A high thermal conductivity silicon nitride substrate and preparation method thereof
Through the ball milling method and the modified treatment of carbon powder, silica and magnesium yttriethoxysilane and superdispersant, the problems of high preparation cost and poor thermal conductivity of silicon nitride are solved by combining perfluorooctyl triethoxysilane and superdispersant. , high thermal conductivity and high quality silicon nitride substrate preparation are achieved.
Patent Information
- Application Number
- CN202410904590.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-08
AI Technical Summary
The existing silicon nitride preparation methods are costly and the thermal conductivity is affected by the oxygen content. How to reduce the preparation cost and improve the thermal conductivity while ensuring the quality of silicon nitride is an important issue.
After the carbon powder, silicon dioxide and yttrium oxide are modified by ball milling, a high thermal conductivity silicon nitride substrate is prepared by casting molding and pneumatic sintering, and the silicon dioxide is reduced by perfluorooctyl triethoxysilane. The surface oxygen content combined with the dual action of superdispersant achieves stable dispersion and high thermal conductivity.
It effectively reduces the preparation cost of silicon nitride substrates, improves thermal conductivity, simplifies the preparation process, and obtains high-purity and high-quality silicon nitride substrates.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of silicon nitride material preparation, in particular to a high thermal conductivity silicon nitride substrate and a preparation method thereof. Background Art
[0002] Silicon nitride is a high-performance semiconductor material with good thermal conductivity, electrical insulation, high temperature resistance and chemical stability. Therefore, it is widely used in heat dissipation devices in the fields of electronics, aerospace and automobiles. However, the preparation cost of silicon nitride is relatively high, mainly due to the high price of silicon nitride raw powder. In addition, the thermal conductivity of silicon nitride is also affected by its oxygen content. The higher the oxygen content, the worse the thermal conductivity.
[0003] There are currently two main methods for preparing silicon nitride: one is the high-temperature solid-phase reaction method, and the other is the chemical vapor deposition method. The high-temperature solid-phase reaction method is to react silicon powder and nitrogen at high temperature to generate silicon nitride. The advantage of this method is that the process is simple, but the energy consumption is high, and the purity of the obtained silicon nitride is not high; the chemical vapor deposition method is to deposit a silicon nitride film on the surface of the substrate through a chemical reaction. The advantage of this method is that the purity of the obtained silicon nitride is high, but the equipment is complex and the cost is high.
[0004] The existing silicon nitride preparation methods have the following main problems: first, the preparation cost is high, mainly due to the high price of silicon nitride raw powder; second, the thermal conductivity of the obtained silicon nitride is affected by its oxygen content. The higher the oxygen content, the worse the thermal conductivity. Therefore, how to reduce the preparation cost and improve the thermal conductivity of silicon nitride while ensuring the quality of silicon nitride is an important issue facing the current silicon nitride preparation technology. Summary of the invention
[0005] The object of the present invention is to provide a high thermal conductivity silicon nitride substrate and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A method for preparing a high thermal conductivity silicon nitride substrate comprises the following steps:
[0008] Step S1: putting carbon powder, silicon dioxide, magnesium oxide and yttrium oxide into a ball mill, adding a solvent and a hyperdispersant, and performing ball milling to obtain a suspension; adding a binder and a plasticizer to the suspension, and performing secondary ball milling to obtain a slurry;
[0009] Step S2: tape-casting the slurry to obtain a green sheet, drying it, and placing it in nitrogen for debinding to obtain a green sheet after debinding;
[0010] Step S3: sintering the debinded green sheet in nitrogen to obtain a silicon nitride substrate.
[0011] Furthermore, in step S1, the mass ratio of carbon powder, silicon dioxide, magnesium oxide and yttrium oxide is 1: (0.3-0.5): (0.2-0.4): (0.2-0.4).
[0012] Furthermore, in step S1, the particle sizes of carbon powder, silicon dioxide, magnesium oxide and yttrium oxide are 20-80 nm.
[0013] Furthermore, in step S1, the silicon dioxide is subjected to modification treatment, and the specific modification process is as follows:
[0014] The silicon dioxide, anhydrous ethanol and deionized water are uniformly mixed, the pH value of the system is adjusted to 10-12, perfluorooctyltriethoxysilane is added, and the mixture is reacted at 50-65° C. for 4-6 hours. After filtering, washing and drying, the modified silicon dioxide is obtained.
[0015] In the above technical scheme, the surface of silicon dioxide is modified by perfluorooctyltriethoxysilane to introduce perfluoroalkyl groups, which effectively reduces the oxygen content on the surface of silicon dioxide. In addition, during the sintering process, the perfluoroalkyl groups grafted on the surface of the modified silicon dioxide can play a synergistic role with the sintering aid, which can effectively reduce the secondary phase and lattice oxygen content of silicon nitride, promote grain growth, increase the density of silicon nitride, and thus improve the thermal conductivity of silicon nitride.
[0016] Furthermore, the mass ratio of silicon dioxide, anhydrous ethanol, deionized water and perfluorooctyltriethoxysilane is 1:(6-8):(2-3):(0.1-0.3).
[0017] Furthermore, in step S1, the solvent is a mixture of one or more of ethanol, xylene, n-butanol, and butanone in any proportion, and its amount is 60-90% of the total mass of carbon powder, silicon dioxide, magnesium oxide, and yttrium oxide.
[0018] Furthermore, in step S1, the preparation method of the hyperdispersant is as follows:
[0019] Step (1): uniformly mix polyvinylidene fluoride-hexafluoropropylene resin and N,N-dimethylformamide, add aqueous hydrogen peroxide solution, then add aqueous potassium hydroxide solution, react at 10-20°C for 4-6h, adjust the system pH to 2-3, filter, wash, and dry to obtain a terminal carboxyl fluorine-containing compound; uniformly mix sodium borohydride and tetrahydrofuran, drip a mixed solution of the terminal carboxyl fluorine-containing compound and tetrahydrofuran under ice bath conditions, drip for 1-2h, react for 1-2h, continue to drip a mixed solution of sulfuric acid and diethyl ether, drip for 30-50min, react for 10-12h, heat to 80-90°C, reflux for 2-4h, quench, rotary evaporate, wash, and dry to obtain a terminal hydroxyl fluorine-containing compound;
[0020] Step (2): uniformly mix the terminal hydroxyl fluorine-containing compound and tetrahydrofuran, add benzenesulfonyl chloride and triethylamine, react for 5-7 hours in an ice bath, transfer to heptane and mix evenly, filter, rotary evaporate, wash and dry to obtain an intermediate;
[0021] Step (3): The intermediate, N,N-dimethyl-1,3-diaminopropane and tetrahydrofuran are mixed evenly, reacted at 20-30° C. for 22-24 hours, and then subjected to rotary evaporation, washing and drying to obtain a hyperdispersant.
[0022] In the above technical scheme, the polymer chain of polyvinylidene fluoride-hexafluoropropylene is broken under an oxidative degradation reaction to generate a low molecular weight fluorocarbon polymer with carboxyl groups at both ends, i.e., a terminal carboxyl fluorine-containing compound; then, a sodium borohydride / sulfuric acid composite reduction system is used to reduce the terminal carboxyl fluorine-containing compound to a terminal hydroxyl fluorine-containing compound; finally, the terminal hydroxyl fluorine-containing compound is used as a solvated chain segment, and amine groups are introduced at both ends thereof as anchoring groups to obtain a hyperdispersant with an amphiphilic structure, which can simultaneously interact with the surfaces of hydrophobic silica and other powder particles to prevent the particles from precipitating or agglomerating in the solvent, so that the solid particles are evenly dispersed in the solvent, thereby maintaining the stability of the system.
[0023] Furthermore, in the step (1), the mass ratio of the polyvinylidene fluoride-hexafluoropropylene resin, N,N-dimethylformamide, aqueous hydrogen peroxide solution and aqueous potassium hydroxide solution is 1:(2-4):(0.6-0.8):(0.58-0.62).
[0024] Furthermore, in step (1), the concentration of the aqueous hydrogen peroxide solution is 30 wt %, and the concentration of the aqueous potassium hydroxide solution is 45 wt %.
[0025] Furthermore, in the step (1), the mass ratio of the terminal carboxyl fluorine-containing compound to tetrahydrofuran is 1:(4-5), the mass ratio of sodium borohydride to tetrahydrofuran is 1:(9-10), and the mass ratio of sulfuric acid to diethyl ether is 1:(3-5).
[0026] Furthermore, in the step (1), the mass ratio of the terminal carboxyl fluorine-containing compound, sodium borohydride and sulfuric acid is 1: (0.08-0.10): (0.15-0.20).
[0027] Furthermore, in step (1), the concentration of sulfuric acid is 37 wt %.
[0028] Furthermore, in step (2), the mass ratio of the terminal hydroxyl fluorine-containing compound to tetrahydrofuran is 1:(4-5), the mass of benzenesulfonyl chloride is 0.12-0.15 times the mass of the terminal hydroxyl fluorine-containing compound, and the mass of triethylamine is 3-5% of the mass of the terminal hydroxyl fluorine-containing compound.
[0029] Furthermore, in the step (3), the mass ratio of the intermediate to N,N-dimethyl-1,3-diaminopropane and tetrahydrofuran is 1:(0.07-0.10):(4-5).
[0030] Furthermore, in step S1, the amount of the hyperdispersant used is 0.5-2.5% of the total mass of the carbon powder, silicon dioxide, magnesium oxide and yttrium oxide.
[0031] Furthermore, in step S1, the binder is polyvinyl butyral, and its usage is 5-8% of the total mass of carbon powder, silicon dioxide, magnesium oxide and yttrium oxide.
[0032] Furthermore, in step S1, the plasticizer is butyl benzyl phthalate, and its usage is 0.4-0.6 times of the mass of the binder.
[0033] Furthermore, in step S1, the process conditions for ball milling are: using silicon nitride balls as ball milling media, a ball-to-material ratio of 2-5:1, a ball milling time of 12-24 hours, and a ball milling speed of 400-500 r / min.
[0034] Furthermore, in step S2, the process conditions of tape casting are: the speed of the tape casting is 0.2-5.0 m / min, and the thickness of the green sheet is 0.4-0.6 mm.
[0035] Furthermore, in step S2, the drying process conditions are: drying temperature 70-80° C., and drying time 2-4 hours.
[0036] Furthermore, in step S2, the process conditions for debinding are: heating to 550-600°C at a rate of 2-5°C / min, keeping the temperature for 2-5h, and then naturally cooling to room temperature.
[0037] Furthermore, in step S3, the process conditions of gas pressure sintering are: heating to 1750-1850° C. at a rate of 5-10° C. / min, keeping the temperature for 2-8 hours, and then naturally cooling to room temperature.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] 1. A high thermal conductivity silicon nitride substrate and a preparation method thereof of the present invention mainly use nano-carbon powder and nano-silicon dioxide, nano-magnesium oxide, and nano-yttrium oxide as raw materials. The prices of these raw materials are relatively low, thereby effectively reducing the preparation cost of the silicon nitride substrate. Compared with the existing silicon nitride preparation method, the method of the present invention is more economical. During the sintering process, the reduction effect of the carbon powder can reduce the oxygen content of the substrate, thereby improving the thermal conductivity of the substrate.
[0040] 2. The preparation method of the present invention is simple and easy, avoiding the complex steps such as high-temperature solid-phase reaction or chemical vapor deposition required in the existing silicon nitride preparation method, thereby greatly simplifying the preparation process and improving production efficiency; the preparation method of the present invention can obtain a silicon nitride substrate with high purity and good quality, because the present invention uses nano-level raw materials, which have small particle size and high activity, which is conducive to improving the completeness of the reaction, thereby obtaining a high-quality silicon nitride substrate.
[0041] 3. A high thermal conductivity silicon nitride substrate and a preparation method thereof of the present invention comprises the following steps: surface modification of silicon dioxide by perfluorooctyltriethoxysilane to introduce perfluoroalkyl groups, thereby effectively reducing the oxygen content on the surface of silicon dioxide; and during the sintering process, the perfluoroalkyl groups grafted on the surface of the modified silicon dioxide can play a synergistic role with the sintering aid, effectively reducing the secondary phase and lattice oxygen content of silicon nitride, being beneficial to grain growth, and increasing the density of silicon nitride, thereby increasing the thermal conductivity of silicon nitride.
[0042] 4. A high thermal conductivity silicon nitride substrate and a preparation method thereof of the present invention uses -NR2 as an anchoring group and a terminal hydroxyl fluorine-containing compound as a solvation chain segment to form a unique amphiphilic structure to obtain a hyperdispersant; through the dual effects of the anchoring group and the solvation chain, the hyperdispersant can effectively interact with the powder particles and the dispersion medium at the same time to achieve a stable dispersion state, prevent the powder particles from precipitating or agglomerating in the solvent, thereby maintaining the stable uniformity of the slurry, and further improving the thermal conductivity of the silicon nitride substrate. DETAILED DESCRIPTION
[0043] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] In this embodiment, the carbon powder has a particle size of 20 nm; the silicon dioxide has a particle size of 20 nm; the magnesium oxide has a particle size of 40 nm; the yttrium oxide has a particle size of 20 nm; the polyvinylidene fluoride-hexafluoropropylene resin has a model of French Arkema 2801, and the polyvinyl butyral has a model of Kuraray B60H.
[0045] Embodiment 1: A method for preparing a high thermal conductivity silicon nitride substrate, comprising the following processes:
[0046] Step S1: 500 g of carbon powder, 150 g of silicon dioxide, 100 g of magnesium oxide and 100 g of yttrium oxide are placed in a ball mill, 510 parts of xylene and 4.25 g of a hyperdispersant are added, and ball milling is performed (using silicon nitride balls as ball milling media, a ball-to-material ratio of 2:1, a ball milling time of 12 h, and a ball milling speed of 400 r / min) to obtain a suspension; 42.5 g of polyvinyl butyral and 17 g of butyl benzyl phthalate are added to the suspension, and secondary ball milling is performed (using silicon nitride balls as ball milling media, a ball-to-material ratio of 2:1, a ball milling time of 12 h, and a ball milling speed of 400 r / min) to obtain a slurry;
[0047] Step S2: The slurry is subjected to tape casting (the casting belt speed is 0.2 m / min) to obtain a 0.4 mm thin plate green body, which is then dried (drying temperature is 70°C and drying time is 2 h), and then placed in nitrogen for debinding (heating to 550°C at a rate of 2°C / min, keeping the temperature for 2 h, and then naturally cooling to room temperature) to obtain a debinded thin plate green body;
[0048] Step S3: sintering the debinded green sheet in nitrogen (heating to 1750° C. at a rate of 5° C. / min, keeping the temperature for 2 hours, and then cooling naturally to room temperature) to obtain a silicon nitride substrate;
[0049] In step S1, silicon dioxide is modified, and the specific modification process is as follows:
[0050] 150 g of silicon dioxide, 900 g of anhydrous ethanol and 300 g of deionized water were mixed evenly, the pH of the system was adjusted to 10, 15 g of perfluorooctyltriethoxysilane was added, and the mixture was reacted at 50° C. for 4 h. After filtering, washing and drying, modified silicon dioxide was obtained.
[0051] In step S1, the preparation method of the hyperdispersant is as follows:
[0052] Step (1): 4.25 g of polyvinylidene fluoride-hexafluoropropylene resin and 8.5 g of N,N-dimethylformamide are mixed evenly, 2.55 g of 30 wt% hydrogen peroxide aqueous solution is added, and then 2.5 g of 45 wt% potassium hydroxide aqueous solution is added, and the mixture is reacted at 10° C. for 4 h, and the pH value of the system is adjusted to 2. After filtering, washing and drying, a terminal carboxyl group-containing fluorine-containing compound is obtained; 0.34 g of sodium borohydride and 3.06 g of tetrahydrofuran are mixed evenly, and a mixed solution of 4.25 g of the terminal carboxyl group-containing fluorine-containing compound and 17 g of tetrahydrofuran is added dropwise under ice bath conditions for 1 h, and the mixture is reacted for 1 h. A mixed solution of 0.64 g of 37 wt% sulfuric acid and 1.92 g of ether is added dropwise for 30 min, and the mixture is reacted for 10 h. The mixture is heated to 80° C., and the mixture is refluxed for 2 h. After quenching, rotary evaporation, washing and drying, a terminal hydroxyl group-containing fluorine-containing compound is obtained;
[0053] Step (2): 4.25 g of a terminal hydroxyl fluorine-containing compound and 17 g of tetrahydrofuran were mixed evenly, 0.51 g of benzenesulfonyl chloride and 0.13 g of triethylamine were added, and the mixture was reacted in an ice bath for 5 h, and then the mixture was transferred to heptane and mixed evenly, and then filtered, rotary evaporated, washed, and dried to obtain an intermediate;
[0054] Step (3): 4.25 g of the intermediate, 0.3 g of N,N-dimethyl-1,3-diaminopropane and 17 g of tetrahydrofuran were mixed evenly, reacted at 20° C. for 22 h, and then subjected to rotary evaporation, washing and drying to obtain a hyperdispersant.
[0055] Embodiment 2: A method for preparing a high thermal conductivity silicon nitride substrate, comprising the following processes:
[0056] Step S1: 500 g of carbon powder, 200 g of silicon dioxide, 150 g of magnesium oxide and 150 g of yttrium oxide are placed in a ball mill, 700 g of xylene and 10 g of a hyperdispersant are added, and ball milling is performed (using silicon nitride balls as ball milling media, a ball-to-material ratio of 3:1, a ball milling time of 20 h, and a ball milling speed of 450 r / min) to obtain a suspension; 50 g of polyvinyl butyral and 25 g of butyl benzyl phthalate are added to the suspension, and secondary ball milling is performed (using silicon nitride balls as ball milling media, a ball-to-material ratio of 3:1, a ball milling time of 20 h, and a ball milling speed of 450 r / min) to obtain a slurry;
[0057] Step S2: The slurry is subjected to tape casting (the casting belt speed is 1.0 m / min) to obtain a 0.5 mm thin plate green body, which is then dried (drying temperature is 75°C and drying time is 3 h), and then placed in nitrogen for debinding (heating to 580°C at a rate of 4°C / min, keeping the temperature for 3 h, and then naturally cooling to room temperature) to obtain a debinded thin plate green body;
[0058] Step S3: sintering the debinded green sheet in nitrogen (heating to 1800° C. at a rate of 8° C. / min, keeping the temperature for 6 hours, and then cooling naturally to room temperature) to obtain a silicon nitride substrate;
[0059] In step S1, silicon dioxide is modified, and the specific modification process is as follows:
[0060] 200 g of silicon dioxide, 1400 g of anhydrous ethanol and 500 g of deionized water were mixed evenly, the pH of the system was adjusted to 11, 40 g of perfluorooctyltriethoxysilane was added, and the mixture was reacted at 60° C. for 5 h. After filtering, washing and drying, modified silicon dioxide was obtained.
[0061] In step S1, the preparation method of the hyperdispersant is as follows:
[0062] Step (1): 10 g of polyvinylidene fluoride-hexafluoropropylene resin and 30 g of N,N-dimethylformamide are mixed evenly, 7 g of 30 wt% hydrogen peroxide aqueous solution is added, and then 6 g of 45 wt% potassium hydroxide aqueous solution is added, and the mixture is reacted at 15°C for 5 h, and the pH value of the system is adjusted to 2.5. After filtering, washing and drying, a terminal carboxyl group-containing fluorine-containing compound is obtained; 0.9 g of sodium borohydride and 8.5 g of tetrahydrofuran are mixed evenly, and a mixed solution of 10 g of the terminal carboxyl group-containing fluorine-containing compound and 45 g of tetrahydrofuran is added dropwise under ice bath conditions for 1 h, and the mixture is reacted for 1.5 h. A mixed solution of 1.6 g of 37 wt% sulfuric acid and 6.4 g of ether is added dropwise for 40 min, and the mixture is reacted for 11 h. The mixture is heated to 85°C, and the mixture is refluxed for 3 h. After quenching, rotary evaporation, washing and drying, a terminal hydroxyl group-containing fluorine-containing compound is obtained;
[0063] Step (2): 10 g of a terminal hydroxyl fluorine-containing compound and 45 g of tetrahydrofuran were mixed evenly, 1.3 g of benzenesulfonyl chloride and 0.4 g of triethylamine were added, and the mixture was reacted in an ice bath for 6 h, and then the mixture was transferred to heptane and mixed evenly, and then filtered, rotary evaporated, washed, and dried to obtain an intermediate;
[0064] Step (3): 10 g of the intermediate, 0.8 g of N,N-dimethyl-1,3-diaminopropane and 45 g of tetrahydrofuran were mixed evenly, reacted at 25° C. for 23 h, and then subjected to rotary evaporation, washing and drying to obtain a hyperdispersant.
[0065] Embodiment 3: A method for preparing a high thermal conductivity silicon nitride substrate, comprising the following process:
[0066] Step S1: 500 g of carbon powder, 250 g of silicon dioxide, 200 g of magnesium oxide and 200 g of yttrium oxide are placed in a ball mill, 1035 g of xylene and 28.75 g of a hyperdispersant are added, and ball milling is performed (using silicon nitride balls as ball milling media, a ball-to-material ratio of 5:1, a ball milling time of 24 h, and a ball milling speed of 500 r / min) to obtain a suspension; 92 g of polyvinyl butyral and 55.2 g of butyl benzyl phthalate are added to the suspension, and secondary ball milling is performed (using silicon nitride balls as ball milling media, a ball-to-material ratio of 5:1, a ball milling time of 24 h, and a ball milling speed of 500 r / min) to obtain a slurry;
[0067] Step S2: The slurry is subjected to tape casting (the casting belt speed is 5.0 m / min) to obtain a 0.6 mm thin plate green body, which is then dried (drying temperature is 80°C, and drying time is 4 hours), and then placed in nitrogen for debinding (heating to 600°C at a rate of 5°C / min, keeping the temperature for 5 hours, and then naturally cooling to room temperature) to obtain a debinded thin plate green body;
[0068] Step S3: sintering the debinded green sheet in nitrogen (heating to 1850° C. at a rate of 10° C. / min, keeping the temperature for 8 hours, and then cooling naturally to room temperature) to obtain a silicon nitride substrate;
[0069] In step S1, silicon dioxide is modified, and the specific modification process is as follows:
[0070] 250 g of silicon dioxide, 2000 g of anhydrous ethanol and 750 g of deionized water were mixed evenly, the pH of the system was adjusted to 12, 75 g of perfluorooctyltriethoxysilane was added, and the mixture was reacted at 65° C. for 6 h. After filtering, washing and drying, modified silicon dioxide was obtained;
[0071] In step S1, the preparation method of the hyperdispersant is as follows:
[0072] Step (1): 30 g of polyvinylidene fluoride-hexafluoropropylene resin and 140 g of N,N-dimethylformamide are mixed evenly, 24 g of a 30 wt% hydrogen peroxide aqueous solution is added, and then 18.6 g of a 45 wt% potassium hydroxide aqueous solution is added, and the mixture is reacted at 20° C. for 6 h, and the pH value of the system is adjusted to 3. After filtering, washing, and drying, a terminal carboxyl group-containing fluorine-containing compound is obtained; 3 g of sodium borohydride and 30 g of tetrahydrofuran are mixed evenly, and a mixed solution of 30 g of the terminal carboxyl group-containing fluorine-containing compound and 150 g of tetrahydrofuran is added dropwise under ice bath conditions, and the mixture is added dropwise for 2 h, and the mixture is reacted for 2 h. 6 g of a mixed solution of 35 wt% sulfuric acid and 30 g of ether is added dropwise for 50 min, and the mixture is reacted for 12 h. The mixture is heated to 90° C., and the mixture is refluxed for 4 h. After quenching, rotary evaporation, washing, and drying, a terminal hydroxyl group-containing fluorine-containing compound is obtained;
[0073] Step (2): 30 g of the terminal hydroxyl fluorine-containing compound and 150 g of tetrahydrofuran were mixed evenly, 4.5 g of benzenesulfonyl chloride and 1.5 g of triethylamine were added, and the mixture was reacted in an ice bath for 7 h, and then the mixture was transferred to heptane and mixed evenly, and then filtered, rotary evaporated, washed, and dried to obtain an intermediate;
[0074] Step (3): 30 g of the intermediate, 3 g of N,N-dimethyl-1,3-diaminopropane and 150 g of tetrahydrofuran were mixed evenly, reacted at 30° C. for 24 h, and after rotary evaporation, washing and drying, a hyperdispersant was obtained.
[0075] Comparative Example 1: A method for preparing a high thermal conductivity silicon nitride substrate, comprising the following processes:
[0076] Compared with Example 2, in Comparative Example 1, the hyperdispersant in step S1 is replaced with sodium phosphate of the same mass, and the other steps are the same as those in Example 2.
[0077] Comparative Example 2: A method for preparing a high thermal conductivity silicon nitride substrate, comprising the following processes:
[0078] Compared with Example 2, in step S1 of Comparative Example 2, the mass ratio of carbon powder, silicon dioxide, magnesium oxide and yttrium oxide is 1:2:0.3:0.3, and the other steps are the same as those in Example 2.
[0079] Comparative Example 3: A method for preparing a high thermal conductivity silicon nitride substrate, comprising the following processes:
[0080] Compared with Example 2, in Comparative Example 3, no modification treatment is performed on the silicon dioxide, and other steps are the same as those in Example 2.
[0081] Comparative Example 4: A method for preparing a high thermal conductivity silicon nitride substrate, comprising the following processes:
[0082] In step S1, the preparation method of the hyperdispersant is as follows:
[0083] Step (1): 10 g of polyvinylidene fluoride-hexafluoropropylene resin and 30 g of N,N-dimethylformamide are mixed evenly, 7 g of 30 wt% hydrogen peroxide aqueous solution is added, and then 6 g of 45 wt% potassium hydroxide aqueous solution is added, and the mixture is reacted at 15°C for 5 h, and the pH value of the system is adjusted to 2.5. After filtering, washing and drying, a terminal carboxyl group-containing fluorine-containing compound is obtained; 0.9 g of sodium borohydride and 8.5 g of tetrahydrofuran are mixed evenly, and a mixed solution of 10 g of the terminal carboxyl group-containing fluorine-containing compound and 45 g of tetrahydrofuran is added dropwise under ice bath conditions for 1 h, and the mixture is reacted for 1.5 h. A mixed solution of 1.6 g of 37 wt% sulfuric acid and 6.4 g of ether is added dropwise for 40 min, and the mixture is reacted for 11 h. The mixture is heated to 85°C, and the mixture is refluxed for 3 h. After quenching, rotary evaporation, washing and drying, a terminal hydroxyl group-containing fluorine-containing compound is obtained;
[0084] Step (2): 10 g of a terminal hydroxyl fluorine-containing compound and 45 g of tetrahydrofuran were mixed evenly, 1.3 g of benzenesulfonyl chloride and 0.4 g of triethylamine were added, and the mixture was reacted in an ice bath for 6 h, and then the mixture was transferred to heptane and mixed evenly, and then filtered, rotary evaporated, washed, and dried to obtain an intermediate;
[0085] Step (3): 10 g of the intermediate, 10 g of N,N-dimethyl-1,3-diaminopropane and 45 g of tetrahydrofuran were mixed evenly, reacted at 25° C. for 23 h, and then subjected to rotary evaporation, washing and drying to obtain a hyperdispersant;
[0086] Compared with Example 2, the mass ratio of the intermediate and N,N-dimethyl-1,3-diaminopropane in Comparative Example 4 is 1:1; the other steps are the same as those in Example 2.
[0087] Experiment: The silicon nitride substrates obtained in Examples 1-3 and Comparative Examples 1-4 were used to prepare samples, and their properties were tested and the test results were recorded:
[0088] Thermal conductivity was tested at 25 °C using a laser pulse instrument (Netzsch LFA 467, GER). Flexural strength was tested using the three-point bending method, with a span of 30 mm and a loading rate of 0.5 mm / min. Fracture toughness was determined using the single-edge notched beam method (SENB), with a notch depth of 2 mm, a span of 24 mm, and a loading rate of 0.05 mm·min. -1 .
[0089] Test Results
[0090]
[0091] According to the data in the above table, we can clearly draw the following conclusions:
[0092] 1. Compared with Examples 1-3, the thermal conductivity, flexural strength and fracture toughness of the product obtained in Comparative Example 1 are all reduced, indicating that the hyperdispersant prepared by the present invention has better dispersibility than sodium phosphate, thereby maintaining the stable uniformity of the slurry.
[0093] 2. Compared with Examples 1-3, the thermal conductivity, flexural strength and fracture toughness of the products obtained in Comparative Examples 2 and 3 are all reduced, which indicates that the performance of the silicon nitride substrate prepared by the present invention is affected by its component ratio. By selecting the component ratio within the said range, a high thermal conductivity silicon nitride substrate can be prepared; in addition, the present invention effectively reduces the oxygen content on the surface of silicon dioxide by modifying the silicon dioxide, which is beneficial to grain growth and improves the density of silicon nitride.
[0094] 3. Compared with Examples 1-3, the thermal conductivity, flexural strength and fracture toughness of the product obtained in Comparative Example 4 are all reduced. It can be seen that the performance of the hyperdispersant prepared by the present invention is affected by the ratio of each reagent in its preparation process. By selecting a mass ratio within the range, the prepared hyperdispersant can effectively prevent the powder particles from precipitating or agglomerating in the solvent, thereby maintaining the stable uniformity of the slurry and improving the performance and stability of the product.
[0095] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0096] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a high thermal conductivity silicon nitride substrate, characterized in that: The steps include: Step S1: putting nano carbon powder, nano silicon dioxide, nano magnesium oxide and nano yttrium oxide into a ball mill, adding a solvent and a hyperdispersant, and performing ball milling to obtain a suspension; adding a binder and a plasticizer to the suspension, and performing secondary ball milling to obtain a slurry; Step S2: tape-casting the slurry to obtain a green sheet, drying it, and placing it in nitrogen for debinding to obtain a green sheet after debinding; Step S3: sintering the debinded green sheet in nitrogen to obtain a silicon nitride substrate; In the step S1, the mass ratio of nano carbon powder, nano silicon dioxide, nano magnesium oxide and nano yttrium oxide is 1: (0.3-0.5): (0.2-0.4): (0.2-0.4); In step S1, the nano-silicon dioxide is subjected to modification treatment, and the specific modification process is as follows: The nano-silica is mixed evenly with anhydrous ethanol and deionized water, the pH of the system is adjusted to 10-12, perfluorooctyl triethoxysilane is added, and the mixture is reacted at 50-65°C for 4-6 hours, and the modified nano-silica is obtained after filtering, washing and drying. In step S1, the preparation method of the hyperdispersant is as follows: Step (1): uniformly mix polyvinylidene fluoride-hexafluoropropylene resin and N,N-dimethylformamide, add aqueous hydrogen peroxide solution, then add aqueous potassium hydroxide solution, react at 10-20°C for 4-6h, adjust the system pH to 2-3, filter, wash, and dry to obtain a terminal carboxyl fluorine-containing compound; uniformly mix sodium borohydride and tetrahydrofuran, drip a mixed solution of the terminal carboxyl fluorine-containing compound and tetrahydrofuran under ice bath conditions, drip for 1-2h, react for 1-2h, continue to drip a mixed solution of sulfuric acid and diethyl ether, drip for 30-50min, react for 10-12h, heat to 80-90°C, reflux for 2-4h, quench, rotary evaporate, wash, and dry to obtain a terminal hydroxyl fluorine-containing compound; Step (2): uniformly mix the terminal hydroxyl fluorine-containing compound and tetrahydrofuran, add benzenesulfonyl chloride and triethylamine, react for 5-7 hours in an ice bath, transfer to heptane and mix evenly, filter, rotary evaporate, wash and dry to obtain an intermediate; Step (3): uniformly mix the intermediate, N,N-dimethyl-1,3-diaminopropane and tetrahydrofuran, react at 20-30° C. for 22-24 hours, and obtain a hyperdispersant after rotary evaporation, washing and drying; In the step (1), the mass ratio of polyvinylidene fluoride-hexafluoropropylene resin, N,N-dimethylformamide, aqueous hydrogen peroxide solution and aqueous potassium hydroxide solution is 1: (2-4): (0.6-0.8): (0.58-0.62); In step (1), the concentration of the aqueous hydrogen peroxide solution is 30 wt %, and the concentration of the aqueous potassium hydroxide solution is 45 wt %; In the step (1), the mass ratio of the terminal carboxyl fluorine-containing compound to tetrahydrofuran is 1:(4-5), the mass ratio of sodium borohydride to tetrahydrofuran is 1:(9-10), and the mass ratio of sulfuric acid to diethyl ether is 1:(3-5); In the step (1), the mass ratio of the terminal carboxyl fluorine-containing compound, sodium borohydride and sulfuric acid is 1: (0.08-0.10): (0.15-0.20); In step (1), the concentration of sulfuric acid is 37wt%; In the step (2), the mass ratio of the terminal hydroxyl fluorine-containing compound to tetrahydrofuran is 1:(4-5), the mass of benzenesulfonyl chloride is 0.12-0.15 times the mass of the terminal hydroxyl fluorine-containing compound, and the mass of triethylamine is 3-5% of the mass of the terminal hydroxyl fluorine-containing compound; In the step (3), the mass ratio of the intermediate to N,N-dimethyl-1,3-diaminopropane and tetrahydrofuran is 1:(0.07-0.10):(4-5); In the step S1, the amount of the superdispersant used is 0.5-2.5% of the total mass of the nano-carbon powder, nano-silicon dioxide, nano-magnesium oxide and nano-yttrium oxide.
2. The method for preparing a high thermal conductivity silicon nitride substrate according to claim 1, characterized in that: In the step S1, the solvent is a mixture of one or more of ethanol, xylene, n-butanol and butanone in any proportion, and the amount of the solvent is 60-90% of the total mass of the nano-carbon powder, nano-silicon dioxide, nano-magnesium oxide and nano-yttrium oxide.
3. The method for preparing a high thermal conductivity silicon nitride substrate according to claim 1, characterized in that: In the step S1, the binder is polyvinyl butyral, and the amount thereof is 5-8% of the total mass of the nano-carbon powder, nano-silicon dioxide, nano-magnesium oxide and nano-yttrium oxide.
4. The method for preparing a high thermal conductivity silicon nitride substrate according to claim 1, characterized in that: In step S2, the process conditions of tape casting are: the speed of the tape casting is 0.2-5.0 m / min, and the thickness of the green sheet is 0.4-0.6 mm.
5. The method for preparing a high thermal conductivity silicon nitride substrate according to claim 1, characterized in that: In step S2, the process conditions for debinding are: heating to 550-600°C at a rate of 2-5°C / min, keeping the temperature for 2-5h, and then naturally cooling to room temperature.
6. The method for preparing a high thermal conductivity silicon nitride substrate according to claim 1, characterized in that: In step S3, the process conditions of gas pressure sintering are: heating to 1750-1850° C. at a rate of 5-10° C. / min, keeping the temperature for 2-8 hours, and then naturally cooling to room temperature.
7. A high thermal conductivity silicon nitride substrate prepared according to the preparation method according to any one of claims 1 to 6.
Citation Information
Cited By
A debinding process for high thermal conductivity silicon nitride substrate
CN119775029A