051] The beneficial effects of the present invention are:

[0052] 1. In order to realize the in-situ neutron diffraction of the single crystal high-temperature alloy in the vacuum chamber, a circular neutron incident window and a rectangular neutron transmission window are opened on the vacuum cavity. The normal direction of these windows is parallel to the neutron beam, and water channels are provided on the periphery for forced cooling. The material of the incident window and the transmission window is a vanadium-nickel alloy containing about 4%-4.3% nickel (mass fraction) with a thickness of 1.5mm-3mm processed by hot rolling. This type of alloy will not produce obvious elastic scattering when encountering a neutron beam, so it is transparent to neutrons, which can minimize the stray signals generated by the incident beam and the transmission beam, thereby being beneficial to obtain clear and less-interfered neutron diffraction signals during in-situ diagnosis. In addition, this type of alloy has good hot processing characteristics, high mechanical strength and high room temperature thermal conductivity, which can meet the requirements of mechanical rolling, vacuum sealing and heat dissipation respectively.

[0053] 2. Two rectangular neutron diffraction windows are opened on the cavity of the vacuum diffraction chamber where neutron diffraction occurs. The normal direction of the window is 90° to the neutron beam to meet the needs of detecting the diffraction intensity at medium angles. Both diffraction windows are made of aluminum alloy with a grade of LY12 and a thickness of 2mm-3mm. The main purpose of selecting such aluminum alloy is to minimize the absorption and scattering of neutrons and obtain high-intensity neutron diffraction signals from single crystal high-temperature alloy samples. In addition, this type of alloy also has good machinability, medium mechanical strength, and high thermal conductivity, which can meet the requirements of mechanical rolling, vacuum sealing, and heat dissipation respectively.

[0054] 3. In order to achieve the melt and temperature gradient required for single crystal growth, a combination of upper and lower segmented heating elements is used to segmentally heat the ceramic crucible and the single crystal high-temperature alloy raw material inside. Among them, the upper heating element is used to obtain a temperature higher than the liquidus temperature of the single crystal high-temperature alloy, which is used for melting the alloy and heat preservation of the melt, while the lower heating element is used to obtain an appropriate temperature lower than the solidus temperature of the single crystal high-temperature alloy, which is used to form the necessary temperature gradient inside the heating element to ensure that the alloy melt is directional solidified along the direction of the heat flow. The heating element is made of cylindrical metal Mo or Nb with a single layer thickness of 1mm-3mm. Selecting metal Mo or Nb as a heating element can meet the basic requirements of obtaining a high temperature of up to 1600℃. At the same time, the absorption and scattering of neutrons are weaker than that of Ni, the main element in the high-temperature alloy, which is conducive to obtaining neutron signals. In addition, metal Mo or Nb has better high-temperature strength and durability than other high-melting-point metals. The heating element is the most important component of the single crystal growth system. The incident neutron beam needs to pass through the Mo or Nb tube without holes to irradiate the alumina membrane shell and the innermost single crystal high-temperature alloy. The diffraction beam neutrons generated by the single crystal high-temperature alloy also need to pass through the alumina membrane shell and the cylindrical Mo or Nb heating element and then reach the mid-angle detector through the diffraction window. The purpose of the cylindrical and non-perforated design is to prevent the area where the single crystal high-temperature alloy is located from generating large temperature fluctuations due to thermal radiation, thereby affecting the growth conditions of the single crystal.

[0055] 4. In order to minimize the lateral temperature gradient of the upper and lower heating elements, a heat preservation layer design made of six layers of metal Mo or Nb tubes coaxial with the heating element is adopted, and the adjacent heat preservation elements are separated by a spacing of 2mm-5mm to ensure that the heat transfer between the heat preservation layers is thermal radiation. In order to reduce the absorption and interference of the neutron beam, circular through holes are opened on the front and back of the lower heat preservation element near the bottom, and rectangular through holes are opened on both sides of the lower heat preservation element near the bottom. The central axis height of all through holes is kept consistent. These through holes serve as barrier-free passages for neutron incidence, transmission and diffraction, respectively, and their sizes increase proportionally from the innermost to the outermost heat preservation layer, and the sizes of the neutron incidence window, transmission window and diffraction windows on both sides opened on the vacuum diffraction chamber cavity increase proportionally from the inside to the outside, forming a conical neutron incidence passage and transmission passage and a pyramidal neutron diffraction passage. These passages are necessary conditions for obtaining the neutron diffraction signals required for in-situ diagnosis. The upper heating element and the upper insulation layer are coaxially arranged with the lower heating element and the lower heating element, and the upper and lower heating elements and the upper and lower insulation layers are separated by a circular alumina ceramic partition with a central hole, and the partition has both thermal insulation and electrical insulation functions.

[0056] 5. A cylindrical pull-out rod is provided in the single crystal growth system for neutron diffraction. The pull-out rod is connected to a ceramic crucible containing a single crystal high-temperature alloy rod through a three-section cylindrical connector made of metal Mo or Nb, wherein the outer diameter of the top of the connector is the same as the inner diameter of the ceramic crucible, the outer diameter of the middle of the connector is the same as the outer diameter of the pull-out rod, and the outer diameter of the bottom of the connector is the same as the inner diameter of the blind hole opened at the top of the pull-out rod. The pull-out rod is made of 304 or 316L stainless steel, with a blind hole at the top, a flange and a screw hole for fixing at the bottom, and an O-type rubber ring is used to achieve vacuum sealing. The maximum stroke of the pull-out rod is 80mm, and its pull-out rate is controlled by a stepping linear motor, and the value can be preset in up to eight stages within the range of 0.06mm / min -60mm / min.

[0057] 6. During directional solidification, the growth direction of dendrites is parallel to the direction of heat flow, but the crystallographic direction of dendrites in the plane perpendicular to the heat flow has a certain randomness. In order to ensure that a sufficiently strong neutron diffraction signal is obtained in the mid-angle detector during directional solidification, the sample needs to be properly rotated around the growth direction of the single crystal high-temperature alloy when necessary. This rotation is achieved by a rotary motor installed on the pull rod, and the rotation angle is adjustable in the range of ±180º.

[0058] 7. The connection of various parts of the vacuum system is controlled by pneumatic valves, the power supply of the mechanical pump and molecular pump is controlled by digital control methods, the vacuum degree at a specific position in the vacuum chamber is monitored by a digital composite vacuum gauge, the heating power and insulation time of the upper and lower heating elements are controlled by a PLC program controller, and 10 sets of thermocouples are used to detect the local temperature of the single crystal growth system, and the signals are converted into digital signals and integrated through network cables to the touch-screen console of the integrated control system, which are used for real-time display, program control and manual intervention of the vacuum system, single crystal growth system and fault alarm. Two sets of thermocouples are used to control the heating temperature settings of the upper and lower heating elements.

[0059] 8. Based on the neutron diffraction signals detected by the medium angle detector installed on the neutron source (neither the neutron source nor the neutron detector belongs to the scope of the present invention), the directional solidification process of the single crystal high temperature alloy is diagnosed in situ. When the orientation of the columnar dendrites deviates, a diffraction spot with a continuously changing position will be generated on the detector. When the columnar dendrites undergo plastic deformation, the diffraction spots on the detector will increase in area and decrease in intensity. When recrystallization occurs in the columnar dendrites after plastic deformation, multiple sets of diffraction spots will be detected on the detector. When macroscopic stress appears in the columnar dendrites, it will appear as a displacement of the diffraction spots on the detector. When striped crystals appear in the single crystal high temperature alloy rod, the detector will detect diffraction spots whose interplanar spacing and crystallographic orientation are different from those of the columnar dendrites in the surrounding trunk area. These spots will appear continuously at a certain stage of directional solidification. Based on the correlation between the changes in diffraction spots and growth defects, real-time diagnosis of the directional solidification process of single-crystal high-temperature alloys can be achieved in situ and at the minute level, and continuous analysis can be made to analyze the conditions for the occurrence and duration of defects, thereby providing technical data for process optimization and innovative design in industrial production.

[0060] 9. The diagnostic system and method involved in the present invention are not limited to the directional solidification process of single crystal high-temperature alloys. In addition, they can also be used for the real-time diagnosis of the structural evolution during the heat treatment process of high-temperature alloys and other medium- and high-melting-point metals or alloys solidification and heat treatment processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 A schematic diagram of the connection of an in-situ diagnostic system for a single crystal high-temperature alloy directional solidification process provided by the present invention;

[0062] Figure 2 It is an enlarged schematic diagram of the connection between the vacuum unit and the vacuum chamber in the present invention;

[0063] Figure 3 This is a structural diagram of the vacuum environment system for neutron diffraction in the present invention;

[0064] Figure 4 This is a structural diagram of the heating element and the thermal insulation layer of the directional solidification single crystal growth system of the present invention;

[0065] Figure 5 It is a structural diagram of the neutron diffraction path of the vacuum chamber and the heating element in the present invention;

[0066] Figure 6 It is a structural diagram of the directional solidification single crystal growth system in the present invention;

[0067] Figure 7 It is the structural diagram of the comprehensive control system in the present invention;

[0068] Figure 8The diffraction spectrum of the DD6 single crystal high temperature alloy detected by the single module of the angle detector during the directional solidification process in the test results of the embodiment;

[0069] in:

[0070] 1-Pump body support, 2-rotary vane vacuum pump, 3-solenoid valve, 4-turbo molecular pump, 5-vacuum gate valve, 6-bypass, 7-bellows vertical support frame, 8-large diameter bellows, 9-bellows horizontal support frame, 10-resistance vacuum gauge, 11-ionization vacuum gauge, 12-vacuum chamber, 13-movable vacuum chamber top cover, 14-pneumatic plug rod for melt pouring, 15-upper heating element electrode I, 16-lower heating element electrode I, 17-upper heating element electrode II, 18-lower heating element electrode II, 19-upper heating element temperature control thermocouple, 20-neutron incident window, 21-air release valve, 22-left neutron diffraction window, 23-right neutron diffraction window, 24-sample rotation mechanism, 25-sample up and down pulling mechanism, 26-vacuum chamber bracket, 27-cooling water pipe, 28-chiller, 29-cooling water row, 30-charging port, 31-temperature control thermocouple connecting wire, 32-temperature measurement thermocouple connecting wire, 33-heating power supply control cabinet, 34-sensor connecting wire, 35-touch control screen, 36-integrated control system;

[0071] 2-1- vacuum chamber support rod, 2-2- vacuum chamber bottom plate, 2-3- temperature measuring thermocouple insertion port I, 2-4- temperature measuring thermocouple insertion port II, 2-5- vacuum chamber top cover water inlet, 2-6- melt pouring pneumatic plugging system interface, 2-7- vacuum chamber top cover water outlet, 2-9- temperature measuring thermocouple insertion port III, 2-10- temperature measuring thermocouple insertion port IV; 2-11- pull rod insertion port; 2-12- connecting pipe;

[0072] 3-1-heating element support frame, 3-2-lower heating element insulation bottom plate, 3-3-six-layer parallel insulation bottom plate, 3-4-lower heating element fastening rivet, 3-5-lower heating element lead electrode insulation sleeve, 3-6-upper heating element six-layer coaxial insulation cylinder, 3-7-upper heating element lead electrode insulation sleeve, 3-8-six-layer parallel insulation top cover, 3-9-top handle, 3-10-insulation layer top cover support rod, 3-11-upper heating element electrode fixing frame, 3-12-upper heating element thermocouple insertion port, 3-13-upper heating element heating cylinder, 3-14-lower heating element electrode fixing frame, 3-15-lower heating element thermocouple insertion port, 3-16-lower heating element heating cylinder, 3-17-insulation layer bottom plate support rod; 3-18-alumina ceramic insulation baffle;

[0073] 4-1-conical neutron incident through hole, 4-2-left pyramidal 90° neutron diffraction through hole, 4-3-pyramidal neutron transmission through hole, 4-4-right pyramidal 90° neutron diffraction through hole; 4-5-neutron transmission window;

[0074] 5-1-pull rod, 5-2-liquid metal cooling tank, 5-3-ceramic crucible, 5-4-funnel-shaped chemical pool, 5-5-movable vacuum chamber top cover fixing screws;

[0075] 6-1-cabinet, 6-2-lower heating element temperature control meter, 6-3-upper heating element temperature control meter, 6-4-molecular pump tachometer, 6-5-resistance vacuum gauge, 6-7-ionization gauge, 6-8-upper heating element voltmeter, 6-9-upper heating element ammeter, 6-10-lower heating element voltmeter, 6-11-lower heating element ammeter. DETAILED DESCRIPTION

[0076] In order to better explain the present invention and facilitate understanding, the technical solutions and effects of the present invention are described in detail below through specific implementation modes in conjunction with the accompanying drawings.

[0077] In order to realize neutron in-situ and real-time diagnosis of the directional solidification process of single crystal superalloy based on neutron diffraction, three essential conditions need to be created. The specific conditions include:

[0078] (1) The vacuum degree is 0.0001Pa-1Pa vacuum environment, which is used to protect single crystal high-temperature alloys from oxidation during heating, melting and cooling;

[0079] (2) High temperature environment with precise temperature control (the maximum temperature of the upper and lower heating elements can reach 1600°C), and the temperature control accuracy can reach ±3°C;

[0080] (3) Remote control is used to meet the operator's need to avoid neutron radiation in a remote control room far away from the directional solidification site through modern communication technology to start, shut down and monitor the vacuum and high-temperature environment in real time.

[0081] When designing the above system, special mechanism design is required to meet the basic requirements of directional solidification of single crystal high temperature alloy in vacuum, and also consider the attenuation and absorption of neutrons by mechanical mechanism, control mechanism, sensor, etc., and reduce the interference to neutron detector. The specific considerations are as follows:

[0082] (1) When designing a vacuum system, it is necessary to consider opening neutron incident windows, diffraction windows, and transmission windows on the front, side, and back of the vacuum chamber. The materials of these windows must absorb neutrons as little as possible and not generate additional stray signals while meeting the vacuum sealing condition. In addition, the vacuum chamber needs to be forced to cool, on the one hand to ensure the sealing of the vacuum chamber, and on the other hand to ensure the thermal radiation of the vacuum chamber to the neutron detector.

[0083] (2) When designing the heating system, it is necessary to consider materials with high temperature strength, resistance to neutron irradiation and low neutron absorption to make the heating elements used for melting and temperature gradient control. At the same time, it is necessary to consider opening up neutron incidence, diffraction and transmission channels in the design of the insulation layer. In order to achieve the temperature gradient G in the longitudinal direction required for directional solidification, an upper heating element and a lower heating element are set up, and the upper and lower heating elements are insulated and electrically insulated by an alumina ceramic partition.

[0084] (3) When designing a remote control system, it is necessary to consider the layout of sensors away from the incident, diffraction, and transmission paths of the neutron beam. At the same time, a programmable touch-screen monitoring interface should be used to display and control the status and parameters of the vacuum system and single crystal growth system in real time, and alarms should be issued for abnormal signals to remind operators to make necessary interventions to ensure the safe operation of the neutron source facility.

[0085] Based on the above considerations, the present invention provides a neutron in-situ diagnostic system and method for the directional solidification process of a single crystal high-temperature alloy, such as Figure 1-7 As shown, a neutron in-situ diagnostic system for a single crystal high-temperature alloy directional solidification process comprises: a vacuum environment system suitable for carrying out time-of-flight neutron in-situ diffraction, a single crystal growth system and an integrated control system 36.

[0086] The vacuum environment system includes a vacuum chamber 12, a vacuum unit and a vacuum measurement system, a neutron passage, and a cooling water subsystem. The neutron passage is arranged on the cavity of the vacuum diffraction chamber. The vacuum chamber 12 is a stainless steel cylindrical vacuum chamber with a water-cooled double-layer structure, fixed on a vacuum chamber bracket 26, a vacuum chamber support rod 2-1 is connected to the bottom of the vacuum chamber bottom plate 2-2, and the vacuum chamber support rod 2-1 is fixed on the vacuum chamber bracket 26. The top of the vacuum chamber 12 is a movable vacuum chamber top cover 13, which is connected and fixed by a movable vacuum chamber top cover fixing screw 5-5; the movable vacuum chamber top cover 13 is provided with a vacuum chamber top cover water inlet 2-5 and a vacuum chamber top cover water outlet 2-7. The neutron passage includes a neutron incident window 20, a neutron diffraction window and a neutron transmission window 4-5. The neutron incident window 20 is made of a vanadium-nickel alloy that is transparent to neutrons, has a circular shape, and is arranged at the position where the neutron beam enters the vacuum chamber 12; the neutron diffraction window is made of an aluminum alloy with low neutron absorption, has a square shape, and is arranged on the side wall of the vacuum chamber 12 at a 90° angle to the incident neutron beam. There are two of them, which are arranged oppositely, namely the left neutron diffraction window 22 and the right neutron diffraction window; the neutron transmission windows 4-5 are made of a vanadium-nickel alloy that is transparent to neutrons, have a square shape, and are arranged on the vacuum chamber 12 facing the neutron incident window 20.

[0087] The side wall of the vacuum chamber 12 is provided with six thermocouple insertion ports for inserting thermocouples, namely, temperature measuring thermocouple insertion port I 2-3, temperature measuring thermocouple insertion port II 2-4, temperature measuring thermocouple insertion port III 2-9, temperature measuring thermocouple insertion port IV 2-10, lower heating element temperature control thermocouple insertion port, and upper heating element temperature control thermocouple insertion port.

[0088] A loading port 30 is disposed at the upper portion of the vacuum chamber 12 .

[0089] The movable vacuum chamber top cover 13 is provided with a pneumatic plugging system interface 2-6 for melt pouring in the middle, which is used to insert the pneumatic plugging rod 14 for melt pouring and is electrically connected to the integrated control system 36; the vacuum chamber bottom plate 2-2 is provided with a pull rod insertion port 2-11 for directional solidification in the middle.

[0090] The vacuum unit includes a rotary vane vacuum pump 2 fixed by a pump body bracket 1, a solenoid valve 3 is installed between the rotary vane vacuum pump 2 and the turbomolecular pump 4, the turbomolecular pump 4 is connected to the connecting pipe 2-12 welded on the vacuum chamber 12 through a large-diameter bellows 8, and is connected to the inside of the vacuum chamber 12 for vacuuming; the ionization vacuum gauge 11 and the resistance vacuum gauge 10 are connected to the connecting pipe 2-12 through a standard flange interface to form a vacuum measurement system. A venting valve 21 is arranged on the connecting pipe 2-12. A bellows horizontal support frame 9 and a bellows vertical support frame 7 are arranged outside the large-diameter bellows 8. A bypass 6 is arranged between the solenoid valve 3 and the turbomolecular pump 4, and a vacuum gate valve 5 is arranged on the turbomolecular pump 4. A temperature sensor is arranged inside the vacuum chamber 12, and is electrically connected to the integrated control system 36 through a sensor connection line 34.

[0091] The cooling water subsystem includes a water chiller 28, which is connected to the middle cavity of the double wall of the vacuum chamber 12, the flange at the temperature measuring thermocouple insertion port, the flange at the upper heating element electrode and the lower heating element electrode, the turbomolecular pump 4, and the movable vacuum chamber top cover 13 through a cooling water row 29 and a cooling water pipe 27, so as to cool down the neutron incident window 20, the left neutron diffraction window 22, the right neutron diffraction window 23, the neutron transmission windows 4-5, the middle cavity of the vacuum chamber 12, and the turbomolecular pump 4. The cooling water circulates in the middle cavity of the double wall of the vacuum chamber 12 to achieve the purpose of cooling.

[0092] The single crystal growth system is provided with a heating element and a heat preservation layer, a funnel-shaped chemical material pool 5-4, a sample rotating mechanism 24, a sample upper and lower pulling mechanism 25, and a liquid metal cooling tank 5-2, wherein the heating element, the heat preservation layer, and the funnel-shaped chemical material pool 5-4 are placed in the vacuum chamber 12, and the sample rotating mechanism 24, the sample upper and lower pulling mechanism 25, and the liquid metal cooling tank 5-2 are placed outside the vacuum chamber 12. The liquid metal cooling tank 5-2 is a 304 stainless steel tank containing liquid metal.

[0093] The heating element in the single crystal growth system serves as a heating and temperature control mechanism, including an upper heating element, an upper insulation layer, a lower heating element and a lower insulation layer. The upper heating element and the lower heating element are coaxially arranged, and the upper insulation layer and the lower insulation layer are coaxially arranged. The upper heating element is a melting furnace with the highest temperature, the heating temperature is 1600°C, and the temperature control accuracy is ±3°C. The lower heating element is a insulation furnace with a maximum insulation temperature of 1500°C and a temperature control accuracy of ±3°C.

[0094] The single crystal growth system includes a heating element support frame 3-1 fixed on the bottom plate 2-2 of the vacuum chamber, the lower heating element is arranged on the heating element support frame 3-1, an alumina ceramic insulation baffle 3-18 is placed on the top, and the upper heating element is coaxially arranged above the ceramic baffle. The upper insulation layer and the upper heating element, the lower heating element and the lower insulation layer are composed of seven layers of cylinders with different diameters. The innermost layer is the heating element heating cylinder, the upper part is the upper heating element heating cylinder 3-13, and the remaining six layers are insulation layers, with a spacing of 2mm-5mm between adjacent layers, and the lower part is the lower heating element heating cylinder; the remaining six layers are insulation layers, with a spacing of 2mm-5mm between adjacent layers. The alumina ceramic insulation baffle 3-18 has a central opening and is coaxial with the heating element and the insulation layer. The outside of the upper heating element heating cylinder 3-13 is the upper heating element six-layer coaxial insulation cylinder 3-6, and the outside of the lower heating element heating cylinder 3-16 is the lower heating element six-layer coaxial insulation cylinder. The bottom of the lower heating element heating cylinder 3-16 is fixed by the lower heating element fastening rivet 3-4.

[0095] The side wall of the upper heating element heating cylinder 3-13 is provided with two upper heating element thermocouple insertion ports 3-12, and the upper heating element heating cylinder 3-13 is provided with an upper heating element electrode I 15 and an upper heating element electrode II 17, wherein the upper heating element electrode I 15 is the access end, and the upper heating element electrode II 17 is the access end, which is fixed by the upper heating element electrode fixing frame 3-11. The upper heating element electrode I 15 is externally sleeved with an upper heating element lead-in electrode insulating sleeve, and the upper heating element electrode II 17 is externally sleeved with an upper heating element lead-out electrode insulating sleeve 3-7. The side wall of the lower heating element heating cylinder 3-16 is provided with three lower heating element thermocouple insertion ports 3-15, and the lower heating element heating cylinder 3-16 is provided with a lower heating element electrode I 16 and a lower heating element electrode II 18, wherein the lower heating element electrode I 16 is the access end, and the lower heating element electrode II 18 is the access end, which is fixed by the lower heating element electrode fixing frame 3-14. The lower heating element electrode I16 is externally sheathed with a lower heating element lead-in electrode insulating sleeve, and the lower heating element electrode II18 is externally sheathed with a lower heating element lead-out electrode insulating sleeve 3-5. The upper heating element electrode I15, the lower heating element electrode I16, the upper heating element electrode II17 and the lower heating element electrode II18 extend outward to the side wall of the vacuum chamber 12 and are electrically connected to the heating power supply control cabinet 33.

[0096] The upper heating element temperature control thermocouple 19 of the upper heating element thermocouple insertion port 3-12 is electrically connected to the heating power supply control cabinet 33 through the temperature control thermocouple connecting wire 31 passing through the upper heating element temperature control thermocouple insertion port on the side wall of the vacuum chamber 12, and the lower heating element temperature control thermocouple of the lower heating element thermocouple insertion port 3-15 is electrically connected to the heating power supply control cabinet 33 through the connecting wire passing through the lower heating element temperature control thermocouple insertion port on the side wall of the vacuum chamber 12.

[0097] The temperature measuring thermocouples installed at the temperature measuring thermocouple insertion ports I 2-3, II 2-4, III 2-9 and IV 2-10 on the side wall of the vacuum chamber 12 are electrically connected to the heating power supply control cabinet 33 via the temperature measuring thermocouple connecting wire 32.

[0098] The heating power supply control cabinet 33 is electrically connected to the integrated control system 36 .

[0099] The top of the upper heating element heating cylinder 3-13 is the top of the insulation layer, which is a six-layer parallel insulation top cover 3-8 corresponding to the six insulation layers respectively. The six-layer parallel insulation top cover 3-8 is provided with an insulation layer top cover support rod 3-10 for support and fixation, and the top insulation board is provided with an upper top handle 3-9. The bottom of the lower heating element heating cylinder 3-16 is provided with six layers of parallel insulation bottom plates 3-3 corresponding to the six insulation layers respectively. The six layers of parallel insulation bottom plates 3-3 are provided with insulation layer bottom plate support rods 3-17 for support and fixation. A lower heating element insulation bottom plate 3-2 is provided between the bottom of the six layers of parallel insulation bottom plates 3-3 and the heating element support frame 3-1. The upper and lower heating elements and the upper and lower insulation layers are separated by an alumina ceramic insulation baffle 3-18 with a central opening to achieve electrical insulation between the upper and lower heating cylinders.

[0100] The lower part of the lower insulation layer cylinder outside the lower heating element is provided with through holes for neutron incidence, transmission and two-way diffraction, as well as thermocouple installation channels and electrode connection channels. The bottom of the lower heating element heating cylinder 3-16 is not provided with holes. The sizes of the through holes increase proportionally from the innermost layer to the outermost layer, thereby forming a conical through hole from the inside to the outside, specifically a conical neutron incidence through hole 4-1, a left-side pyramidal 90° neutron diffraction through hole 4-2, a pyramidal neutron transmission through hole 4-3, and a right-side pyramidal 90° neutron diffraction through hole 4-4.

[0101] The lower heating element heating cylinder 3-16 is provided with a coaxial ceramic crucible 5-3 inside, and the top of the ceramic crucible 5-3 is arranged opposite to the funnel-shaped chemical pool 5-4 in the upper heating element heating cylinder 3-13; the top of the vacuum chamber 12 is provided with a pneumatic plug rod 14 for melt pouring, which penetrates from the outside into the bottom of the funnel-shaped chemical pool 5-4 in the upper heating element heating cylinder 3-13, and is used for sealing between the funnel-shaped chemical pool 5-4 and the ceramic crucible 5-3. The bottom pouring method is adopted, and the melt enters through the funnel-shaped chemical pool 5-4, which serves as an alumina membrane shell for growing high-temperature alloy single crystals.

[0102] The sample up and down pulling mechanism 25 includes a pulling rod 5-1, the top of which passes through the liquid metal cooling tank 5-2 and is connected to the ceramic crucible 5-3 through a molybdenum joint, one end of which is inserted into the interior of the ceramic crucible 5-3, and the other end is inserted into the interior of the pulling rod 5-1; the bottom of the pulling rod 5-1 is connected to a slide seat, and the slide seat moves up and down on the pulling rod guide rail, the pulling rod guide rail is connected to the pulling rod drive motor, and the pulling rod guide rail is fixed to the vacuum chamber bracket 26 through the pulling rod guide rail bracket. The pulling rod drive motor rotates, driving the pulling rod guide rail to rotate, and then driving the slide seat together with the pulling rod 5-1 and the ceramic crucible 5-3 to move up and down along the pulling rod guide rail.

[0103] The end of the pulling rod 5 - 1 is provided with a sample rotating mechanism 24 , which includes a motor. The pulling rod 5 - 1 is connected to the output end of the motor, so that the pulling rod 5 - 1 can rotate around its own axis.

[0104] The sample up and down pulling mechanism 25 and the sample rotating mechanism 24 are electrically connected to the integrated control system 36. The programmable logic controller (PLC) unit of the integrated control system 36 is used to control the uniform or variable speed up and down movement of the pulling rod 5-1 and the rotation around the central axis. The pulling rate is adjustable within the range of 0.1mm / min-60mm / min, the maximum stroke is 80mm, and the rotation angle is ±180°.

[0105] The integrated control system 36 includes a programmable logic controller (PLC), which serves as a main console. An interactive human-machine control interface, i.e., a touch control screen 35, is installed on the top of the cabinet 6-1, which is used to realize remote control of the vacuum environment system, remote control of the temperature sensor in the vacuum chamber 12, and remote control of the single crystal growth pull rod 5-1. The front of the programmable logic controller (PLC) is provided with a lower heating element temperature control meter 6-2, an upper heating element temperature control meter 6-3, a molecular pump speed meter 6-4, a resistance vacuum gauge 6-5, a detachable remote touch control screen 35, an ionization gauge 6-7, an upper heating element voltage meter 6-8, an upper heating element current meter 6-9, a lower heating element voltage meter 6-10, and a lower heating element current meter 6-11.

[0106] Neutrons enter the vacuum chamber 12 from the incident window on the front side of the vacuum chamber 12, and are irradiated onto the heating element, the ceramic crucible 5-3 filled with alloy melt, and the single crystal high-temperature alloy inside thereof through the through holes opened on the thermal insulation layer, causing diffraction and transmission. Two diffraction beams with an angle of 90° with the incident beam reach the medium-angle detector from the diffraction windows on the left and right sides of the vacuum chamber 12, and at the same time, the transmitted neutron beam reaches the low-angle detector through the transmission window on the back side of the vacuum chamber.

[0107] A neutron in-situ diagnosis method for a single crystal high temperature alloy directional solidification process is carried out by using the neutron in-situ diagnosis system for a single crystal high temperature alloy directional solidification process, and specifically comprises the following steps.

[0108] Step 1: Prepare the materials. Put the raw materials into the funnel-shaped material pool 5-4 according to the proportion.

[0109] Step 2: Evacuate. Using the touch control screen 35 of the integrated control system 36, start the vacuum unit consisting of the rotary vane vacuum pump 2 and the turbomolecular pump 4 to evacuate the vacuum chamber 12 of the neutron diffraction vacuum system until the pressure in the vacuum chamber 12 is lower than a specified value.

[0110] Step 3: Melting. The heating element in the single crystal growth system is powered by the touch control screen 35 of the integrated control system 36, and the raw materials in the funnel-shaped material pool 5-4 are heated and melted into alloy liquid according to the preset heating program and steps.

[0111] Step 4: Pouring and temperature gradient control. With the help of the touch control screen 35 of the integrated control system 36, the pneumatic plug rod 14 for melt pouring is lifted, and the melt enters the ceramic crucible 5-3, which is the alumina membrane shell for growing high-temperature alloy single crystals, through the funnel-shaped material pool 5-4. The temperature and temperature gradient of the upper and lower heating elements are adjusted by remotely controlling the heating power supply control cabinet 33 through the integrated control system 36. The temperature of the lower heating element area is controlled by the liquid metal in the liquid metal cooling tank 5-2. Keep warm for 5 minutes to 10 minutes until the temperature is stable.

[0112] Step 5: Directional solidification. With the help of the touch control screen 35 of the integrated control system 36, the pull rod 5-1 of the single crystal growth system is started, and the alumina film shell containing the single crystal high-temperature alloy melt is pulled down at a constant speed or a variable speed according to the preset program to make the alloy melt directionally solidified.

[0113] Step 6: During the directional solidification process, a neutron beam is introduced through the incident window, and then irradiates the alumina membrane shell and the high-temperature alloy in the solidification stage after passing through the heating element. The neutron diffraction signal generated in the 90° direction passes through the heating element, and then exits from the left neutron diffraction window 22 and the right neutron diffraction window and reaches the mid-angle detectors on both sides. By analyzing the flight time, wavelength, intensity and position information of the neutron signal received on the detector, the deviation of the single crystal orientation, the decrease of the crystallization integrity of the single crystal, and the appearance of defects such as streaky crystals and recrystallization during the directional solidification of the single crystal high-temperature alloy are diagnosed in real time.

[0114] The above system was installed in a certain location and the energy-resolved imaging spectrometer of the Spallation Neutron Source Science Center was used to conduct in-situ diagnosis of the directional solidification process of single crystal high-temperature alloy. The test conditions are as follows:

[0115] Single crystal high temperature alloy grade: DD6 single crystal high temperature alloy;

[0116] Vacuum degree: The vacuum unit reaches 0.006Pa within 30 minutes after startup;

[0117] Heating temperature: heat to 800℃ within 30 minutes, keep warm for 10 minutes; heat to 1200℃ within 20 minutes, keep warm for 10 minutes; heat to 1500℃ within 10 minutes;

[0118] Melting temperature and time: 1500℃, keep warm for 30 min;

[0119] Upper heating furnace temperature: 1500℃;

[0120] Lower heating furnace temperature: 1300℃;

[0121] Pulling rate: 0.48 mm / min;

[0122] Pulling stroke: 30 mm;

[0123] Pulling time: 62.5 min.

[0124] The diffraction spectrum of a single module of the angle detector in the test results is as follows: Figure 8 As shown, the tests indicate that the facilities of the various subsystems and neutron sources are compatible and can meet the technical requirements for neutron in-situ diagnosis of the directional solidification process of single crystal high-temperature alloys.

Claims

1. A neutron in-situ diagnostic system for the directional solidification process of a single crystal high-temperature alloy, characterized in that: It includes a vacuum environment system suitable for time-of-flight neutron in-situ diffraction, a single crystal growth system and a comprehensive control system for controlling the vacuum environment system and the single crystal growth system; The vacuum environment system comprises a vacuum chamber, a vacuum unit and a vacuum measurement system for evacuating the vacuum chamber, a neutron passage, and a cooling water subsystem for cooling. The neutron passage is arranged on the cavity of the vacuum chamber; the neutron passage comprises a neutron incident window, a neutron diffraction window, and a neutron transmission window. The neutron incident window is made of a vanadium-nickel alloy transparent to neutrons, the neutron diffraction window is made of an aluminum alloy with low absorption to neutrons, and is arranged on a side wall of the vacuum chamber at a direction of 90° to the incident neutron beam, and the neutron transmission window is made of a vanadium-nickel alloy transparent to neutrons, and is arranged on a side wall of the vacuum chamber directly facing the neutron incident window; The vacuum chamber has a water-cooled double-layer structure; The single crystal growth system is provided with a heating element and a heat preservation layer, a funnel-shaped chemical material pool, a sample rotating mechanism, a sample upper and lower pulling mechanism and a liquid metal cooling tank, wherein the heating element, the heat preservation layer and the funnel-shaped chemical material pool are placed inside a vacuum chamber, and the sample rotating mechanism, the sample upper and lower pulling mechanism and the liquid metal cooling tank are placed outside the vacuum chamber; The heating element in the single crystal growth system comprises an upper heating element, an upper thermal insulation layer, a lower heating element and a lower thermal insulation layer, wherein the upper heating element and the lower heating element are coaxially arranged, and the upper thermal insulation layer and the lower thermal insulation layer are coaxially arranged; and further comprises a circular alumina ceramic thermal insulation baffle having a central opening and being coaxial with the heating element and the thermal insulation layer, wherein the circular alumina ceramic thermal insulation baffle is placed on the top of the lower heating element, and the upper heating element and the upper thermal insulation layer are placed on the circular alumina ceramic thermal insulation baffle; The upper insulation layer and the upper heating element are composed of seven layers of cylinders with different diameters, the innermost layer is the upper heating element heating cylinder, and the remaining six layers are the upper insulation layer; the lower insulation layer and the lower heating element are composed of seven layers of cylinders with different diameters, the innermost layer is the lower heating element heating cylinder, and the remaining six layers are the lower insulation layer; A coaxial ceramic crucible is arranged inside the lower heating element heating cylinder, and the top of the ceramic crucible is arranged opposite to the funnel-shaped chemical pool in the upper heating element heating cylinder; a pneumatic plugging rod for melt pouring is arranged on the top of the vacuum chamber, which penetrates from the outside into the bottom of the funnel-shaped chemical pool in the upper heating element heating cylinder; The sample up and down pulling mechanism includes a pulling rod, the top of the pulling rod passes through the liquid metal cooling tank and is connected to the ceramic crucible through a molybdenum joint, one end of the molybdenum joint is inserted into the ceramic crucible, and the other end is inserted into the pulling rod; the bottom of the pulling rod is connected to the slide seat, the slide seat moves up and down on the pulling rod guide rail, the pulling rod guide rail is connected to the pulling rod drive motor, and the pulling rod guide rail is fixed to the vacuum chamber bracket through the pulling rod guide rail bracket; A sample rotating mechanism is arranged at the end of the pulling rod. The sample rotating mechanism comprises a motor. The pulling rod is connected to the output end of the motor.

2. The neutron in-situ diagnostic system for the directional solidification process of a single crystal high-temperature alloy according to claim 1, characterized in that: The neutron incident window is circular in shape and is arranged at the position where the neutron beam enters the vacuum chamber; the neutron diffraction window is square in shape, and there are two of them, which are arranged oppositely, namely the left neutron diffraction window and the right neutron diffraction window; the neutron transmission window is square in shape; A loading port is provided at the upper part of the vacuum chamber; A thermocouple insertion port is provided on the side wall of the vacuum chamber, and a temperature-controlling thermocouple and a temperature-measuring thermocouple are installed thereon, which are electrically connected to a heating power supply control cabinet, and the heating power supply control cabinet is electrically connected to an integrated control system.

3. The neutron in-situ diagnostic system for the directional solidification process of a single crystal high-temperature alloy according to claim 2, characterized in that: The vacuum chamber is a stainless steel cylindrical vacuum chamber, which is fixed on a vacuum chamber bracket. A vacuum chamber support rod is connected to the bottom of the vacuum chamber bottom plate, and the vacuum chamber support rod is connected and fixed to the vacuum chamber bracket; the top of the vacuum chamber is a movable vacuum chamber top cover, which is connected and fixed by the movable vacuum chamber top cover fixing screws.

4. The neutron in-situ diagnostic system for the directional solidification process of a single crystal high-temperature alloy according to claim 2, characterized in that: The vacuum unit includes a rotary vane vacuum pump fixed by a pump body bracket, an electromagnetic valve is installed between the rotary vane vacuum pump and the turbomolecular pump, the turbomolecular pump is connected to the connecting pipe welded on the vacuum chamber through a large-diameter bellows, and is communicated with the interior of the vacuum chamber, and an ionization vacuum gauge, a resistance vacuum gauge and a venting valve are arranged on the connecting pipe; a bellows horizontal support frame and a bellows vertical support frame are arranged outside the large-diameter bellows; a bypass is arranged between the electromagnetic valve and the turbomolecular pump, and a vacuum gate valve is arranged on the turbomolecular pump; a temperature sensor is arranged inside the vacuum chamber.

5. The neutron in-situ diagnostic system for the directional solidification process of a single crystal high-temperature alloy according to claim 2, characterized in that: The cooling water subsystem includes a chiller, which is connected to the middle cavity of the double wall of the vacuum chamber, the flange at the temperature measuring thermocouple insertion port, the flange at the upper heating element electrode and the lower heating element electrode, the turbomolecular pump, and the movable vacuum chamber top cover through a cooling water row and a cooling water pipe, so as to cool the neutron incident window, the left neutron diffraction window, the right neutron diffraction window, the neutron transmission window, the middle cavity of the vacuum chamber and the turbomolecular pump; the cooling water circulates in the middle cavity of the double wall of the vacuum chamber to achieve the purpose of cooling.

6. The neutron in-situ diagnostic system for the directional solidification process of a single crystal high-temperature alloy according to claim 2, characterized in that: The liquid metal cooling tank is a 304 stainless steel tank containing liquid metal.

7. The neutron in-situ diagnostic system for the directional solidification process of a single crystal high-temperature alloy according to claim 6, characterized in that: It also includes a heating element support frame fixed on the bottom plate of the vacuum chamber, and the lower heating element is arranged on the heating element support frame; the upper insulation layer and the upper heating element have a spacing of 2mm-5mm between adjacent layers; the lower insulation layer and the lower heating element have a spacing of 2mm-5mm between adjacent layers; The top of the upper heating element heating cylinder is the top of the insulation layer, which is a six-layer parallel insulation top cover corresponding to the six insulation layers respectively, and the six-layer parallel insulation top cover is provided with an insulation layer top cover support rod for support and fixation, and the top insulation board is provided with an upper top handle; the bottom of the lower heating element heating cylinder is provided with six layers of parallel insulation bottom plates corresponding to the six insulation layers respectively, and the six layers of parallel insulation bottom plates are provided with insulation layer bottom plate support rods for support and fixation; a lower heating element insulation bottom plate is provided between the bottom of the six layers of parallel insulation bottom plates and the heating element support frame; The lower part of the lower insulation layer outside the lower heating element is provided with through holes for neutron incidence, transmission and two-way diffraction, as well as thermocouple installation channels and electrode connection channels. The bottom of the heating tube of the lower heating element is not provided with holes. The sizes of the through holes increase proportionally from the innermost layer to the outermost layer, thereby forming a conical through hole from the inside to the outside.

8. The neutron in-situ diagnostic system for the directional solidification process of a single crystal high-temperature alloy according to claim 7, characterized in that: The side wall of the upper heating body heating cylinder is provided with a plurality of upper heating body thermocouple insertion ports, and the upper heating body heating cylinder is provided with an upper heating body electrode I and an upper heating body electrode II, wherein the upper heating body electrode I is the access end, and the upper heating body electrode II is the access end; the upper heating body electrode I is externally sleeved with an upper heating body introduction electrode insulating sleeve, and the upper heating body electrode II is externally sleeved with an upper heating body lead-out electrode insulating sleeve; the side wall of the lower heating body heating cylinder is provided with a plurality of lower heating body thermocouple insertion ports, and the lower heating body heating cylinder is provided with a lower heating body electrode I and a lower heating body electrode II, wherein the lower heating body electrode I is the access end, and the lower heating body electrode II is the access end; the lower heating body electrode I is externally sleeved with a lower heating body introduction electrode insulating sleeve, and the lower heating body electrode II is externally sleeved with a lower heating body lead-out electrode insulating sleeve; the upper heating body electrode I, the lower heating body electrode I, the upper heating body electrode II and the lower heating body electrode II extend outwardly to the side wall of the vacuum chamber and are electrically connected to the heating power supply control cabinet.

9. The neutron in-situ diagnostic system for the directional solidification process of a single crystal high-temperature alloy according to claim 8, characterized in that: The integrated control system comprises a programmable logic controller, which serves as a main console. An interactive human-machine control interface, namely a touch control screen, is installed on the top of the cabinet.

10. A neutron in-situ diagnosis method for a single crystal high temperature alloy directional solidification process, using the neutron in-situ diagnosis system for a single crystal high temperature alloy directional solidification process according to any one of claims 1 to 9, characterized in that: The specific steps include: Step 1: Prepare materials: put the raw materials into the funnel-shaped material pool according to the proportion; Step 2: Vacuuming: Using the integrated control system, start the vacuum unit consisting of a rotary vane vacuum pump and a turbomolecular pump to evacuate the vacuum chamber of the vacuum system for neutron diffraction until the pressure in the vacuum chamber is lower than the specified value; Step 3: Melting: With the help of the integrated control system, the heating element in the single crystal growth system is powered, and the raw materials in the funnel-shaped material pool are heated and melted into alloy liquid according to the preset heating program and steps; Step 4: Pouring and temperature gradient control: With the help of the integrated control system, the pneumatic plug rod for melt pouring is lifted, and the melt is passed through the funnel-shaped material pool into the ceramic crucible, which is the alumina membrane shell used to grow high-temperature alloy single crystals. The integrated control system remotely controls the heating power supply control cabinet to adjust the temperature and temperature gradient of the upper and lower heating elements. The temperature of the lower heating element area is controlled by the liquid metal in the liquid metal cooling tank. Keep warm for 5 minutes to 10 minutes until the temperature is stable. Step 5: Directional solidification: With the help of the integrated control system, the pull rod of the single crystal growth system is started, and the alumina film shell containing the single crystal high-temperature alloy melt is pulled down at a uniform or variable speed according to the preset program to make the alloy melt directionally solidified; Step six: During the directional solidification process, a neutron beam is introduced through the incident window, passes through the heating element, and then irradiates the alumina membrane shell and the high-temperature alloy in the solidification stage. The neutron diffraction signal generated in the 90° direction passes through the heating element, and then is emitted from the left neutron diffraction window and the right neutron diffraction window and reaches the mid-angle detectors on both sides; by analyzing the flight time, i.e., wavelength, intensity and position information of the neutron signal received on the detector, the deviation of the single crystal orientation, the decrease in the crystallization integrity of the single crystal, and the appearance of streak crystals and recrystallization defects that occur during the directional solidification of the single crystal high-temperature alloy are diagnosed in real time.

Citation Information

Patent Citations

  • Method for expressing gamma / gamma' phase crystal lattice mismatching degree in nickel-based high-temperature alloy

    CN104345071A

  • Single crystal stress tensor measuring method based on monochromatic X-ray diffraction

    CN110715946A

  • Method for evaluating freckle formation tendency of single-crystal high-temperature alloy

    CN115586317A

  • Device and method for eliminating zebra crystal of nickel-based single-crystal high-temperature alloy blade

    CN115625291A

  • Method for adjusting directional solidification temperature field and optimizing casting miscellaneous crystals by locally wrapping cotton on mold shell

    CN116689741A