A zirconium-niobium alloy intervertebral disc product with coating and its preparation process

By using zirconium-niobium alloy material in artificial cervical intervertebral discs and forming a zirconia ceramic layer and an oxygen-rich transition layer, the problems of metal ion precipitation and articular surface wear in the prior art are solved, and the service life and durability of the prosthesis are improved.

CN118453952BActive Publication Date: 2024-11-22CHANGZHOU GEASURE MEDICAL DEVICES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410619386.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-19
Publication Date
2024-11-22
Estimated Expiration
2044-05-19

AI Technical Summary

Technical Problem

Existing artificial cervical intervertebral disc materials such as TC4 titanium alloy and cobalt-chromium molybdenum have problems with metal ion precipitation and joint surface wear, which cannot meet the higher patient needs.

Method used

Using zirconium niobium alloy material, zirconia ceramic layer and oxygen-rich transition layer are formed on its surface, and titanium or hydroxyapatite coating is added to the back-to-inner liner to improve biocompatibility and corrosion resistance through oxidation treatment. Reduce metal ion precipitation and joint surface wear.

Benefits of technology

It effectively reduces the wear rate of the joint surface, improves the service life of the prosthesis, and enhances the toughness and corrosion resistance of zirconium niobium alloy, adapts to the complex movement and load requirements of the cervical vertebrae area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004846391350000081
    Figure BDA0004846391350000081
  • Figure FHA0000007572050000011
    Figure FHA0000007572050000011
Patent Text Reader

Abstract

The present invention belongs to the technical field of artificial joints, and specifically relates to a zirconium-niobium alloy intervertebral disc product with a coating and a preparation process thereof. The technical points are as follows: a zirconium-niobium alloy intervertebral disc product with a coating comprises an upper end plate, an inner liner and a lower end plate; the inner liner is located between the upper end plate and the lower end plate, and the surface of the inner liner contacts the surfaces of the upper end plate and the lower end plate respectively; the upper end plate and the lower end plate are zirconium-niobium alloys coated with a zirconium oxide ceramic layer material; an oxygen-rich transition layer is provided between the zirconium oxide ceramic layer and the zirconium-niobium alloy; a coating is provided on the side of the upper end plate and the lower end plate facing away from the inner liner. The zirconium-niobium alloy intervertebral disc product with a coating provided by the present invention and its preparation process have the advantages of reducing metal ion precipitation and reducing joint surface wear, thereby further reducing the wear rate of the joint surface and increasing the service life of the prosthesis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of artificial joints, and in particular relates to a zirconium-niobium alloy intervertebral disc product with a coating and a preparation process thereof. Background Art

[0002] Artificial cervical discs can maintain the mobility of the cervical spine while treating cervical spondylosis. The efficacy is better than traditional ACDF (anterior cervical discectomy, decompression and fusion), avoiding the formation of false joints, reducing the incidence of spondylosis, and significantly reducing the rate of secondary surgery in the lesion gap and adjacent gap. Although it has been more than 50 years since the first artificial cervical disc was implanted, artificial disc technology has developed by leaps and bounds in the past 20 years. More and more implant prostheses have appeared, giving doctors more choices and applications. More high-quality post-clinical studies have proved that the efficacy of CDA (cervical disc replacement) is definitely better than ACDF.

[0003] In the prior art, artificial cervical intervertebral discs are usually made of TC4 titanium alloy or cobalt-chromium-molybdenum materials. These materials have the disadvantages of metal ion precipitation and large wear on the articular surface, and cannot meet the higher needs of patients. Summary of the invention

[0004] The purpose of the present invention is to provide a zirconium-niobium alloy intervertebral disc product with a coating and a preparation process thereof, which has the advantages of reducing metal ion precipitation and reducing joint surface wear, thereby further reducing the wear rate of the joint surface and increasing the service life of the prosthesis.

[0005] The technical objectives of the present invention are achieved by the following technical solutions:

[0006] A zirconium-niobium alloy intervertebral disc product with a coating comprises an upper end plate, an inner liner and a lower end plate; the inner liner is located between the upper end plate and the lower end plate, and the surface of the inner liner contacts the surfaces of the upper end plate and the lower end plate respectively;

[0007] The upper and lower end plates are made of zirconium-niobium alloy coated with zirconium oxide ceramic layer material;

[0008] An oxygen-rich transition layer is provided between the zirconium oxide ceramic layer and the zirconium-niobium alloy;

[0009] The upper end plate and the lower end plate are provided with a coating on the side facing away from the inner lining.

[0010] The intervertebral disc product provided in the present invention has upper and lower end plates made of zirconium-niobium alloy material. The zirconium-niobium alloy end plates have good biocompatibility and can reduce the risk of postoperative rejection and infection. They also have good bone bonding properties and are conducive to the growth and repair of bone tissue. The present invention performs an oxidation treatment on them to form a ceramic-like layer on the surface, so that they have excellent mechanical properties and corrosion resistance, and can provide stable support and a long service life.

[0011] The present invention also provides an oxygen-rich transition layer between the zirconium oxide ceramic layer and the zirconium-niobium alloy to improve the corrosion resistance of the oxide film and prevent the corrosive medium in the external environment from invading the interior of the alloy, thereby protecting the alloy matrix from corrosion and oxidation, and improving the strength and hardness of the alloy while maintaining good toughness.

[0012] Furthermore, the coating includes a titanium coating and / or a hydroxyapatite coating, and has a thickness of 5 to 10 μm.

[0013] Furthermore, in the zirconium-niobium alloy, the zirconium content is 90-99%.

[0014] Furthermore, the ratio of the thickness of the zirconium oxide ceramic layer to the thickness of the oxygen-rich transition layer is (1-2):(2-3).

[0015] Furthermore, the thickness of the zirconium oxide ceramic layer is 8 to 15 μm.

[0016] Since the present invention provides an intervertebral disc product, particularly an intervertebral disc prosthesis for the cervical spine, the intervertebral disc prosthesis for the cervical spine is different from other joint prostheses: the cervical spine region has a larger range of motion and bears greater forces, so the cervical spine prosthesis needs to have better stability and durability to withstand the complex movements and loads in the cervical spine region, and the design of the cervical spine prosthesis needs to take into account the patient's daily activity needs, including head rotation, head tilting, and head lowering, so it is necessary to ensure the adaptability and mobility of the prosthesis to maintain the patient's quality of life. The soft tissue around the cervical spine region is relatively fragile, and when designing the cervical spine prosthesis, it is necessary to minimize damage to the surrounding soft tissue to reduce surgical risks and the occurrence of complications.

[0017] In view of the above differences, the present invention limits the content ratio of zirconium and niobium in the zirconium-niobium alloy. By increasing the niobium content, the toughness and strength of the intervertebral disc prosthesis are enhanced; and according to the requirements of the cervical intervertebral disc for flexibility and durability, the thickness of the oxygen-rich transition layer and the thickness of the zirconium oxide ceramic layer are increased.

[0018] Furthermore, the inner liner is made of ultra-high molecular weight polyethylene material.

[0019] Furthermore, the oxygen content of the oxygen-rich transition layer is 10-40%.

[0020] If the oxygen content is too high, it will lead to excessive generation of oxides in the interface layer, making the interface layer too thick, which may increase the brittleness of the interface layer, causing the interface layer to peel off or crack, and reducing the bonding strength and stability of the interface; if the oxygen content is too low, it will lead to insufficient generation of oxides in the interface layer, and it will be impossible to form a sufficient oxide layer, resulting in insufficient bonding force of the interface layer, reducing the bonding strength and stability between the zirconium-niobium alloy and the zirconium oxide ceramic layer; in the present invention, limiting the oxygen content helps to promote the formation of the interface layer and enhance the bonding strength between the zirconium-niobium alloy and the zirconium oxide ceramic layer.

[0021] The present invention also provides a process for preparing a zirconium-niobium alloy intervertebral disc product with a coating, comprising the following steps:

[0022] S1. Using zirconium-niobium alloy powder as raw material, manufacture upper end plate parts and lower end plate parts according to the product size of intervertebral disc;

[0023] S2, performing oxidation treatment on the upper end plate component and the lower end plate component to form a zirconium oxide ceramic layer and an oxygen-rich transition layer on the surface;

[0024] S3, preparing a coating on the side of the upper end plate component and the lower end plate component facing away from the inner lining to obtain an upper end plate and a lower end plate;

[0025] S4. Combine the upper end plate, the lower end plate and the inner liner to obtain an intervertebral disc product.

[0026] Furthermore, the oxidation treatment is a high-temperature oxidation treatment, and the thickness of the oxygen-rich transition layer and the zirconium oxide ceramic layer is regulated by controlling the temperature and the amount of oxygen introduced.

[0027] Furthermore, in step S3, the coating is prepared by plasma spraying.

[0028] Furthermore, the specific operations of step S2 are as follows:

[0029] S21, placing the upper end plate component and the lower end plate component in a tube furnace, and introducing an inert gas containing 15-20% by mass of oxygen;

[0030] S22, heat to T1°C at t1°C / min, and maintain the temperature for 3 to 5 minutes;

[0031] S23, cool down to T2℃ at t2℃ / min, maintain the temperature for 3-5min;

[0032] S24. Take out after cooling naturally to room temperature.

[0033] Furthermore, the temperature control model in step S2 is as follows:

[0034] Wherein, h1 and h2 are the thickness of the zirconia ceramic layer and the thickness of the oxygen-rich transition layer, respectively, in μm; the temperature range of T1 is 800-900°C, and the temperature range of T2 is 450-550°C.

[0035] The oxygen-rich transition layer provided by the present invention contains not only zirconium oxide but also part of niobium oxide. The combination of zirconium oxide and niobium oxide can greatly improve the toughness and strength of the oxygen-rich transition layer, making the strength and toughness of the upper and lower end plates provided by the present invention more in line with the requirements of cervical intervertebral disc prosthesis.

[0036] The formation of niobium oxide requires a higher temperature. Therefore, in the present invention, the insulation temperature is increased during the heating stage in order to promote the formation of niobium oxide, thereby forming the oxygen-rich transition layer required by the present invention. In the present invention, the formation of niobium oxide can be avoided during the insulation stage after cooling, and only a zirconium oxide ceramic layer is formed at a lower temperature, thereby avoiding the doping of niobium oxide from affecting the compactness of the zirconium oxide ceramic layer, thereby affecting the wear resistance of the upper and lower end plates, and the doping of niobium oxide will also affect the biocompatibility of the zirconium oxide ceramic layer.

[0037] The temperature control model provided in the present invention can accurately control the temperature change process by setting the heating and cooling rates and the temperature holding time, thereby ensuring that the formation of the oxygen-rich transition layer and the zirconia ceramic layer is carried out within a suitable temperature range.

[0038] In summary, the present invention has the following beneficial effects:

[0039] The present invention provides a zirconium-niobium alloy intervertebral disc product with a coating and a preparation process thereof, which has the advantages of reducing metal ion precipitation and reducing joint surface wear, thereby further reducing the joint surface wear rate and increasing the service life of the prosthesis. DETAILED DESCRIPTION

[0040] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, a zirconium-niobium alloy intervertebral disc product with a coating and its preparation process proposed in accordance with the present invention, its specific implementation method, characteristics and effects are described in detail as follows.

[0041] The present embodiment provides a coated zirconium-niobium alloy intervertebral disc product, comprising an upper end plate, an inner liner and a lower end plate; the inner liner is located between the upper end plate and the lower end plate, and the surface of the inner liner contacts the surfaces of the upper end plate and the lower end plate respectively;

[0042] The upper and lower end plates are made of zirconium-niobium alloy coated with zirconium oxide ceramic layer material;

[0043] An oxygen-rich transition layer is provided between the zirconium oxide ceramic layer and the zirconium-niobium alloy;

[0044] The upper end plate and the lower end plate are provided with a coating on the side facing away from the inner lining.

[0045] The intervertebral disc product provided in this specific embodiment has upper and lower end plates manufactured from zirconium-niobium alloy material. The zirconium-niobium alloy end plates have good biocompatibility and can reduce the risk of postoperative rejection and infection. They also have good bone bonding properties and are conducive to the growth and repair of bone tissue. The present invention performs an oxidation treatment on them to form a ceramic-like layer on the surface, so that they have excellent mechanical properties and corrosion resistance, and can provide stable support and a long service life.

[0046] The present invention also provides an oxygen-rich transition layer between the zirconium oxide ceramic layer and the zirconium-niobium alloy to improve the corrosion resistance of the oxide layer and prevent the corrosive medium in the external environment from invading the interior of the alloy, thereby protecting the alloy matrix from corrosion and oxidation, and improving the strength and hardness of the alloy while maintaining good toughness.

[0047] The coating provided in this specific embodiment includes a titanium coating and / or a hydroxyapatite coating, and has a thickness of 5 to 10 μm.

[0048] In the zirconium-niobium alloy provided in this specific embodiment, the zirconium content is 90-99%.

[0049] The ratio of the thickness of the zirconium oxide ceramic layer to the thickness of the oxygen-rich transition layer provided in this specific embodiment is (1-2):(2-3).

[0050] The thickness of the zirconium oxide ceramic layer provided in this specific embodiment is 8 to 15 μm.

[0051] Since the specific implementation method provides an intervertebral disc product, especially an intervertebral disc prosthesis for the cervical spine, the intervertebral disc prosthesis for the cervical spine is different from other joint prostheses: the range of motion in the cervical spine area is larger, and the force it bears is also larger. Therefore, the cervical prosthesis needs to have better stability and durability to withstand the complex movements and loads in the cervical spine area, and the design of the cervical prosthesis needs to take into account the patient's daily activity needs, including head rotation, head tilting, head lowering and other movements. Therefore, it is necessary to ensure the adaptability and mobility of the prosthesis to maintain the patient's quality of life. The soft tissue around the cervical spine area is relatively fragile. When designing a cervical prosthesis, it is necessary to minimize damage to the surrounding soft tissue to reduce surgical risks and complications. Therefore, this specific implementation method limits the content ratio of zirconium and niobium in the zirconium-niobium alloy. By increasing the niobium content, the toughness and strength of the intervertebral disc prosthesis are enhanced; and according to the requirements of the cervical intervertebral disc for flexibility and durability, the thickness of the oxygen-rich transition layer and the thickness of the zirconium oxide ceramic layer are increased.

[0052] In this specific embodiment, the liner is an ultra-high molecular weight polyethylene material.

[0053] In this specific embodiment, if the oxygen content is too high, it will lead to excessive generation of oxides in the interface layer, so that the interface layer becomes too thick, which will increase the brittleness of the interface layer, cause the interface layer to peel off or crack, and reduce the bonding strength and stability of the interface; if the oxygen content is too low, it will lead to insufficient generation of oxides in the interface layer, and it will be impossible to form a sufficient oxide layer, so that the bonding force of the interface layer is insufficient, and the bonding strength and stability between the zirconium-niobium alloy and the zirconium oxide ceramic layer are reduced; in the present invention, the oxygen content is limited to promote the formation of the interface layer and enhance the bonding strength between the zirconium-niobium alloy and the zirconium oxide ceramic layer, therefore, the oxygen content of the oxygen-rich transition layer is preferably 10-40%.

[0054] This specific embodiment also provides a preparation process of a zirconium-niobium alloy intervertebral disc product with a coating, comprising the following steps:

[0055] S1. Using zirconium-niobium alloy powder as raw material, manufacture upper end plate parts and lower end plate parts according to the product size of intervertebral disc;

[0056] S2, performing oxidation treatment on the upper end plate component and the lower end plate component to form a zirconium oxide ceramic layer and an oxygen-rich transition layer on the surface;

[0057] S3, preparing a coating on the side of the upper end plate component and the lower end plate component facing away from the inner lining to obtain an upper end plate and a lower end plate;

[0058] S4. Combine the upper end plate, the lower end plate and the inner liner to obtain an intervertebral disc product.

[0059] Among them, step S1 preferably adopts a 3D printing method, using zirconium-niobium alloy powder as a raw material to produce an upper end plate component and a lower end plate component according to the size of the intervertebral disc product.

[0060] The oxidation treatment in step S2 is preferably a high-temperature oxidation treatment, and the thickness of the oxygen-rich transition layer and the zirconium oxide ceramic layer can be regulated by controlling the temperature and the amount of oxygen introduced.

[0061] Step S3 preferably comprises preparing the coating by plasma spraying.

[0062] In order to provide an oxygen-rich transition layer more suitable for cervical vertebrae prosthesis, the oxygen-rich transition layer contains not only zirconium oxide but also part of niobium oxide; the toughness and strength of the oxygen-rich transition layer are greatly improved by compounding zirconium oxide and niobium oxide. The specific operation of step S2 is as follows:

[0063] S21, placing the upper end plate component and the lower end plate component in a tube furnace, and introducing an inert gas containing 15-20% by mass of oxygen;

[0064] S22, heat to T1°C at t1°C / min, and maintain the temperature for 3 to 5 minutes;

[0065] S23, cool down to T2℃ at t2℃ / min, maintain the temperature for 3-5min;

[0066] S24. Take out after cooling naturally to room temperature.

[0067] More preferably, the temperature control model in step S2 is as follows:

[0068]

[0069] Among them, h1 and h2 are the thickness of the zirconia ceramic layer and the thickness of the oxygen-rich transition layer, respectively, in μm; the temperature range of T1 is 800-900°C, the temperature range of T2 is 450-550°C, and t2 is 0.5-2°C / min.

[0070] Example 1

[0071] This embodiment provides a zirconium-niobium alloy intervertebral disc product with a coating, comprising an upper end plate 1, an inner liner 2 and a lower end plate 3; the inner liner 2 is located between the upper end plate 1 and the lower end plate 3, and the surface of the inner liner 2 is in contact with the surface of the upper end plate 1 and the surface of the lower end plate 3 respectively;

[0072] The upper and lower end plates are made of zirconium-niobium alloy coated with zirconium oxide ceramic layer material;

[0073] An oxygen-rich transition layer is provided between the zirconium oxide ceramic layer and the zirconium-niobium alloy;

[0074] A hydroxyapatite coating with a thickness of 8 μm is provided on the side of the upper end plate and the lower end plate facing away from the inner liner; the zirconium content is 92.5%; the ratio of the thickness of the zirconia ceramic layer to the thickness of the oxygen-rich transition layer is 1:2; the thickness of the zirconia ceramic layer is 10 μm; the inner liner is made of ultra-high molecular weight polyethylene material; the oxygen content of the oxygen-rich transition layer is 30%.

[0075] This embodiment also provides a preparation process of a zirconium-niobium alloy intervertebral disc product with a coating, comprising the following steps:

[0076] S1. Using zirconium-niobium alloy powder as raw material, the upper end plate component and the lower end plate component are manufactured by 3D printing according to the product size of the intervertebral disc;

[0077] S2, performing oxidation treatment on the upper end plate component and the lower end plate component to form a zirconium oxide ceramic layer and an oxygen-rich transition layer on the surface;

[0078] S3, using plasma spraying technology to prepare a hydroxyapatite coating on the side of the upper end plate component and the lower end plate component facing away from the inner lining, to obtain an upper end plate and a lower end plate;

[0079] S4. Combine the upper end plate, the lower end plate and the inner liner to obtain an intervertebral disc product.

[0080] Among them, step S1 preferably adopts 3D printing to use zirconium-niobium alloy powder as raw material to produce upper end plate components and lower end plate components according to the product size of the intervertebral disc.

[0081] The oxidation treatment in step S2 is a high-temperature oxidation treatment, and the thickness of the oxygen-rich transition layer and the zirconium oxide ceramic layer is regulated by controlling the temperature and the amount of oxygen introduced.

[0082] In step S3, the coating is prepared by plasma spraying.

[0083] In order to provide an oxygen-rich transition layer more suitable for cervical vertebrae prosthesis, the oxygen-rich transition layer contains not only zirconium oxide but also part of niobium oxide; the toughness and strength of the oxygen-rich transition layer are greatly improved by compounding zirconium oxide and niobium oxide. The specific operation of step S2 is as follows:

[0084] S21, placing the upper end plate component and the lower end plate component in a tube furnace, and introducing an inert gas containing 20% ​​by mass of oxygen;

[0085] S22, heat to T1°C at t1°C / min, maintain temperature for 5 min;

[0086] S23, cool down to T2℃ at t2℃ / min, maintain the temperature for 5min;

[0087] S24. Take out after cooling naturally to room temperature.

[0088] The temperature control model in step S2 is as follows:

[0089] Wherein, h1 and h2 are the thickness of the zirconia ceramic layer and the thickness of the oxygen-rich transition layer, respectively, in μm; the temperature of T1 is 900°C, the temperature of T2 is 450°C, and t2 = 1°C / min.

[0090] Then through calculation we can know that: t1 / t2=2, t1=2℃ / min.

[0091] Example 2

[0092] This embodiment provides a zirconium-niobium alloy intervertebral disc product with a coating, comprising an upper end plate 1, an inner liner 2 and a lower end plate 3; the inner liner 2 is located between the upper end plate 1 and the lower end plate 3, and the surface of the inner liner 2 is in contact with the surface of the upper end plate 1 and the surface of the lower end plate 3 respectively;

[0093] The upper and lower end plates are made of zirconium-niobium alloy coated with zirconium oxide ceramic layer material;

[0094] An oxygen-rich transition layer is provided between the zirconium oxide ceramic layer and the zirconium-niobium alloy;

[0095] A hydroxyapatite coating with a thickness of 6 μm is provided on the side of the upper end plate and the lower end plate facing away from the inner liner; the zirconium content is 91.3%; the ratio of the thickness of the zirconia ceramic layer to the thickness of the oxygen-rich transition layer is 1:3; the thickness of the zirconia ceramic layer is 8 μm; the inner liner is made of ultra-high molecular weight polyethylene material; the oxygen content of the oxygen-rich transition layer is 30%.

[0096] This embodiment also provides a preparation process of a zirconium-niobium alloy intervertebral disc product with a coating, comprising the following steps:

[0097] S1. Using zirconium-niobium alloy powder as raw material, the upper end plate component and the lower end plate component are manufactured by 3D printing according to the product size of the intervertebral disc;

[0098] S2, performing oxidation treatment on the upper end plate component and the lower end plate component to form a zirconium oxide ceramic layer and an oxygen-rich transition layer on the surface;

[0099] S3, using plasma spraying technology to prepare a hydroxyapatite coating on the side of the upper end plate component and the lower end plate component facing away from the inner lining, to obtain an upper end plate and a lower end plate;

[0100] S4. Combine the upper end plate, the lower end plate and the inner liner to obtain an intervertebral disc product.

[0101] Among them, step S1 preferably adopts 3D printing to use zirconium-niobium alloy powder as raw material to produce upper end plate components and lower end plate components according to the product size of the intervertebral disc.

[0102] The oxidation treatment in step S2 is a high-temperature oxidation treatment, and the thickness of the oxygen-rich transition layer and the zirconium oxide ceramic layer is regulated by controlling the temperature and the amount of oxygen introduced.

[0103] In step S3, the coating is prepared by plasma spraying.

[0104] In order to provide an oxygen-rich transition layer more suitable for cervical vertebrae prosthesis, the oxygen-rich transition layer contains not only zirconium oxide but also part of niobium oxide; the toughness and strength of the oxygen-rich transition layer are greatly improved by compounding zirconium oxide and niobium oxide. The specific operation of step S2 is as follows:

[0105] S21, placing the upper end plate component and the lower end plate component in a tube furnace, and introducing an inert gas containing 18% by mass of oxygen;

[0106] S22, heat to T1°C at t1°C / min, maintain temperature for 5 min;

[0107] S23, cool down to T2℃ at t2℃ / min, maintain the temperature for 5min;

[0108] S24. Take out after cooling naturally to room temperature.

[0109] The temperature control model in step S2 is as follows:

[0110] Wherein, h1 and h2 are the thickness of the zirconia ceramic layer and the thickness of the oxygen-rich transition layer, respectively, in μm; the temperature of T1 is 800°C, the temperature of T2 is 450°C, and t2 = 1°C / min.

[0111] Then through calculation we can know that: t1 / t2=2.3, t1=2.3℃ / min.

[0112] Example 3

[0113] This embodiment provides a zirconium-niobium alloy intervertebral disc product with a coating, comprising an upper end plate 1, an inner liner 2 and a lower end plate 3; the inner liner 2 is located between the upper end plate 1 and the lower end plate 3, and the surface of the inner liner 2 is in contact with the surface of the upper end plate 1 and the surface of the lower end plate 3 respectively;

[0114] The upper and lower end plates are made of zirconium-niobium alloy coated with zirconium oxide ceramic layer material;

[0115] An oxygen-rich transition layer is provided between the zirconium oxide ceramic layer and the zirconium-niobium alloy;

[0116] A hydroxyapatite coating with a thickness of 8 μm is provided on the side of the upper end plate and the lower end plate facing away from the inner liner; the zirconium content is 90.8%; the ratio of the thickness of the zirconia ceramic layer to the thickness of the oxygen-rich transition layer is 1:2; the thickness of the zirconia ceramic layer is 8 μm; the inner liner is made of ultra-high molecular weight polyethylene material; the oxygen content of the oxygen-rich transition layer is 30%.

[0117] This embodiment also provides a preparation process of a zirconium-niobium alloy intervertebral disc product with a coating, comprising the following steps:

[0118] S1. Using zirconium-niobium alloy powder as raw material, the upper end plate component and the lower end plate component are manufactured by 3D printing according to the product size of the intervertebral disc;

[0119] S2, performing oxidation treatment on the upper end plate component and the lower end plate component to form a zirconium oxide ceramic layer and an oxygen-rich transition layer on the surface;

[0120] S3, using plasma spraying technology to prepare a hydroxyapatite coating on the side of the upper end plate component and the lower end plate component facing away from the inner lining, to obtain an upper end plate and a lower end plate;

[0121] S4. Combine the upper end plate, the lower end plate and the inner liner to obtain an intervertebral disc product.

[0122] Among them, step S1 preferably adopts 3D printing to use zirconium-niobium alloy powder as raw material to produce upper end plate components and lower end plate components according to the product size of the intervertebral disc.

[0123] The oxidation treatment in step S2 is a high-temperature oxidation treatment, and the thickness of the oxygen-rich transition layer and the zirconium oxide ceramic layer is regulated by controlling the temperature and the amount of oxygen introduced.

[0124] In step S3, the coating is prepared by plasma spraying.

[0125] In order to provide an oxygen-rich transition layer more suitable for cervical vertebrae prosthesis, the oxygen-rich transition layer contains not only zirconium oxide but also part of niobium oxide; the toughness and strength of the oxygen-rich transition layer are greatly improved by compounding zirconium oxide and niobium oxide. The specific operation of step S2 is as follows:

[0126] S21, placing the upper end plate component and the lower end plate component in a tube furnace, and introducing an inert gas containing 20% ​​by mass of oxygen;

[0127] S22, heat to T1°C at t1°C / min, maintain temperature for 5 min;

[0128] S23, cool down to T2℃ at t2℃ / min, maintain the temperature for 5min;

[0129] S24. Take out after cooling naturally to room temperature.

[0130] The temperature control model in step S2 is as follows:

[0131] Wherein, h1 and h2 are the thickness of the zirconia ceramic layer and the thickness of the oxygen-rich transition layer, respectively, in μm; the temperature of T1 is 850°C, the temperature of T2 is 450°C, and t2=2°C / min.

[0132] Then through calculation we can know that: t1 / t2=1.8, t1=3.6℃ / min.

[0133] Comparative Example 1

[0134] This embodiment provides a zirconium-niobium alloy intervertebral disc product with a coating, comprising an upper end plate 1, an inner liner 2 and a lower end plate 3; the inner liner 2 is located between the upper end plate 1 and the lower end plate 3, and the surface of the inner liner 2 is in contact with the surface of the upper end plate 1 and the surface of the lower end plate 3 respectively;

[0135] The upper and lower end plates are made of zirconium-niobium alloy coated with zirconium oxide ceramic layer material;

[0136] A hydroxyapatite coating with a thickness of 8 μm is provided on the side of the upper end plate and the lower end plate facing away from the inner lining; the zirconium content is 92.5%; the thickness of the zirconium oxide ceramic layer is 10 μm; and the inner lining is made of ultra-high molecular weight polyethylene material.

[0137] This embodiment also provides a preparation process of a zirconium-niobium alloy intervertebral disc product with a coating, comprising the following steps:

[0138] S1. Using zirconium-niobium alloy powder as raw material, the upper end plate component and the lower end plate component are manufactured by 3D printing according to the product size of the intervertebral disc;

[0139] S2, performing oxidation treatment on the upper end plate component and the lower end plate component to form a zirconium oxide ceramic layer on the surface;

[0140] S3, using plasma spraying technology to prepare a hydroxyapatite coating on the side of the upper end plate component and the lower end plate component facing away from the inner lining, to obtain an upper end plate and a lower end plate;

[0141] S4. Combine the upper end plate, the lower end plate and the inner liner to obtain an intervertebral disc product.

[0142] Among them, step S1 preferably adopts 3D printing to use zirconium-niobium alloy powder as raw material to produce upper end plate components and lower end plate components according to the product size of the intervertebral disc.

[0143] The oxidation treatment in step S2 is a high-temperature oxidation treatment, and the thickness of the oxygen-rich transition layer and the zirconium oxide ceramic layer is regulated by controlling the temperature and the amount of oxygen introduced.

[0144] In step S3, the coating is prepared by plasma spraying.

[0145] The specific operations of step S2 are as follows:

[0146] S21, placing the upper end plate component and the lower end plate component in a tube furnace, and introducing an inert gas containing 20% ​​by mass of oxygen;

[0147] S22, heat to T2°C at t1°C / min, maintain temperature for 5 min;

[0148] S24. Take out after cooling naturally to room temperature.

[0149] The temperature control model in step S2 is as follows:

[0150] The temperature of T2 is 450°C, and t1 = 2°C / min.

[0151] Performance Testing

[0152] The intervertebral disc products prepared in Examples 1 to 3 were tested for wear resistance and cytological bioactivity. The results are shown in Table 1.

[0153] The wear resistance test method is as follows: the friction and wear test of the film layer is carried out on a ball-disc friction tester, the friction material is a silicon nitride ball with a diameter of 5mm, the load is 1N, the relative sliding speed is 0.2m / s, and the wear resistance is determined by the wear amount; the contact angle test is carried out using a contact angle tester produced by Dataphysics in Germany. The test instrument has its own droplet system and sample stage for loading objects. The test is carried out at room temperature and is measured by dropping a droplet with a volume of 4 microliters on the sample. Three points are taken on each sample surface for measurement, and the average value is taken as the contact angle size of the sample surface.

[0154] The cytological bioactivity test method is as follows: a human osteoblast-like cell line MG-63 osteoblast model is used to conduct a cytological bioactivity experiment on the intervertebral disc product. The MG-63 osteoblasts are revived with a high-glucose cell culture medium containing 10% fetal bovine serum, and cultured in a cell culture incubator at 37°C, 95% humidity, and 5% CO2 concentration. The medium is changed every other day, and the cell morphology is observed under an optical microscope. The MG-63 osteoblasts in the logarithmic growth phase are prepared into a cell suspension.

[0155] The standard samples of the experimental group and the control group were sterilized by γ-ray irradiation for 2 hours and placed in a 24-well plate. The prepared MG-63 cell suspension was inoculated on the surface of each group of samples, and the cell culture was terminated after 24 hours. The number of cell adhesion and proliferation was detected by acridine orange fluorescence staining. Rinse with PBS (phosphate buffer, 1L PBS formula: 8g sodium chloride, 0.2g potassium chloride, 1.44g disodium hydrogen phosphate, 0.24g potassium dihydrogen phosphate) for 3 times, fix with 95% ethanol for 5 minutes, stain with 0.05% acridine orange for 5 minutes, and rinse with PBS for 3 times; observe and count the number of cells adhering to and proliferating on the surface of the material under a fluorescence microscope.

[0156] Table 1. Test results

[0157] <![CDATA[Wear resistance (m 3 / Nm)]]> Water contact angle (degrees) 24h cell count Example 1 4.66 48 <![CDATA[6.8×10 7 ]]> Example 2 4.73 46 <![CDATA[7.2×10 7 ]]> Example 3 4.58 49 <![CDATA[6.5×10 7 ]]> Comparative Example 1 4.46 50 <![CDATA[4.3×10 7 ]]>

[0158] From the above data, it can be seen that the above embodiments of the present invention achieve the following technical effects: the intervertebral disc prosthesis provided by the present invention has excellent wear resistance and biocompatibility.

[0159] From the comparison of the data of Comparative Example 1 and Example 1, it can be seen that in the absence of an oxygen-rich transition layer, the wear resistance and biological properties of the product are both reduced.

[0160] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been presented as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A zirconium-niobium alloy intervertebral disc product with a coating, characterized in that: The intervertebral disc product comprises an upper end plate, an inner liner and a lower end plate; the inner liner is located between the upper end plate and the lower end plate, and the surface of the inner liner contacts the surfaces of the upper end plate and the lower end plate respectively; The upper end plate and the lower end plate are made of zirconium-niobium alloy coated with zirconium oxide ceramic layer material; An oxygen-rich transition layer is provided between the zirconium oxide ceramic layer and the zirconium-niobium alloy; The upper end plate and the lower end plate are provided with a coating on one side facing away from the inner lining; The preparation process of the zirconium-niobium alloy intervertebral disc product with coating comprises the following steps: S1. Using zirconium-niobium alloy powder as raw material, manufacture upper end plate parts and lower end plate parts according to the product size of intervertebral disc; S2, performing oxidation treatment on the upper end plate component and the lower end plate component to form a zirconium oxide ceramic layer and an oxygen-rich transition layer on the surface; S3, preparing a coating on the side of the upper end plate component and the lower end plate component facing away from the inner lining to obtain an upper end plate and a lower end plate; S4, combining the upper end plate, the lower end plate and the liner to obtain an intervertebral disc product; The specific operations of step S2 are as follows: S21, placing the upper end plate component and the lower end plate component in a tube furnace, and introducing an inert gas containing 15-20% by mass of oxygen; S22, heat to T1°C at t1°C / min, and maintain the temperature for 3 to 5 minutes; S23, cool down to T2℃ at t2℃ / min, maintain the temperature for 3-5min; S24, take out after cooling naturally to room temperature; The temperature control model in step S2 is as follows: Wherein, h1 and h2 are the thickness of the zirconia ceramic layer and the thickness of the oxygen-rich transition layer, respectively, in μm; the temperature range of T1 is 800-900°C, and the temperature range of T2 is 450-550°C; The oxygen content of the oxygen-rich transition layer is 10-40%; The coating comprises a titanium coating and / or a hydroxyapatite coating, and has a thickness of 5 to 10 μm; The zirconium content in the zirconium-niobium alloy is 90-99%.

2. The zirconium-niobium alloy intervertebral disc product with coating according to claim 1, characterized in that: The thickness ratio of the zirconium oxide ceramic layer to the oxygen-rich transition layer is (1-2):(2-3).

3. The zirconium-niobium alloy intervertebral disc product with coating according to claim 1, characterized in that: The thickness of the zirconium oxide ceramic layer is 8-15 μm.

4. The zirconium-niobium alloy intervertebral disc product with coating according to claim 1, characterized in that: The liner is made of ultra high molecular weight polyethylene material.

5. The zirconium-niobium alloy intervertebral disc product with coating according to claim 1, characterized in that: The oxidation treatment is a high-temperature oxidation treatment, and the thickness of the oxygen-rich transition layer and the zirconium oxide ceramic layer are regulated by controlling the temperature and the amount of oxygen introduced.

6. The zirconium-niobium alloy intervertebral disc product with coating according to claim 5, characterized in that: In step S3, the coating is prepared by plasma spraying.