A kind of anti-corrosion and environmentally friendly foam plastic insulation pipe and preparation method thereof
By using rare earth nanomodified polyurethane foam material and high-density polyethylene external protective layer in rigid polyurethane foam insulation pipes, the problem of poor insulation effect in the northern high-altitude areas is solved, and more efficient insulation and corrosion resistance are achieved. Reduces energy consumption and carbon emissions.
Patent Information
- Application Number
- CN202410488646.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-04-23
AI Technical Summary
The existing rigid polyurethane foam insulation pipes have poor insulation effects in the northern high-altitude areas, resulting in increased energy consumption and increased carbon emissions, and the dimensional stability of the material is relatively average.
Rare earth nanomodified polyurethane foam material is used as the insulation layer, and high-density polyethylene material in the steel pipe jacket is used as the outer protective layer. The closed porosity and bonding strength of the material are improved through specific preparation methods to form more efficient insulation performance.
It significantly improves the insulation effect, reduces water absorption and heat loss, enhances anti-corrosion performance, and has low process cost and more environmentally friendly materials. Compared with the thermal insulation pipes, the insulation effect is 5-10 times higher than that of commercially available insulation pipes.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of advanced petrochemical new materials, and in particular to an anti-corrosion and environmentally friendly foam plastic thermal insulation pipe and a preparation method thereof. Background Art
[0002] Foam insulation pipe has many characteristics such as heat preservation, thermal insulation, waterproof, sound insulation, cold resistance, flame retardant, corrosion resistance, light capacity, high strength, simple and quick construction, etc. It is more and more widely used. With its gradual promotion, it has become an important pipeline in the fields of construction, transportation, petroleum, chemical industry, electricity, refrigeration, etc. Direct buried insulation pipe is mostly used for various indoor and outdoor pipelines.
[0003] Compared with traditional insulation pipes, the use of polyurethane insulation pipes can further reduce energy transportation costs, and has better insulation performance and lower costs. At the same time, it has strong waterproof performance and its service life is greatly improved compared to traditional insulation pipes.
[0004] Prior art, application number "201510894298.X", a rigid polyurethane foam plastic spray insulation pipe and a spraying method, specifically discloses "a rigid polyurethane foam plastic spray insulation pipe and a spraying method. Traditional rigid polyurethane foam plastic insulation pipes have excellent insulation effects in low-cold areas of my country, but when used in high-cold areas in the north, due to the uneven distribution of the lowest temperature in the natural environment and the prescribed polyurethane insulation layer thickness standard, the insulation effect is poor, resulting in increased energy consumption and increased carbon emissions. A rigid polyurethane foam plastic spray insulation pipe, which comprises: a working pipe, a rigid polyurethane plastic foam spray insulation layer, the working pipe (1) has a rigid polyurethane plastic foam spray insulation layer (2) outside, the working pipe is a hard straight pipe, and the material of the working pipe can be a steel pipe or a plastic pipe. The present invention is applied to a rigid polyurethane foam plastic spray insulation pipe and a spraying method", which mainly uses conventional rigid polyurethane as the insulation layer, the closed cell rate is relatively low, and its dimensional stability performance is relatively general.
[0005] Based on this, we proposed an anti-corrosion and environmentally friendly foam plastic insulation pipe, hoping to solve the shortcomings of the existing technology. Summary of the invention
[0006] 1. Technical issues to be resolved
[0007] In view of the deficiencies in the prior art, the present invention provides an anti-corrosion and environmentally friendly foam plastic thermal insulation pipe and a preparation method thereof.
[0008] (II) Technical solution
[0009] To achieve the above-mentioned purpose, the present invention provides the following technical solutions:
[0010] An anti-corrosion and environmentally friendly foam plastic insulation pipe, with an outer protective layer on the outer jacket of a steel pipe;
[0011] A thermal insulation layer is provided between the steel pipe and the outer protective layer;
[0012] The thermal insulation layer is made of rare earth nano-modified polyurethane foam plastic material;
[0013] The outer protective layer is made of high-density polyethylene material.
[0014] As a further technical solution, the rare earth nano-modified polyurethane foam plastic comprises the following components by weight: 80-90 parts of polyol, 30-40 parts of isocyanate, 4-6 parts of rare earth modified nano-bentonite, 0.1-0.15 parts of stannous octoate, 0.8-1.2 parts of surfactant, 0.3-0.5 parts of diethanolamine, and 4-6 parts of deionized water.
[0015] As a further technical solution, the method for preparing the rare earth modified nano bentonite is:
[0016] (1) First, disperse nano-bentonite in deionized water and perform ultrasonic dispersion for 10 min to obtain a nano-bentonite dispersion;
[0017] (2) adjusting the pH of the nano-bentonite dispersion prepared above, specifically: adjusting the pH of the nano-bentonite dispersion obtained above to 3-4, then adding rare earth chloride, adjusting the temperature to 70° C., keeping the temperature for 2 hours, and then filtering to obtain pretreated nano-bentonite;
[0018] (3) adding the pretreated nano-bentonite to toluene for ultrasonic dispersion, adding 3-aminopropyltriethoxysilane, adjusting the temperature to 102-106° C., stirring for 4 hours, filtering, washing with anhydrous ethanol, and drying to obtain rare earth modified nano-bentonite.
[0019] As a further technical solution: the mass fraction of nano-bentonite in the nano-bentonite dispersion in step (1) is 10-12%.
[0020] As a further technical solution: in step (2), the pH of the nano-bentonite dispersion is adjusted using a 5% by mass nitric acid solution;
[0021] The mixing mass ratio of the nano-bentonite dispersion to the rare earth chloride is 1000:1-1.6.
[0022] As a further technical solution, the rare earth chloride is cerium chloride or lanthanum chloride.
[0023] As a further technical solution, the mixing ratio of the pretreated nano-bentonite and toluene in step (3) is 10-15 g: 120 mL;
[0024] The pretreated nano-bentonite and 3-aminopropyltriethoxysilane are mixed in a mass ratio of 3:1.
[0025] As a further technical solution, the surfactant is an organosilicon surfactant.
[0026] As a further technical solution, the polyol is a polyether polyol.
[0027] A method for preparing an anti-corrosion and environmentally friendly foam plastic thermal insulation pipe, comprising:
[0028] Weigh the following according to weight parts: polyol, rare earth modified nano bentonite, stannous octoate, surfactant, diethanolamine, isocyanate, and deionized water;
[0029] Adding polyol, rare earth modified nano bentonite, stannous octoate, surfactant, diethanolamine and deionized water into a mixer in sequence, stirring and mixing, to obtain a first mixture;
[0030] Add isocyanate to the first mixture, stir and mix again, inject between the steel pipe and the outer protective layer, and then foam and shape.
[0031] The material of polyurethane insulation pipe is hard polyurethane foam, which fully fills the gap between steel pipe and casing, and has a certain bonding strength, so that the steel pipe, outer casing and insulation layer form a solid whole. The insulation pipe made of this raw material has good thermal insulation performance, extremely low heat loss, and can greatly save energy in long-term operation.
[0032] After multiple experiments and certifications, the temperature resistance, thermal conductivity and environmental performance of polyurethane insulation pipes have reached high standards. It is a real high-performance product with thermal insulation and corrosion resistance. It can play an important role in the urban thermal pipeline industry.
[0033] (III) Beneficial effects
[0034] Compared with the prior art, the present invention provides an anti-corrosion and environmentally friendly foam plastic insulation pipe, which has the following beneficial effects:
[0035] The anti-corrosion and environmentally friendly foam plastic insulation pipe prepared by the present invention adopts high-density polyethylene as the outer protective layer and adopts rare earth nano-modified polyurethane foam plastic material to make the insulation layer. It not only has excellent anti-corrosion performance, but also has excellent thermal insulation performance, low processing cost, and more environmentally friendly process materials. Compared with commercially available insulation pipes, the insulation effect is improved by 5-10 times.
[0036] The present invention adopts rare earth nano-modified polyurethane foam plastic material to make the insulation layer, and its water absorption rate is very low, and the average water absorption rate is maintained at 0.16kg / m 2 The lower water absorption rate is mainly due to the higher closed-pore rate in the insulation layer, which not only reduces the water absorption rate, but also significantly improves the insulation effect of the insulation pipe. In pipeline transportation, it can greatly reduce the heat loss during transportation.
[0037] The present invention adopts rare earth nano-modified polyurethane foam plastic material to make the insulation layer. During the molding process of the nano-modified polyurethane foam plastic, it will be tightly bonded to the outer surface of the steel pipe and the inner surface of the outer protective layer, thereby tightly combining the two together, which can effectively isolate the penetration of corrosion factors, thereby greatly protecting the steel pipe and reducing corrosion. DETAILED DESCRIPTION
[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] An anti-corrosion and environmentally friendly foam plastic insulation pipe, with an outer protective layer on the outer jacket of a steel pipe;
[0040] A thermal insulation layer is provided between the steel pipe and the outer protective layer;
[0041] The thermal insulation layer is made of rare earth nano-modified polyurethane foam plastic material;
[0042] The outer protective layer is made of high-density polyethylene material.
[0043] The rare earth nano-modified polyurethane foam plastic comprises the following components by weight: 80-90 parts of polyol, 30-40 parts of isocyanate, 4-6 parts of rare earth modified nano-bentonite, 0.1-0.15 parts of stannous octoate, 0.8-1.2 parts of surfactant, 0.3-0.5 parts of diethanolamine and 4-6 parts of deionized water.
[0044] The preparation method of the rare earth modified nano bentonite is:
[0045] (1) First, disperse nano-bentonite in deionized water and perform ultrasonic dispersion for 10 min to obtain a nano-bentonite dispersion;
[0046] (2) adjusting the pH of the nano-bentonite dispersion prepared above, specifically: adjusting the pH of the nano-bentonite dispersion obtained above to 3-4, then adding rare earth chloride, adjusting the temperature to 70° C., keeping the temperature for 2 hours, and then filtering to obtain pretreated nano-bentonite;
[0047] (3) adding the pretreated nano-bentonite to toluene for ultrasonic dispersion, adding 3-aminopropyltriethoxysilane, adjusting the temperature to 102-106° C., stirring for 4 hours, filtering, washing with anhydrous ethanol, and drying to obtain rare earth modified nano-bentonite.
[0048] The mass fraction of nano-bentonite in the nano-bentonite dispersion in step (1) is 10-12%.
[0049] In step (2), the pH of the nano-bentonite dispersion is adjusted using a 5% nitric acid solution;
[0050] The mixing mass ratio of the nano-bentonite dispersion to the rare earth chloride is 1000:1-1.6.
[0051] The rare earth chloride is cerium chloride or lanthanum chloride.
[0052] When cerium chloride is used, the prepared rare earth nano-modified polyurethane foam plastic material has more advantages in thermal insulation performance, while when lanthanum chloride is used, the prepared rare earth nano-modified polyurethane foam plastic material has a more obvious improvement effect in improving dimensional stability.
[0053] The mixing ratio of the pretreated nano-bentonite and toluene in step (3) is 10-15 g: 120 mL;
[0054] The pretreated nano-bentonite and 3-aminopropyltriethoxysilane are mixed in a mass ratio of 3:1.
[0055] The surfactant is an organic silicon surfactant.
[0056] The polyol is a polyether polyol.
[0057] A method for preparing an anti-corrosion and environmentally friendly foam plastic thermal insulation pipe, comprising:
[0058] Weigh the following according to weight parts: polyol, rare earth modified nano bentonite, stannous octoate, surfactant, diethanolamine, isocyanate, and deionized water;
[0059] Adding polyol, rare earth modified nano bentonite, stannous octoate, surfactant, diethanolamine and deionized water into a mixer in sequence, stirring and mixing, to obtain a first mixture;
[0060] Add isocyanate to the first mixture, stir and mix again, inject between the steel pipe and the outer protective layer, and then foam and shape.
[0061] The anti-corrosion and environmentally friendly foam plastic insulation pipe is tested, and the product quality of the present invention reaches various physical and chemical performance indicators of GB / T29046-2012 and GB / T29047-2012, and is packaged and stored after passing the test.
[0062] The anti-corrosion and environmentally friendly foam plastic insulation pipe prepared by the present invention can be widely used in liquid and gas transportation pipelines, specifically in chemical pipelines, insulation engineering petroleum, central heating networks, central air-conditioning ventilation ducts, municipal engineering and other fields.
[0063] According to calculations by the applicant, under normal circumstances, the anti-corrosion and environmentally friendly foam plastic insulation pipe prepared by the present invention can reduce the project cost by about 27.5%.
[0064] The following are specific embodiments:
[0065] Example 1
[0066] An anti-corrosion and environmentally friendly foam plastic insulation pipe, an outer protective layer is arranged on the outer sleeve of a steel pipe; an insulation layer is arranged between the steel pipe and the outer protective layer; the insulation layer is made of rare earth nano-modified polyurethane foam plastic material; the outer protective layer is made of high-density polyethylene material. The rare earth nano-modified polyurethane foam plastic comprises the following components by weight: 80 parts of polyether polyol, 30 parts of isocyanate, 4 parts of rare earth modified nano-bentonite, 0.1 parts of stannous octoate, 0.8 parts of organosilicon surfactant, 0.3 parts of diethanolamine, and 4 parts of deionized water.
[0067] The preparation method of rare earth modified nano bentonite is:
[0068] (1) First, disperse nano-bentonite in deionized water and disperse it by ultrasonic for 10 minutes to obtain a nano-bentonite dispersion; the mass fraction of nano-bentonite in the nano-bentonite dispersion is 10%.
[0069] (2) adjusting the pH of the nano-bentonite dispersion prepared above, specifically: adjusting the pH of the nano-bentonite dispersion obtained above to 3, then adding rare earth chloride, adjusting the temperature to 70° C., keeping the temperature for 2 hours, and then filtering to obtain pretreated nano-bentonite; adjusting the pH of the nano-bentonite dispersion with a 5% by mass nitric acid solution; the mass ratio of the nano-bentonite dispersion to the rare earth chloride is 1000:1.
[0070] The rare earth chloride is lanthanum chloride.
[0071] (3) Add the pretreated nano-bentonite to toluene for ultrasonic dispersion, then add 3-aminopropyltriethoxysilane, adjust the temperature to 102°C, keep stirring for 4 hours, then filter, wash with anhydrous ethanol, and dry to obtain rare earth modified nano-bentonite; the mixing ratio of the pretreated nano-bentonite and toluene is 10g:120mL; the mixing mass ratio of the pretreated nano-bentonite and 3-aminopropyltriethoxysilane is 3:1.
[0072] Example 2
[0073] An anti-corrosion and environmentally friendly foam plastic insulation pipe, an outer protective layer is arranged on the outer sleeve of a steel pipe; an insulation layer is arranged between the steel pipe and the outer protective layer; the insulation layer is made of rare earth nano-modified polyurethane foam plastic material; the outer protective layer is made of high-density polyethylene material. The rare earth nano-modified polyurethane foam plastic comprises the following components by weight: 80 parts of polyether polyol, 30 parts of isocyanate, 4 parts of rare earth modified nano-bentonite, 0.1 parts of stannous octoate, 0.8 parts of organosilicon surfactant, 0.3 parts of diethanolamine, and 4 parts of deionized water.
[0074] The preparation method of rare earth modified nano bentonite is:
[0075] (1) First, disperse nano-bentonite in deionized water and disperse it by ultrasonic for 10 minutes to obtain a nano-bentonite dispersion; the mass fraction of nano-bentonite in the nano-bentonite dispersion is 10%.
[0076] (2) adjusting the pH of the nano-bentonite dispersion prepared above, specifically: adjusting the pH of the nano-bentonite dispersion obtained above to 3, then adding rare earth chloride, adjusting the temperature to 70° C., keeping the temperature for 2 hours, and then filtering to obtain pretreated nano-bentonite; adjusting the pH of the nano-bentonite dispersion with a 5% by mass nitric acid solution; the mass ratio of the nano-bentonite dispersion to the rare earth chloride is 1000:1.
[0077] The rare earth chloride is cerium chloride.
[0078] (3) Add the pretreated nano-bentonite to toluene for ultrasonic dispersion, then add 3-aminopropyltriethoxysilane, adjust the temperature to 102°C, keep stirring for 4 hours, then filter, wash with anhydrous ethanol, and dry to obtain rare earth modified nano-bentonite; the mixing ratio of the pretreated nano-bentonite and toluene is 10g:120mL; the mixing mass ratio of the pretreated nano-bentonite and 3-aminopropyltriethoxysilane is 3:1.
[0079] Example 3
[0080] An anti-corrosion and environmentally friendly foam plastic insulation pipe, an outer protective layer is arranged on the outer sleeve of a steel pipe; an insulation layer is arranged between the steel pipe and the outer protective layer; the insulation layer is made of rare earth nano-modified polyurethane foam plastic material; the outer protective layer is made of high-density polyethylene material. The rare earth nano-modified polyurethane foam plastic comprises the following components by weight: 85 parts of polyether polyol, 36 parts of isocyanate, 5 parts of rare earth modified nano-bentonite, 0.12 parts of stannous octoate, 0.9 parts of organosilicon surfactant, 0.4 parts of diethanolamine, and 5 parts of deionized water.
[0081] The preparation method of rare earth modified nano bentonite is:
[0082] (1) First, disperse nano-bentonite in deionized water and disperse it by ultrasonic for 10 minutes to obtain a nano-bentonite dispersion; the mass fraction of nano-bentonite in the nano-bentonite dispersion is 11.5%.
[0083] (2) adjusting the pH of the nano-bentonite dispersion prepared above, specifically: adjusting the pH of the nano-bentonite dispersion obtained above to 3.8, then adding rare earth chloride, adjusting the temperature to 70° C., keeping the temperature for 2 hours, and then filtering to obtain pretreated nano-bentonite; adjusting the pH of the nano-bentonite dispersion with a 5% by mass nitric acid solution; the mass ratio of the nano-bentonite dispersion to the rare earth chloride is 1000:1.2.
[0084] The rare earth chloride is cerium chloride.
[0085] (3) Add the pretreated nano-bentonite to toluene for ultrasonic dispersion, then add 3-aminopropyltriethoxysilane, adjust the temperature to 103°C, keep stirring for 4 hours, then filter, wash with anhydrous ethanol, and dry to obtain rare earth modified nano-bentonite; the mixing ratio of the pretreated nano-bentonite and toluene is 12g:120mL; the mixing mass ratio of the pretreated nano-bentonite and 3-aminopropyltriethoxysilane is 3:1.
[0086] Example 4
[0087] An anti-corrosion and environmentally friendly foam plastic insulation pipe, an outer protective layer is arranged on the outer sleeve of a steel pipe; an insulation layer is arranged between the steel pipe and the outer protective layer; the insulation layer is made of rare earth nano-modified polyurethane foam plastic material; the outer protective layer is made of high-density polyethylene material. The rare earth nano-modified polyurethane foam plastic comprises the following components by weight: 90 parts of polyether polyol, 40 parts of isocyanate, 6 parts of rare earth modified nano-bentonite, 0.15 parts of stannous octoate, 1.2 parts of organic silicon surfactant, 0.5 parts of diethanolamine, and 6 parts of deionized water.
[0088] The preparation method of rare earth modified nano bentonite is:
[0089] (1) First, disperse nano-bentonite in deionized water and disperse it by ultrasonic for 10 minutes to obtain a nano-bentonite dispersion; the mass fraction of nano-bentonite in the nano-bentonite dispersion is 12%.
[0090] (2) adjusting the pH of the nano-bentonite dispersion prepared above, specifically: adjusting the pH of the nano-bentonite dispersion obtained above to 4, then adding rare earth chloride, adjusting the temperature to 70° C., keeping the temperature for 2 hours, and then filtering to obtain pretreated nano-bentonite; adjusting the pH of the nano-bentonite dispersion with a 5% by mass nitric acid solution; the mass ratio of the nano-bentonite dispersion to the rare earth chloride is 1000:1.6.
[0091] The rare earth chloride is lanthanum chloride.
[0092] (3) Add the pretreated nano-bentonite to toluene for ultrasonic dispersion, then add 3-aminopropyltriethoxysilane, adjust the temperature to 106°C, keep stirring for 4 hours, then filter, wash with anhydrous ethanol, and dry to obtain rare earth modified nano-bentonite; the mixing ratio of the pretreated nano-bentonite and toluene is 15g:120mL; the mixing mass ratio of the pretreated nano-bentonite and 3-aminopropyltriethoxysilane is 3:1.
[0093] Comparative Example 1:
[0094] On the basis of Example 1, the raw materials were adjusted, and rare earth modified nano bentonite was not added, and the rest of the technical scheme remained unchanged.
[0095] Comparative Example 2:
[0096] On the basis of Example 1, the raw materials were adjusted, the rare earth modified nano bentonite was replaced with an equal amount of nano bentonite, and the rest of the technical scheme remained unchanged.
[0097] The technical indicators of the nano bentonite used in the present invention are:
[0098] Table 1
[0099] index parameter Appearance off white Montmorillonite content% 97.65 Wafer thickness / nm 12.36 Humidity percentage / % 1.28
[0100] test:
[0101] The thermal conductivity of the insulation layer in the embodiment and the comparative example was tested according to GB / T10294 standard;
[0102] Table 2
[0103] Thermal conductivity W / (m·K) Example 1 0.022 Example 2 0.010 Example 3 0.011 Example 4 0.020 Comparative Example 1 0.043 Comparative Example 2 0.036
[0104] It can be seen from Table 2 that the insulation layer of the anti-corrosion and environmentally friendly foam plastic insulation pipe prepared by the present invention has a lower thermal conductivity coefficient, and thus has better insulation performance.
[0105] The closed porosity of the thermal insulation layer of the embodiment and the comparative sample was tested and compared with that of the thermal insulation layer according to GB / T10799-2008:
[0106] Table 3
[0107] Closed cell rate% Example 1 93.0 Example 2 95.8 Example 3 95.0 Example 4 93.9 Comparative Example 1 85.2 Comparative Example 2 87.3
[0108] It can be seen from Table 3 that the interior of the insulation layer of the anti-corrosion and environmentally friendly foam plastic insulation pipe prepared by the method of the present invention has a closed-cell pore structure with a higher proportion.
[0109] The dimensional stability test of the thermal insulation layer of the embodiment and the comparative example was carried out according to GB / T8811-2008 (at -20°C and relative humidity 100%):
[0110] Table 4
[0111] Dimensional change rate % Example 1 -0.08 Example 2 -0.14 Example 3 -0.16 Example 4 -0.09 Comparative Example 1 -0.24 Comparative Example 2 -0.20
[0112] It can be seen from Table 4 that the insulation layer of the anti-corrosion and environmentally friendly foam plastic insulation pipe prepared by the present invention has excellent dimensional stability.
[0113] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An anti-corrosion and environmentally friendly foam plastic insulation pipe, characterized in that: There is an outer protective layer on the outer jacket of the steel pipe; A thermal insulation layer is provided between the steel pipe and the outer protective layer; The thermal insulation layer is made of rare earth nano-modified polyurethane foam plastic material; The outer protective layer is made of high-density polyethylene material; the rare earth nano-modified polyurethane foam plastic comprises the following components by weight: 80-90 parts of polyol, 30-40 parts of isocyanate, 4-6 parts of rare earth modified nano bentonite, 0.1-0.15 parts of stannous octoate, 0.8-1.2 parts of surfactant, 0.3-0.5 parts of diethanolamine, and 4-6 parts of deionized water; the preparation method of the rare earth modified nano bentonite is: (1) First, disperse nano-bentonite in deionized water and perform ultrasonic dispersion for 10 min to obtain nano-bentonite dispersion; (2) adjusting the pH of the nano-bentonite dispersion prepared above, specifically: adjusting the pH of the nano-bentonite dispersion obtained above to 3-4, then adding rare earth chloride, adjusting the temperature to 70° C., keeping the temperature for 2 hours, and then filtering to obtain pretreated nano-bentonite; (3) The pretreated nano-bentonite was added to toluene for ultrasonic dispersion, and then 3-aminopropyltriethoxysilane was added. The temperature was adjusted to 102-106° C., and the mixture was stirred for 4 hours. The mixture was then filtered, washed with anhydrous ethanol, and dried to obtain rare earth modified nano-bentonite.
2. The anti-corrosion and environmentally friendly foam plastic insulation pipe according to claim 1, characterized in that: The mass fraction of nano-bentonite in the nano-bentonite dispersion in step (1) is 10-12%.
3. The anti-corrosion and environmentally friendly foam plastic insulation pipe according to claim 1, characterized in that: In step (2), the pH of the nano-bentonite dispersion is adjusted using a 5% by mass nitric acid solution; The mixing mass ratio of the nano-bentonite dispersion to the rare earth chloride is 1000:1-1.
6.
4. The anti-corrosion and environmentally friendly foam plastic insulation pipe according to claim 1, characterized in that: The rare earth chloride is cerium chloride or lanthanum chloride.
5. The anti-corrosion and environmentally friendly foam plastic insulation pipe according to claim 1, characterized in that: The mixing ratio of the pretreated nano-bentonite and toluene in step (3) is 10-15 g: 120 mL; The pretreated nano-bentonite and 3-aminopropyltriethoxysilane are mixed in a mass ratio of 3:
1.
6. The anti-corrosion and environmentally friendly foam plastic insulation pipe according to claim 1, characterized in that: The surfactant is an organic silicon surfactant.
7. The anti-corrosion and environmentally friendly foam plastic insulation pipe according to claim 1, characterized in that: The polyol is a polyether polyol.
8. The method for preparing an anti-corrosion and environmentally friendly foam plastic thermal insulation pipe according to claim 1, characterized in that: include: Weigh the following according to weight parts: polyol, rare earth modified nano bentonite, stannous octoate, surfactant, diethanolamine, isocyanate, and deionized water; Adding polyol, rare earth modified nano bentonite, stannous octoate, surfactant, diethanolamine and deionized water into a mixer in sequence, stirring and mixing, to obtain a first mixture; Add isocyanate to the first mixture, stir and mix again, inject between the steel pipe and the outer protective layer, and then foam and shape.