A method for preparing HVO from bio-oil
By using copper-aluminum nanocomposite oxide catalyst and in-situ polymerization method to reduce moisture adsorption during the HVO preparation process, the impact of impurities and moisture on the catalyst is solved, the catalyst activity and the quality of HVO are improved, and efficient HVO preparation is achieved.
Patent Information
- Application Number
- CN202410906546.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-08
Smart Images

Figure CN118440779B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of HVO preparation, and in particular to a method for preparing HVO from bio-oil. Background Art
[0002] HVO is a fuel produced by hydrogenating vegetable oil or animal fat in the presence of a catalyst. It has similar physical and chemical properties to fossil fuels and can therefore be used as a substitute for fossil fuels. The HVO production process achieves the upgrading of vegetable oil or animal fat, improves its energy utilization value, and reduces dependence on fossil fuels.
[0003] At present, fossil fuels are increasingly in short supply, and the large amount of waste they emit has also had a serious impact on the environment. Therefore, finding a clean, renewable, and alternative energy source to fossil fuels meets the needs of global energy security and sustainable development. HVO, as a new type of fuel, has the advantages of excellent combustion, renewability, safety, and environmental protection. It has become one of the key research directions of clean, renewable alternative energy and has received widespread attention in recent years.
[0004] In the preparation process of HVO, the catalyst has a great influence on the quality and yield of HVO. When the catalytic activity of the catalyst is high, the quality and yield of HVO will be improved. However, the raw material bio-oil used in the preparation process of HVO usually contains a small amount of impurities and a high oxygen content. In the production process, more water will be produced. Water and impurities have a great toxic effect on the catalyst, thus reducing the catalytic activity of the catalyst and even affecting the reactor equipment, affecting the long-term stable operation of the system, thereby increasing production costs and safety hazards.
[0005] In order to reduce the influence of water generated in the production process on the catalyst, it is generally necessary to implement distillation or use a dehydrating agent for dehydration during the production process, or adjust the reaction device or reaction conditions to reduce the influence of water. The Chinese patent application document with publication number CN114410337A discloses a method and device for producing alkyl biofuel by hydrogenation, which reduces the influence of water generated in the hydrogenation process on the catalyst as much as possible by limiting the loading method of the hydrogenation catalyst. However, this method increases the complexity of the reaction system and may require a precise control system and monitoring system. The control requirements for process conditions are also more stringent, thereby increasing the complexity and cost of the operation. Summary of the invention
[0006] In order to solve the problem of the influence of impurities and moisture on the catalyst in the HVO production process and improve the activity of the catalyst, the present application provides a method for preparing HVO from bio-oil.
[0007] A method for preparing HVO from bio-oil comprises the following steps:
[0008] S1: Mix the bio-oil and hydrogen into a reactor, and obtain a C5-500℃ fraction through a hydrogenation pretreatment process under the action of a catalyst;
[0009] S2: Mix the C5-500℃ fraction and hydrogen and enter the reactor. Under the action of the catalyst, the C5+ fraction is obtained through a hydrogenation refining process.
[0010] S3: Mix the C5+ fraction and hydrogen and enter the reactor. Under the action of the catalyst, the HVO is obtained by a single process through hydrogenation isomerization.
[0011] The preparation method of the catalyst comprises the following steps:
[0012] 1) dissolving aluminum nitrate nonahydrate and copper nitrate trihydrate in water, adjusting the pH value to 9-10, heating to 60-80° C., reacting for 9-15 hours, filtering, washing, drying, grinding, calcining, and cooling to obtain copper-aluminum nanocomposite oxide;
[0013] 2) Dispersing the copper-aluminum nanocomposite oxide in water, adding the precursor of the active component, urea and ammonium fluoride, stirring evenly, heating to 110-130° C., reacting for 3-6 hours, washing, drying, calcining and cooling the product to obtain the copper-aluminum nanocomposite oxide loaded with the active component;
[0014] 3) Dispersing the copper-aluminum nanocomposite oxide loaded with active components in an ethanol aqueous solution, adding organic siloxane and ammonia water, heating to 70-90° C., reacting for 12-24 hours, washing, drying and molding, the product is ready.
[0015] The above technical scheme is adopted, and hydrogenation pretreatment is first carried out, the purpose of which is: ① hydrogenation and deoxygenation of fatty acids. When free fatty acids or triglycerides are deoxygenated, alkanes with a carbon chain length equal to or one carbon less than the original carbon chain length are mainly produced. Hydrogenation pretreatment removes most of the free fatty acids, which can alleviate the processing difficulty of subsequent fixed bed hydrofining; ② removal of metals and phospholipids. Hydrogenation pretreatment can remove most of the metals and phospholipids, greatly improving the operation cycle of subsequent fixed bed hydrofining; ③ dechlorination. The chlorine content affects the material selection. After the inorganic chlorine and organic chlorine are removed by hydrogenation pretreatment, the material selection of subsequent hydrofining and hydroisomerization units is reduced, thereby reducing the investment in the unit.
[0016] Then fixed-bed hydrotreating is carried out for the following purposes: ① to remove oxygen, sulfur, nitrogen, phosphorus, metals and other impurities. The oxygen, sulfur, nitrogen, phosphorus, metals and other impurities remaining after hydrogenation pretreatment are poisons to the subsequent hydroisomerization catalyst. After being removed in the hydrotreating stage, the operating cycle of the hydroisomerization catalyst can be increased; ② the gas components such as H2S, NH3, CO and CO2 produced by the stripping reaction and the hydrotreating reaction are poisons and inhibitors of the hydroisomerization catalyst; setting up a stripping tower to remove these gas components can extend the operating cycle of the hydroisomerization catalyst.
[0017] Finally, fixed-bed hydroisomerization is carried out with the following purposes: ① isomerize n-alkanes into isoalkanes. The hydroisomerization reactor improves low-temperature fluidity by isomerizing n-alkanes; ② saturates aromatics to meet the requirements of HVO for aromatics.
[0018] In order to obtain high-quality and high-yield HVO, the core is the hydrogenation catalyst, so it is very important to improve the catalytic activity of the catalyst. First, the copper-aluminum layered double hydroxide is calcined, the hydroxyl groups between the layers shrink and the carbon dioxide is removed, and a copper-aluminum nanocomposite oxide with a large specific surface area is obtained. The catalytic active center is fully exposed and exhibits excellent catalytic performance. Then, due to the large specific surface area of the copper-aluminum nanocomposite oxide, the active components are further loaded to improve its catalytic activity. Moreover, the nanoparticles loaded on the copper-aluminum nanocomposite oxide are similar to the nano-scale ultrastructure in the lotus leaf structure, which can play a certain self-cleaning role, thereby reducing the impact of impurities and moisture generated during the hydrogenation process on the catalyst.
[0019] In addition, due to the high oxygen content of bio-oil, a large amount of water will be produced during the hydrogenation process. Water molecules will greatly reduce the catalytic activity of the catalyst for the following reasons: ① Water molecules may react with the active centers of the catalyst, causing the active centers to degrade or inactivate, thereby reducing the catalytic efficiency and stability of the catalyst; ② On the catalyst surface, water molecules may compete with reactants, such as bio-oil and hydrogen, for adsorption sites, thereby reducing the catalyst's adsorption capacity for reactants and, in turn, reducing the catalytic efficiency; ③ During the hydrogenation process, metal catalysts may be reduced to metals. If water is adsorbed on the catalyst surface, it may affect the reduction process and cause the catalyst to deactivate; ④ Under high temperature conditions, if the catalyst is exposed to water for a long time, it is easy to cause the active components on the catalyst surface to aggregate, resulting in a decrease in strength. The catalyst may pulverize and block the reactor, which is very detrimental to the long-term stable operation of the system.
[0020] Therefore, the in-situ polymerization method is used to perform hydrophobic treatment on the copper-aluminum nanocomposite oxide loaded with active components, so that water molecules are not easily adsorbed on the catalyst surface, the reaction between the catalyst active center and water molecules is reduced, the competitive adsorption of water molecules is weakened, and the number of adsorption sites of reactants, such as bio-oil and hydrogen, on the catalyst is increased. At the same time, the influence of water molecules on the metal reduction process is reduced, and the contact time between the catalyst and water is reduced, thereby improving the catalytic activity of the catalyst and reducing the poisoning of water to the catalyst. At the same time, the in-situ polymerization method makes the nano-silicon dioxide on the copper-aluminum nanocomposite oxide have good dispersion, thereby further improving the hydrophobic performance and specific surface area of the catalyst.
[0021] Preferably, the mass ratio of aluminum nitrate nonahydrate to copper nitrate trihydrate in step 1) is (0.5-1.7):1.
[0022] By adopting the above technical scheme, the copper oxide in the copper-aluminum nanocomposite oxide is reduced to metallic copper under appropriate temperature and pressure, and the metallic copper reacts with hydrogen to form an active center, which can promote the reaction, so when the copper oxide content is high, the catalytic activity of the catalyst will increase. Aluminum oxide in the copper-aluminum nanocomposite oxide can be used as a support for the catalyst carrier, improve the stability of the catalyst, and is also conducive to the dispersion of copper oxide. At the same time, it can also provide a certain amount of acid sites to promote isomerization reaction. However, when the aluminum oxide content is too high, there are more acid sites, which is not conducive to the reduction of copper oxide; when the copper oxide content is too high, the dispersibility of copper oxide deteriorates, and the catalytic activity decreases accordingly, so the mass ratio of copper oxide and aluminum oxide should be controlled within a certain range, that is, the mass ratio of aluminum nitrate nonahydrate and copper nitrate trihydrate should be controlled within an appropriate range.
[0023] Preferably, in step 2), the mass ratio of the copper-aluminum nanocomposite oxide to the precursor of the active component is 1:(0.4-1.5).
[0024] In the above technical scheme, when the copper-aluminum nanocomposite oxide is constant, if too little precursor of the active component is added, the amount of the active component loaded on the copper-aluminum nanocomposite oxide is too small, which is not conducive to improving the catalytic activity of the catalyst; if too much precursor of the active component is added, the dispersibility of the active component on the copper-aluminum nanocomposite oxide becomes poor, which will also reduce the catalytic activity of the catalyst to a certain extent. Therefore, the mass ratio of the copper-aluminum nanocomposite oxide and the precursor of the active component should be controlled within an appropriate range.
[0025] Preferably, in step 3), the mass ratio of the copper-aluminum nanocomposite oxide loaded with active components to the organosiloxane is 1:(5-20).
[0026] By adopting the above technical scheme, when the copper-aluminum nanocomposite oxide carrying active components is certain, if the amount of the added organosiloxane is too much, the nano-silica particles on the copper-aluminum nanocomposite oxide carrying active components may agglomerate, which not only affects the catalytic activity of the catalyst, but also reduces the hydrophobicity of the catalyst; if the amount of the added organosiloxane is too little, the hydrophobicity of the catalyst is poor, and the harm of water molecules to the catalyst will also increase. Therefore, the mass ratio of the copper-aluminum nanocomposite oxide carrying active components to the organosiloxane should be controlled within a certain range.
[0027] Preferably, the bio-oil in step S1 is one or more of vegetable oil, animal fat or waste cooking oil.
[0028] In the above technical solution, the bio-oil can be vegetable oil, such as soybean oil, rapeseed oil, palm oil, peanut oil, sunflower oil, coconut oil, olive oil, cottonseed oil, linseed oil, rice bran oil, etc.; the bio-oil can also be animal fat, such as tallow, sheep oil, lard, fish oil, etc.; the bio-oil can also be waste edible oil, such as waste catering oil, industrial oil, recycled animal and plant oil, etc., so the bio-oil has a wide source, is not only renewable, but also can alleviate environmental pressure. In addition, the oxygen content, impurity content, metal content, etc. of each bio-oil are different, so when different bio-oils are used as raw materials, the yield of the prepared HVO will also be different.
[0029] The above technical solution of the present application includes at least the following beneficial effects:
[0030] 1. The present application obtains a stable copper-aluminum nanocomposite oxide by calcining a copper-aluminum layered double hydroxide, which greatly increases the specific surface area, improves the hydrogen adsorption performance, and fully exposes the active center, thereby improving the catalytic activity of the catalyst.
[0031] 2. The present application not only improves the catalytic activity by loading active components with high catalytic activity on the stable copper-aluminum nanocomposite oxide, but also the ultrastructure of the nanoparticles can reduce the influence of impurities and water molecules on the catalyst to a certain extent.
[0032] 3. The present application adopts an in-situ polymerization method to load hydrophobic nano-silica on the copper-aluminum nano-composite oxide loaded with active components, further reducing the adsorption of water molecules on the catalyst surface, thereby reducing the damage of the catalyst to the water generated during the HVO preparation process and improving the catalytic activity of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a trend chart of the HVO yields of Examples 1-9 and Comparative Examples 1-2. DETAILED DESCRIPTION
[0034] The present application is further described in detail below with reference to the embodiments.
[0035] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.
[0036] Example
[0037] Example 1
[0038] The method for preparing HVO from bio-oil of this embodiment comprises the following steps:
[0039] S1: Soybean oil and hydrogen were mixed in a hydrogen-to-oil volume ratio of 300:1 and fed into a reactor with an expanded bed. The reactor was equipped with three catalyst beds, the pressure was set to 5 MPa, and the space velocity was 0.2 h -1 The reaction adopts a hot high-oil separation process, sets the circulation ratio of the hot high-oil separation circulation pump to 1:1, adjusts the circulating oil volume to control the reaction inlet temperature to 200°C, and obtains a C5-500°C fraction;
[0040] S2: The C5-500℃ fraction and hydrogen are mixed in a hydrogen-to-oil volume ratio of 200:1 and then fed into a fixed bed reactor. The reactor is equipped with three catalyst beds, with cooling hydrogen facilities between the beds. The pressure is set to 4MPa and the space velocity is 0.3h -1 The large-scale device reaction adopts the hot high-oil separation process, and the reaction inlet temperature is controlled at 200°C. The small-scale device reaction adopts the cold high-oil separation process, and a stripping tower is set to remove hydrogen sulfide, ammonia, carbon monoxide and other gases to obtain the C5+ fraction;
[0041] S3: The C5+ fraction and hydrogen are mixed in a hydrogen-to-oil volume ratio of 200:1 and fed into a fixed bed reactor. The reactor is equipped with two catalyst beds, with a hydrogen cooling facility between the beds. The pressure is set to 4 MPa and the space velocity is 0.5 h -1 The large-scale device reaction adopts the hot high-oil separation process, and the reaction inlet temperature is controlled at 250°C. The small-scale device reaction adopts the cold high-oil separation process, adopts a one-time process, sets a fractionation tower, and produces HVO at the bottom of the fractionation tower;
[0042] The method for preparing the catalyst used in steps S1 and S2 in this embodiment comprises the following steps:
[0043] 1) Weigh 5 g of aluminum nitrate nonahydrate, 10 g of copper nitrate trihydrate and 500 mL of deionized water, place in a three-necked flask equipped with a stirring device, stir until completely dissolved, slowly drop 1 mol / L sodium hydroxide solution, adjust the pH value to 9, heat to 60° C., react for 15 h, filter the product, wash until neutral, dry at 60° C. for 12 h, grind and place in a muffle furnace, calcine at 500° C. for 4 h, and cool to obtain a copper-aluminum nanocomposite oxide;
[0044] 2) Weigh 10 g of copper-aluminum nanocomposite oxide and 200 mL of deionized water, place them in a reaction kettle, stir to disperse them evenly, add 4 g of nickel nitrate hexahydrate, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 110° C., react for 6 h, cool the product, wash and dry it, place it in a muffle furnace, and calcine it at 400° C. for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0045] 3) Weigh 10 g of copper-aluminum nanocomposite oxide loaded with active components and 300 mL of 50% ethanol aqueous solution, place in a three-necked flask, add 30 g of methyltrimethoxysilane, 20 g of dimethylsiloxane and 5 mL of 1 mol / L ammonia water, heat to 70 ° C, react for 24 h, wash and dry the product and shape it into a cylinder;
[0046] The method for preparing the catalyst used in step S3 of this embodiment is different from the method for preparing the catalyst used in steps S1 and S2 in that:
[0047] 2) Weigh 10 g of nanocomposite oxide and 200 mL of deionized water, place in a reaction kettle, stir to disperse evenly, add 4 g of silver nitrate, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 110°C, react for 6 h, cool the product, wash, dry, place in a muffle furnace, and calcine at 400°C for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0048] The remaining steps are the same as the preparation method of the catalyst used in steps S1 and S2.
[0049] Example 2
[0050] The method for preparing HVO from bio-oil of this embodiment comprises the following steps:
[0051] S1: Soybean oil and hydrogen were mixed in a hydrogen-to-oil volume ratio of 900:1 and fed into a reactor with an expanded bed. The reactor was equipped with 8 catalyst beds, the pressure was set at 15 MPa, and the space velocity was 1.2 h -1 The reaction adopts a hot high-separation oil process, sets the circulation ratio of the hot high-separation oil circulation pump to 5:1, adjusts the circulating oil volume to control the reaction inlet temperature to 400°C, and obtains a C5-500°C fraction;
[0052] S2: The C5-500℃ fraction and hydrogen are mixed in a hydrogen-to-oil volume ratio of 1500:1 and fed into a fixed bed reactor. The reactor is equipped with 8 catalyst beds, with hydrogen cooling facilities between the beds. The pressure is set at 15MPa and the space velocity is 2h -1The large-scale device reaction adopts the hot high-oil separation process, and the reaction inlet temperature is controlled at 380°C. The small-scale device reaction adopts the cold high-oil separation process, and a stripping tower is set to remove hydrogen sulfide, ammonia, carbon monoxide and other gases to obtain the C5+ fraction;
[0053] S3: The C5+ fraction and hydrogen are mixed in a hydrogen-to-oil volume ratio of 700:1 and fed into a fixed bed reactor. The reactor is equipped with 5 catalyst beds, with hydrogen cooling facilities between the beds. The pressure is set at 15 MPa and the space velocity is 2 h -1 The large-scale device reaction adopts the hot high-oil separation process, and the reaction inlet temperature is controlled at 380°C. The small-scale device reaction adopts the cold high-oil separation process, adopts a one-time process, sets a fractionation tower, and produces HVO at the bottom of the fractionation tower;
[0054] The method for preparing the catalyst used in steps S1 and S2 in this embodiment comprises the following steps:
[0055] 1) Weigh 5 g of aluminum nitrate nonahydrate, 10 g of copper nitrate trihydrate and 500 mL of deionized water, place in a three-necked flask equipped with a stirring device, stir until completely dissolved, slowly drop 1 mol / L sodium hydroxide solution, adjust the pH value to 10, heat to 80° C., react for 9 h, filter and wash the product until it is neutral, dry it at 60° C. for 12 h, grind it and place it in a muffle furnace, calcine it at 500° C. for 4 h, and cool it to obtain a copper-aluminum nanocomposite oxide;
[0056] 2) Weigh 10 g of copper-aluminum nanocomposite oxide and 200 mL of deionized water, place them in a reaction kettle, stir to disperse them evenly, add 4 g of molybdenum nitrate hexahydrate, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 130° C., react for 3 h, cool the product, wash and dry it, place it in a muffle furnace, and calcine it at 400° C. for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0057] 3) Weigh 10 g of copper-aluminum nanocomposite oxide loaded with active components and 300 mL of 50% ethanol aqueous solution, place in a three-necked flask, add 20 g of dimethylsiloxane, 30 g of phenylsiloxane and 5 mL of 1 mol / L ammonia water, heat to 90 ° C, react for 12 h, wash and dry the product and shape it into strips;
[0058] The method for preparing the catalyst used in step S3 of this embodiment is different from the method for preparing the catalyst used in steps S1 and S2 in that:
[0059] 2) Weigh 10 g of nanocomposite oxide and 200 mL of deionized water, place in a reaction kettle, stir to disperse evenly, add 4 g of palladium chloride, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 130°C, react for 3 h, cool the product, wash, dry, place in a muffle furnace, and calcine at 400°C for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0060] The remaining steps are the same as the preparation method of the catalyst used in steps S1 and S2.
[0061] Example 3
[0062] The method for preparing HVO from bio-oil of this embodiment comprises the following steps:
[0063] S1: Soybean oil and hydrogen were mixed in a hydrogen-to-oil volume ratio of 500:1 and fed into a reactor with an expanded bed. The reactor was equipped with 8 catalyst beds, the pressure was set at 10 MPa, and the space velocity was 0.8 h -1 The reaction adopts a hot high-separation oil process, sets the circulation ratio of the hot high-separation oil circulation pump to 3:1, adjusts the circulating oil volume to control the reaction inlet temperature to 300°C, and obtains a C5-500°C fraction;
[0064] S2: The C5-500℃ fraction and hydrogen are mixed in a hydrogen-to-oil volume ratio of 800:1 and fed into a fixed bed reactor. The reactor is equipped with 5 catalyst beds, with cooling hydrogen facilities between the beds. The pressure is set at 10MPa and the space velocity is 1.0h -1 The large-scale device reaction adopts the hot high-oil separation process, and the reaction inlet temperature is controlled at 300°C. The small-scale device reaction adopts the cold high-oil separation process, and a stripping tower is set to remove hydrogen sulfide, ammonia, carbon monoxide and other gases to obtain the C5+ fraction;
[0065] S3: The C5+ fraction and hydrogen are mixed in a hydrogen-to-oil volume ratio of 500:1 and fed into a fixed bed reactor. The reactor is equipped with three catalyst beds, with hydrogen cooling facilities between the beds. The pressure is set at 10 MPa and the space velocity is 1.2 h -1 The large-scale device reaction adopts the hot high-oil separation process, and the reaction inlet temperature is controlled at 330°C. The small-scale device reaction adopts the cold high-oil separation process, adopts a one-time process, sets a fractionation tower, and produces HVO at the bottom of the fractionation tower;
[0066] The method for preparing the catalyst used in steps S1 and S2 in this embodiment comprises the following steps:
[0067] 1) Weigh 5 g of aluminum nitrate nonahydrate, 10 g of copper nitrate trihydrate and 500 mL of deionized water, place in a three-necked flask equipped with a stirring device, stir until completely dissolved, slowly drop 1 mol / L sodium hydroxide solution, adjust the pH value to 10, heat to 70° C., react for 12 h, filter and wash the product until it is neutral, dry it at 60° C. for 12 h, grind it and place it in a muffle furnace, calcine it at 500° C. for 4 h, and cool it to obtain a copper-aluminum nanocomposite oxide;
[0068] 2) Weigh 10 g of copper-aluminum nanocomposite oxide and 200 mL of deionized water, place them in a reaction kettle, stir to disperse them evenly, add 4 g of cobalt nitrate hexahydrate, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 120° C., react for 5 h, cool the product, wash and dry it, place it in a muffle furnace, and calcine it at 400° C. for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0069] 3) Weigh 10 g of copper-aluminum nanocomposite oxide loaded with active components and 300 mL of 50% ethanol aqueous solution, place in a three-necked flask, add 50 g of phenylsiloxane and 5 mL of 1 mol / L ammonia water, heat to 80 ° C, react for 15 h, wash and dry the product and shape it into a sphere;
[0070] The method for preparing the catalyst used in step S3 of this embodiment is different from the method for preparing the catalyst used in steps S1 and S2 in that:
[0071] 2) Weigh 10 g of nanocomposite oxide and 200 mL of deionized water, place in a reaction kettle, stir to disperse evenly, add 4 g of platinum chloride, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 120°C, react for 5 h, cool the product, wash and dry it, place it in a muffle furnace, and calcine it at 400°C for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0072] The remaining steps are the same as the preparation method of the catalyst used in steps S1 and S2.
[0073] Example 4
[0074] The method for preparing HVO from bio-oil in this embodiment is the same as that in Example 3;
[0075] The preparation method of the catalyst used in steps S1 and S2 in this embodiment is different from that in embodiment 3 in that:
[0076] 1) Weigh 17 g of aluminum nitrate nonahydrate, 10 g of copper nitrate trihydrate and 500 mL of deionized water, place in a three-necked flask equipped with a stirring device, stir until completely dissolved, slowly drop 1 mol / L sodium hydroxide solution, adjust the pH value to 10, heat to 70° C., react for 12 h, filter and wash the product until it is neutral, dry it at 60° C. for 12 h, grind it and place it in a muffle furnace, calcine it at 500° C. for 4 h, and cool it to obtain a copper-aluminum nanocomposite oxide;
[0077] The remaining steps are the same as those in Example 3;
[0078] The method for preparing the catalyst used in step S3 of this embodiment is different from the method for preparing the catalyst used in steps S1 and S2 in that:
[0079] 2) Weigh 10 g of nanocomposite oxide and 200 mL of deionized water, place in a reaction kettle, stir to disperse evenly, add 4 g of platinum chloride, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 120°C, react for 5 h, cool the product, wash and dry it, place it in a muffle furnace, and calcine it at 400°C for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0080] The remaining steps are the same as the preparation method of the catalyst used in steps S1 and S2.
[0081] Example 5
[0082] The method for preparing HVO from bio-oil in this embodiment is the same as that in Example 3;
[0083] The preparation method of the catalyst used in steps S1 and S2 in this embodiment is different from that in embodiment 3 in that:
[0084] 1) Weigh 12 g of aluminum nitrate nonahydrate, 10 g of copper nitrate trihydrate and 500 mL of deionized water, place in a three-necked flask equipped with a stirring device, stir until completely dissolved, slowly drop 1 mol / L sodium hydroxide solution, adjust the pH value to 10, heat to 70° C., react for 12 h, filter and wash the product until it is neutral, dry it at 60° C. for 12 h, grind it and place it in a muffle furnace, calcine it at 500° C. for 4 h, and cool it to obtain a copper-aluminum nanocomposite oxide;
[0085] The remaining steps are the same as those in Example 3;
[0086] The method for preparing the catalyst used in step S3 of this embodiment is different from the method for preparing the catalyst used in steps S1 and S2 in that:
[0087] 2) Weigh 10 g of nanocomposite oxide and 200 mL of deionized water, place in a reaction kettle, stir to disperse evenly, add 4 g of platinum chloride, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 120°C, react for 5 h, cool the product, wash and dry it, place it in a muffle furnace, and calcine it at 400°C for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0088] The remaining steps are the same as the preparation method of the catalyst used in steps S1 and S2.
[0089] Example 6
[0090] The method for preparing HVO from bio-oil in this embodiment is the same as that in Example 5;
[0091] The method for preparing the catalyst used in steps S1 and S2 in this embodiment is different from that in embodiment 5 in that:
[0092] 2) Weigh 10 g of copper-aluminum nanocomposite oxide and 200 mL of deionized water, place them in a reaction kettle, stir to disperse them evenly, add 15 g of cobalt nitrate hexahydrate, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 120° C., react for 5 h, cool the product, wash and dry it, place it in a muffle furnace, and calcine it at 400° C. for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0093] The remaining steps are the same as those in Example 5;
[0094] The method for preparing the catalyst used in step S3 of this embodiment is different from the method for preparing the catalyst used in steps S1 and S2 in that:
[0095] 2) Weigh 10 g of nanocomposite oxide and 200 mL of deionized water, place in a reaction kettle, stir to disperse evenly, add 15 g of platinum chloride, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 120°C, react for 5 h, cool the product, wash and dry it, place it in a muffle furnace, and calcine it at 400°C for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0096] The remaining steps are the same as the preparation method of the catalyst used in steps S1 and S2.
[0097] Example 7
[0098] The method for preparing HVO from bio-oil in this embodiment is the same as that in Example 5;
[0099] The method for preparing the catalyst used in steps S1 and S2 in this embodiment is different from that in embodiment 5 in that:
[0100] 2) Weigh 10 g of copper-aluminum nanocomposite oxide and 200 mL of deionized water, place them in a reaction kettle, stir to disperse them evenly, add 12 g of cobalt nitrate hexahydrate, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 120° C., react for 5 h, cool the product, wash and dry it, place it in a muffle furnace, and calcine it at 400° C. for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0101] The remaining steps are the same as those in Example 5;
[0102] The method for preparing the catalyst used in step S3 of this embodiment is different from the method for preparing the catalyst used in steps S1 and S2 in that:
[0103] 2) Weigh 10 g of nanocomposite oxide and 200 mL of deionized water, place in a reaction kettle, stir to disperse evenly, add 12 g of platinum chloride, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 120°C, react for 5 h, cool the product, wash and dry it, place it in a muffle furnace, and calcine it at 400°C for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0104] The remaining steps are the same as the preparation method of the catalyst used in steps S1 and S2.
[0105] Example 8
[0106] The method for preparing HVO from bio-oil in this embodiment is the same as that in Example 7;
[0107] The method for preparing the catalyst used in steps S1 and S2 in this embodiment is different from that in embodiment 7 in that:
[0108] 3) Weigh 10 g of copper-aluminum nanocomposite oxide loaded with active components and 300 mL of 50% ethanol aqueous solution, place in a three-necked flask, add 200 g of phenylsiloxane and 5 mL of 1 mol / L ammonia water, heat to 80 ° C, react for 15 h, wash and dry the product and shape it into a sphere;
[0109] The remaining steps are the same as those in Example 7;
[0110] The method for preparing the catalyst used in step S3 of this embodiment is different from the method for preparing the catalyst used in steps S1 and S2 in that:
[0111] 2) Weigh 10 g of nanocomposite oxide and 200 mL of deionized water, place in a reaction kettle, stir to disperse evenly, add 12 g of platinum chloride, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 120°C, react for 5 h, cool the product, wash and dry it, place it in a muffle furnace, and calcine it at 400°C for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0112] The remaining steps are the same as the preparation method of the catalyst used in steps S1 and S2.
[0113] Example 9
[0114] The method for preparing HVO from bio-oil in this embodiment is the same as that in Example 7;
[0115] The method for preparing the catalyst used in steps S1 and S2 in this embodiment is different from that in embodiment 7 in that:
[0116] 3) Weigh 10 g of copper-aluminum nanocomposite oxide loaded with active components and 300 mL of 50% ethanol aqueous solution, place in a three-necked flask, add 100 g of phenylsiloxane and 5 mL of 1 mol / L ammonia water, heat to 80 ° C, react for 15 h, wash and dry the product and shape it into a sphere;
[0117] The remaining steps are the same as those in Example 7;
[0118] The method for preparing the catalyst used in step S3 of this embodiment is different from the method for preparing the catalyst used in steps S1 and S2 in that:
[0119] 2) Weigh 10 g of nanocomposite oxide and 200 mL of deionized water, place in a reaction kettle, stir to disperse evenly, add 12 g of platinum chloride, 15 g of urea and 3.7 g of ammonium fluoride, stir evenly, heat to 120°C, react for 5 h, cool the product, wash and dry it, place it in a muffle furnace, and calcine it at 400°C for 3 h to obtain a copper-aluminum nanocomposite oxide loaded with active components;
[0120] The remaining steps are the same as the preparation method of the catalyst used in steps S1 and S2.
[0121] Comparative Example
[0122] Comparative Example 1
[0123] The method for preparing HVO from bio-oil of this comparative example comprises the following steps:
[0124] S1: Soybean oil and hydrogen were mixed in a hydrogen-to-oil volume ratio of 500:1 and fed into a reactor with an expanded bed. The reactor was equipped with 8 catalyst beds, the pressure was set at 10 MPa, and the space velocity was 0.8 h -1The reaction adopts a hot high-separation oil process, sets the circulation ratio of the hot high-separation oil circulation pump to 3:1, adjusts the circulating oil volume to control the reaction inlet temperature to 300°C, and obtains a C5-500°C fraction;
[0125] S2: The C5-500℃ fraction and hydrogen are mixed in a hydrogen-to-oil volume ratio of 800:1 and fed into a fixed bed reactor. The reactor is equipped with 5 catalyst beds, with cooling hydrogen facilities between the beds. The pressure is set at 10MPa and the space velocity is 1.0h -1 The large-scale device reaction adopts the hot high-oil separation process, and the reaction inlet temperature is controlled at 300°C. The small-scale device reaction adopts the cold high-oil separation process, and a stripping tower is set to remove hydrogen sulfide, ammonia, carbon monoxide and other gases to obtain the C5+ fraction;
[0126] S3: The C5+ fraction and hydrogen are mixed in a hydrogen-to-oil volume ratio of 500:1 and fed into a fixed bed reactor. The reactor is equipped with three catalyst beds, with hydrogen cooling facilities between the beds. The pressure is set at 10 MPa and the space velocity is 1.2 h -1 The large-scale device reaction adopts the hot high-oil separation process, and the reaction inlet temperature is controlled at 330°C. The small-scale device reaction adopts the cold high-oil separation process, adopts a one-time process, sets a fractionation tower, and produces HVO at the bottom of the fractionation tower;
[0127] The catalyst used in steps S1 and S2 in this comparative example is a mixture of copper oxide and cobalt oxide;
[0128] The catalyst used in step S3 in this comparative example is platinum chloride.
[0129] Comparative Example 2
[0130] The method for preparing HVO from bio-oil in this comparative example is the same as that in Example 3;
[0131] The preparation method of the catalyst used in steps S1 and S2 in this comparative example comprises the following steps:
[0132] Weigh 10g of a mixture of copper oxide and cobalt oxide and 300mL of a 50% ethanol aqueous solution in a three-necked flask, add 50g of phenylsiloxane and 5mL of 1mol / L ammonia water, heat to 80°C, react for 15h, wash and dry the product, and shape it into a sphere.
[0133] The catalyst used in step S3 in this comparative example is platinum chloride.
[0134] Performance testing
[0135] Detection Methods
[0136] 1. HVO yield test: HVO yield = HVO flow / soybean oil flow × 100%. The test results are as follows: Figure 1 shown.
[0137] 2. HVO quality test: Referring to the limits class A index requirements of EN15940 standard, the quality indexes of the HVO products of Examples 1-9 and Comparative Examples 1-2 were tested. The test results are shown in Table 1.
[0138] Table 1 HVO product quality test results of Examples 1-9 and Comparative Examples 1-2
[0139]
[0140] Results Analysis
[0141] contrast Figure 1 It can be seen from the data of Examples 1-3 and Comparative Examples 1-2 that after the hydrogenation catalyst is modified, the yield and quality of HVO are improved to a certain extent, indicating that after the hydrogenation catalyst is modified, the harm of impurities and moisture to the catalyst is reduced and the catalytic activity is improved.
[0142] contrast Figure 1 It can be seen from the data of Examples 3-5 that when the mass ratio of copper oxide to aluminum oxide increases, the yield and quality of HVO are improved to a certain extent. However, when the mass ratio of copper to aluminum is too large, the yield and quality of HVO remain basically unchanged, or even slightly decrease.
[0143] contrast Figure 1 It can be seen from the data of Examples 5-7 that with the increase of the active component loading on the copper-aluminum nanocomposite oxide, the yield and quality of HVO are improved. However, when the active component loading on the copper-aluminum nanocomposite oxide is too large, the yield and quality of HVO are slightly reduced, which may be due to the uneven dispersion of the active component.
[0144] contrast Figure 1 It can be seen from the data of Examples 7-9 that with the increase in the amount of organosiloxane added, the yield and quality of HVO are improved to a certain extent, which may be because the hydrophobicity of the catalyst is improved, reducing the effect of moisture on the catalyst and the hydrogenation reaction.
[0145] It can be seen from Table 1 that the HVO of Examples 1-9 can meet all the indicators under limits class A required by the EN15940 standard.
[0146] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for preparing HVO from bio-oil, characterized in that: The steps include: S1: Mix the bio-oil and hydrogen into a reactor, and obtain a C5-500℃ fraction through a hydrogenation pretreatment process under the action of a catalyst; S2: Mix the C5-500℃ fraction and hydrogen and enter the reactor. Under the action of the catalyst, the C5+ fraction is obtained through a hydrogenation refining process. S3: Mix the C5+ fraction and hydrogen and enter the reactor. Under the action of the catalyst, the HVO is obtained by a single process through hydrogenation isomerization. The catalyst in steps S1 and S2 is a modified copper-aluminum nanocomposite oxide loaded with a non-noble metal in an oxidized state, and the non-noble metal is one of cobalt, molybdenum, tungsten, cerium, iron and nickel; In step S3, the catalyst is a modified copper-aluminum nanocomposite oxide loaded with precious metal nanoparticles, and the precious metal is one of silver, platinum, palladium, rhodium and ruthenium; The preparation method of the catalyst comprises the following steps: 1) dissolving aluminum nitrate nonahydrate and copper nitrate trihydrate in water, adjusting the pH value to 9-10, heating to 60-80° C., reacting for 9-15 hours, filtering, washing, drying, grinding, calcining, and cooling to obtain copper-aluminum nanocomposite oxide; the mass ratio of aluminum nitrate nonahydrate to copper nitrate trihydrate is (0.5-1.7):1; 2) Dispersing the copper-aluminum nanocomposite oxide in water, adding the precursor of the active component, urea and ammonium fluoride, stirring evenly, heating to 110-130° C., reacting for 3-6 hours, washing, drying, calcining and cooling the product to obtain the copper-aluminum nanocomposite oxide loaded with the active component; the mass ratio of the copper-aluminum nanocomposite oxide to the precursor of the active component is 1:(0.4-1.5); 3) Dispersing the copper-aluminum nanocomposite oxide loaded with active components in an ethanol aqueous solution, adding organosiloxane and ammonia water, heating to 70-90° C., reacting for 12-24 hours, washing, drying and molding; the organosiloxane is one or more of methyltrimethoxysilane, dimethylsiloxane, phenylsiloxane and vinylsiloxane; the mass ratio of the copper-aluminum nanocomposite oxide loaded with active components to the organosiloxane is 1:(5-20).
2. The method for preparing HVO from bio-oil according to claim 1, characterized in that: The biological oil in step S1 is one or more of vegetable oil, animal fat or waste cooking oil.
3. The method for preparing HVO from bio-oil according to claim 1, characterized in that: In step S1, the reactor adopts a fully mixed flow reactor or a reactor with an expanded bed, the reactor is provided with 3-8 catalyst beds, the reaction adopts a hot high oil separation process, the circulation ratio of the hot high oil separation circulation pump is 1:1-5:1, the hydrogen oil volume ratio is 300:1-900:1, and the reaction conditions are: pressure 5-15MPa, temperature 200-400°C, space velocity 0.2-1.2h -1 In step S2, the reactor is a fixed bed reactor and a stripping tower is provided. The reactor is provided with 3-8 catalyst beds, and a cold hydrogen facility is provided between the beds. The large-scale device reaction adopts a hot high-oil separation process, and the small-scale device reaction adopts a cold high-oil separation process. The hydrogen-oil volume ratio is 200:1-1500:1, and the reaction conditions are: pressure 4-15MPa, temperature 200-380°C, and space velocity 0.3-2h -1 In step S3, the reactor is a fixed bed reactor and a fractionation tower is provided. The reactor is provided with 2-5 catalyst beds, and a cold hydrogen facility is provided between the beds. The large-scale device reaction adopts a hot high-oil separation process, and the small-scale device reaction adopts a cold high-oil separation process. The hydrogen-oil volume ratio is 200:1-700:1, and the reaction conditions are: pressure 4-15MPa, temperature 250-380°C, and space velocity 0.5-2h -1 .
4. The method for preparing HVO from bio-oil according to claim 1, characterized in that: The catalyst is in the shape of a sphere, a cylinder or a strip.