A method for recovering spent catalyst cesium fluoride produced in the synthesis process of perfluorohexanone

Through high-temperature calcination and multiple water dissolution filtration, the failed cesium fluoride during perfluorohexanone synthesis is recycled, solving the problems of high production costs and environmental pollution, and achieving the recovery of catalytic activity and efficient recovery.

CN118454704BActive Publication Date: 2024-11-08GANSU RUISIKE NEW MATERIAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410795916.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-11-08
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

The failed catalyst cesium fluoride produced during perfluorohexanone synthesis cannot be recycled, resulting in high production costs and environmental pollution.

Method used

Using high-temperature calcination and multiple water dissolution filtration, the failed cesium fluoride is converted into a reusable catalyst, and the oily substance on the surface is removed by high-temperature thermal decomposition, and pulverized in a confined space to prepare into powder to improve recovery efficiency.

Benefits of technology

The failed cesium fluoride has a catalytic activity again, the number of recycled uses reaches the standard of 99.5% for purchase purity, and the impurity ion content only increased by 2,000ppm, which improved the catalytic effect and recycling efficiency, reduced production costs, and avoided environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The present invention discloses a method for recovering the spent catalyst cesium fluoride produced in the synthesis process of perfluorohexanone, which ingeniously utilizes high temperature to thermally decompose the oily substance wrapped on the surface of cesium fluoride into black slag, and then utilizes the characteristics that the black slag is insoluble in water while cesium fluoride is soluble in water to remove the oily substance that affects the catalytic effect. The method can make the cesium fluoride that no longer has catalytic activity in the production process of perfluorohexanone have a catalytic effect again, and the number of times the cesium fluoride is recycled as a catalyst is the same as that of a standard cesium fluoride sample with a purity of 99.5% purchased from outside, and the number of catalytic recycling can reach 3 times. The spent cesium fluoride treated by the method of the present invention is subjected to full element analysis, and the results show that the content of impurity ions (mainly sodium ions and potassium ions) therein is only increased by about 2000ppm compared with the standard cesium fluoride sample with a purity of 99.5% purchased from outside, and the catalytic effect is almost the same as that of the standard sample.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cesium fluoride recovery, and in particular relates to a method for recovering spent catalyst cesium fluoride generated in the synthesis process of perfluorohexanone. Background Art

[0002] Perfluorohexanone (FK-5-1-12), chemically known as perfluoro-2-methyl-3-pentanone, is a fire extinguishing agent launched by 3M Company in the United States to replace halons and freons. Perfluorohexanone has a boiling point of 49°C, is very easy to vaporize, leaves no residue after release, has a short atmospheric residence time (5 days), does not damage the atmospheric ozone layer (ODP=0), has a low global warming potential (GWP=1), and has close to zero harm to the environment and humans. It is a new type of clean, green and environmentally friendly fire extinguishing agent with comprehensive advantages such as high fire extinguishing efficiency, environmental protection, high safety margin, good insulation performance, and no damage to electronic precision equipment. It has been recognized by the international fire protection community and widely used in important places such as aerospace, data centers, libraries, military equipment, subways, etc. It is currently recognized as a substance that can replace hydrofluorocarbon fire extinguishing agents such as heptafluoropropane. The market demand is huge and has broad market prospects.

[0003] There are many methods for synthesizing perfluorohexanone, and most of them use hexafluoropropylene as raw material. In the early days, hexafluoropropylene and hexafluoropropylene oxide were mainly used for reaction under the action of catalyst; later, a method for synthesizing perfluorohexanone using hexafluoropropylene and acyl halide as raw materials appeared. In addition, there are several other synthetic methods, including: preparing perfluorohexanone from potassium perfluorocarboxylate and perfluoropropionyl fluoride at room temperature, and preparing perfluorohexanone from perfluorocarboxylate and perfluoroanhydride. Later, with the in-depth research on perfluorohexanone in China, a series of safer and more efficient synthesis routes were explored. These synthesis routes all use perfluoro-2-methyl-2-pentene (D2) as the reaction raw material, which will inevitably introduce D2 into perfluorohexanone. D2 has certain biological toxicity and pungent odor, which will not only reduce the purity of the perfluorohexanone product, but also have a great impact on its odor and safety. Therefore, D2 should be removed as much as possible to improve the purity of perfluorohexanone. However, D2 and perfluorohexanone have similar polarity, are miscible and have very close boiling points, so it is difficult to separate and remove them by conventional methods such as distillation or extraction.

[0004] Chinese patent CN102992986A discloses a method for preparing perfluorohexanone, that is, using per-4-methyl-2-pentene (D1) or perfluoro-2-methyl-2-pentene (D2) as raw materials, preparing perfluorohexanone through olefin isomerization, olefin epoxidation, and epoxide structure rearrangement. This method has abundant raw material sources, mild reaction conditions, simple process, and high selectivity and conversion rate of each step, which can reach more than 90%. In order to reduce the content of D2 in perfluorohexanone, a separation and purification step is added during the reaction process, and the intermediate product perfluoro-2,3-epoxy-2-methylpentane is washed with fluorine phase water, dried with anhydrous MgSO4, and then bromination addition and distillation purification are used to remove D2. However, this method introduces bromine element as impurities during the bromination addition process, and the intermediate product perfluoro-2,3-epoxy-2-methylpentane needs to be purified, which not only destroys the continuity of the reaction but also involves multiple purification and separation steps. The product has a low boiling point and is volatile, thus resulting in a decrease in the overall yield of perfluorohexanone.

[0005] Chinese patent CN107879912A uses a microchannel reactor to carry out continuous olefin epoxidation reaction. The continuous reaction product is quickly removed from the reactor, shortening the reaction time. However, there is also a problem of reduced conversion rate due to the short residence time of the raw material D2. In addition, the unreacted D2 in the reaction process is removed by distillation of the intermediate product perfluoro-2-methyl-2,3-epoxypentane, which will destroy the continuity of the entire reaction. The multi-step separation and purification operation also leads to a reduced yield of perfluorohexanone.

[0006] In order to solve the above problems, US Pat. No. 6,478,979B1 proposes an improved method, i.e., using KMnO4 as an oxidant to remove dimers under the condition of solvent acetic acid, which can effectively remove dimers in perfluorohexanone. However, potassium permanganate is a strong oxidant, the reaction process is risky, and potassium permanganate needs to be in acidic conditions to exert its oxidizing properties. Therefore, a perfluorohexanone purification method disclosed in CN116969825B will introduce acid value into perfluorohexanone, resulting in excessive acid value and increased acid removal operation. In addition, the solid waste manganese dioxide generated after the potassium permanganate oxidation reaction is also difficult to handle.

[0007] As can be seen from the above-mentioned prior art, in the current mainstream method of synthesizing perfluorohexanone, a fluorine-containing inorganic catalyst is used in almost every step. After multiple experiments, the applicant found that the catalytic effect of cesium fluoride is more excellent than that of other fluorine-containing catalysts. However, when using cesium fluoride as a catalyst, there will be a situation where the catalyst is deactivated and has no catalytic effect after cesium fluoride is used continuously for 3 times, and the deactivated cesium fluoride can no longer be used. However, due to the expensive price of cesium fluoride, about 1.2 million per ton, if perfluorohexanone with an annual output of 1,000 tons is required, the usage of cesium fluoride is about 3 tons, requiring 3.6 million. Therefore, if the deactivated catalyst cesium fluoride is not recycled, the production cost of perfluorohexanone will be greatly increased, and the untreated deactivated cesium fluoride is also a solid waste, which will have an impact on the environment. Therefore, the recovery of the failed catalyst cesium fluoride produced in the process of producing perfluorohexanone has significant economic and social benefits. Summary of the invention

[0008] The invention provides a method for recovering spent catalyst cesium fluoride produced in the synthesis process of perfluorohexanone, the purpose of which is to solve the problem that the cost of cesium fluoride is high and failure to recycle it will result in high production cost of perfluorohexanone and cause solid waste storage that affects the environment.

[0009] To achieve its purpose, the present invention adopts the following technical solutions:

[0010] A method for recovering spent catalyst cesium fluoride produced in the synthesis process of perfluorohexanone comprises the following steps:

[0011] (1) placing the spent catalyst cesium fluoride in a platinum crucible and calcining it under air flow at 400-450° C. to obtain calcined cesium fluoride;

[0012] (2) adding water to dissolve the calcined cesium fluoride obtained in step (1) to obtain a cesium fluoride mixed solution containing black slag;

[0013] (3) The mixed solution obtained in step (2) is first coarsely filtered using filter paper, and then finely filtered using a filter membrane to obtain a light yellow cesium fluoride aqueous solution;

[0014] (4) The cesium fluoride aqueous solution obtained in step (3) is transferred into a platinum crucible, and then calcined for 3-4 hours under air flow conditions of 200-250°C, and then calcined for 3-4 hours under air flow conditions of 400-450°C. After the calcination, the temperature is cooled to room temperature to obtain a cesium fluoride solid;

[0015] (5) further adding water to dissolve the cesium fluoride solid obtained in step (4) to obtain a secondary aqueous solution of cesium fluoride, and the secondary aqueous solution of cesium fluoride is first coarsely filtered using filter paper and then finely filtered using a filter membrane to obtain a clear and transparent aqueous solution of cesium fluoride;

[0016] (6) placing the clear and transparent cesium fluoride aqueous solution obtained in step (5) in a platinum crucible and calcining it under air flow at 200-250° C. for 3-4 hours, then raising the temperature to 400-450° C. and continuing calcining under nitrogen flow until blocky white cesium fluoride crystals are obtained;

[0017] (7) The blocky cesium fluoride crystals obtained in step (6) are crushed in a closed space to obtain white powdery cesium fluoride crystals that can be used as a catalyst.

[0018] As a further preferred embodiment of the technical solution of the present invention, in step (1), the calcination time is 3-4 hours.

[0019] Furthermore, in step (2), the solid-liquid mass ratio of cesium fluoride to water after calcination is 1:3-5.

[0020] Furthermore, in step (3) and step (5), the pore size of the filter paper for coarse filtration is 1 μm, and the pore size of the filter membrane for fine filtration is 0.2 μm.

[0021] Furthermore, in step (5), the solid-liquid mass ratio of cesium fluoride solid to water is 1:3-5.

[0022] Furthermore, in step (6), the calcination time under nitrogen flow conditions is 3-4 hours.

[0023] The beneficial effects of the present invention are:

[0024] 1. The outer surface of the failed cesium fluoride catalyst is covered with a large amount of yellow oily substance ( Figure 1 ), firstly, the reaction substrate cannot contact with the active site of the catalyst, so that the reaction cannot proceed, and secondly, the catalyst will be poisoned and lose its catalytic effect, and cannot react with the reaction substrate. The present invention cleverly utilizes high temperature to thermally decompose the oily substance coated on the surface of cesium fluoride into black residue, and then utilizes the characteristics that the black residue is insoluble in water while cesium fluoride is soluble in water to remove the oily substance that affects the catalytic effect. Furthermore, the present invention adopts secondary high-temperature thermal decomposition to eliminate the problem that a single thermal decomposition will have incomplete decomposition, resulting in the doping of some oily inclusions in the recovered cesium fluoride catalyst, thereby affecting the whiteness and purity of the recovered cesium fluoride, and further affecting the subsequent catalytic effect.

[0025] 2. The method of the present invention can make cesium fluoride that no longer has catalytic activity in the production process of perfluorohexanone have catalytic effect again, and the number of times cesium fluoride is recycled as a catalyst is the same as that of the purchased standard cesium fluoride sample with a purity of 99.5%, and the number of catalytic cycles can also reach 3 times.

[0026] 3. The spent cesium fluoride treated by the method of the present invention was subjected to full element analysis. The results showed that the content of impurity ions (mainly sodium ions and potassium ions) therein was only increased by about 2000ppm compared with the standard cesium fluoride sample with a purity of 99.5% purchased from outside, and the catalytic effect was almost the same as that of the standard sample.

[0027] 4. The block cesium fluoride obtained by the secondary high-temperature thermal decomposition method of the present invention cannot be used as a catalyst, and further processing is required to prepare it into powdered cesium fluoride. There are two problems when preparing powdered cesium fluoride: first, the block cesium fluoride obtained by pyrolysis of the solvent is very easy to adhere to the bottom of the platinum crucible, which is difficult to take out. It is necessary to use strong mechanical force to peel it off from the wall of the platinum crucible. This process will cause the loss of cesium fluoride, resulting in a decrease in yield. In addition, since cesium fluoride is highly toxic, this process is also very easy to cause harm to people, leading to the occurrence of safety accidents; second, the part of the cesium fluoride peeled off from the crucible using strong mechanical force is exposed to the air for a long time and is very easy to become small droplets due to deliquescence, which will also cause a decrease in the yield of cesium fluoride. Therefore, the present invention adopts a method of crushing in a confined space to peel off the block cesium fluoride from the wall of the platinum crucible to prepare powdered cesium fluoride, ensuring a high yield of cesium fluoride.

[0028] 5. The present invention is simple to operate, low in cost, does not require the addition of other agents, and the process flow is easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a photo of the failed cesium fluoride;

[0030] Figure 2 This is a photograph of the cesium fluoride aqueous solution after calcination under air flow at 200°C in Example 1;

[0031] Figure 3 This is a photograph of the cesium fluoride aqueous solution after calcination at 400° C. under air flow in Example 1;

[0032] Figure 4 This is a photo of the clear and transparent cesium fluoride aqueous solution obtained after filtering the secondary cesium fluoride aqueous solution in Example 1;

[0033] Figure 5 This is a photograph of the clear and transparent cesium fluoride aqueous solution in Example 1 when it is calcined under air flow at 200°C;

[0034] Figure 6 This is a photograph of the clear and transparent cesium fluoride aqueous solution in Example 1 after being calcined under air flow at 200° C. and cooled to room temperature;

[0035] Figure 7This is a photo of white bulk cesium fluoride crystals obtained by calcining the clear and transparent cesium fluoride aqueous solution in Example 1 at 400° C. in a nitrogen flow;

[0036] Figure 8 This is a photo of white powdery cesium fluoride crystals obtained by crushing the blocky cesium fluoride crystals in Example 1;

[0037] Fig. 9 This is a gas chromatogram of the synthetic phase after the cesium fluoride obtained by the method of Example 1 of the present invention participates in the catalytic reaction;

[0038] Fig.10 This is the gas chromatogram of the synthetic phase after the catalytic reaction of the standard sample cesium fluoride is completed. DETAILED DESCRIPTION

[0039] The recycling method of the present invention is described in detail below through specific embodiments in conjunction with the accompanying drawings.

[0040] Example 1

[0041] The present embodiment provides a method for recovering spent catalyst cesium fluoride produced in the synthesis process of perfluorohexanone, comprising the following steps:

[0042] (1) Take 50g of spent cesium fluoride ( Figure 1 ) was placed in a platinum crucible and calcined at 400°C for 3 h under air flow to obtain calcined cesium fluoride;

[0043] (2) adding ultrapure water to dissolve the calcined cesium fluoride obtained in step (1) at a solid-liquid mass ratio of 1:3 to obtain a cesium fluoride mixed solution containing a large amount of black slag;

[0044] (3) The mixed solution obtained in step (2) is first coarsely filtered using filter paper with a pore size of 1 μm, and then finely filtered using a filter membrane with a pore size of 0.2 μm to obtain a light yellow cesium fluoride aqueous solution;

[0045] (4) The cesium fluoride aqueous solution obtained in step (3) was transferred into a platinum crucible and then calcined for 3 h under air flow at 200 °C (see the photo after calcination). Figure 2 ), and then calcined in air flow at 400 ° C for 4 h (see the photo after calcination Figure 3 ), after the calcination is completed, the temperature is cooled to room temperature to obtain a light yellow cesium fluoride solid;

[0046] (5) The cesium fluoride solid obtained in step (4) is further dissolved in ultrapure water at a solid-liquid mass ratio of 1:3 to obtain a secondary aqueous solution of cesium fluoride mixed with small black residues. The secondary aqueous solution of cesium fluoride is first coarsely filtered using a filter paper with a pore size of 1 μm, and then finely filtered using a filter membrane with a pore size of 0.2 μm to obtain a clear and transparent aqueous solution of cesium fluoride ( Figure 4 );

[0047] (6) The clear and transparent cesium fluoride aqueous solution obtained in step (5) is placed in a platinum crucible and calcined for 3 h under air flow at 200°C (see the photo of the aqueous solution during calcination). Figure 5 , the aqueous solution cooled to room temperature after calcination is shown in Figure 6 ), then the temperature was raised to 400 °C and calcined for 4 h under nitrogen flow until white cesium fluoride crystals ( Figure 7 );

[0048] (7) The blocky cesium fluoride crystals obtained in step (6) are crushed in a closed space to obtain white powdery cesium fluoride crystals that can be used as a catalyst ( Figure 8 The full element analysis results are shown in Table 1.

[0049]

[0050] The powdered cesium fluoride obtained by the method of this embodiment is used as a catalyst to participate in the catalytic reaction (refer to the invention patent CN112830863A). The gas chromatogram of the synthetic phase after completion is as follows: Fig. 9 shown.

[0051] Fig. 9 It was shown that the chromatographic peak of hexafluoropropylene dimer (D1) appeared in the gas chromatogram, accounting for 91.122%, indicating that the cesium fluoride obtained after treatment by the method of this embodiment has catalytic activity.

[0052] The standard sample cesium fluoride is used as a catalyst to participate in the catalytic reaction (refer to the invention patent CN112830863A). After the completion of the synthesis phase, the gas chromatogram is as follows: Fig.10 As shown, Fig.10 The chromatographic peak of hexafluoropropylene dimer (D1) appeared in the sample, accounting for 92.665%.

[0053] Comparing the gas chromatograms of the products of the catalytic reaction of cesium fluoride obtained by the method of this embodiment and the standard cesium fluoride, the proportions of hexafluoropropylene dimer in the synthetic product are 91.112% and 92.665%, respectively, indicating that the catalytic effects of the two are basically the same, except that the purity of hexafluoropropylene dimer is reduced by 1.553%.

[0054] Example 2

[0055] The present embodiment provides a method for recovering spent catalyst cesium fluoride produced in the synthesis process of perfluorohexanone, comprising the following steps:

[0056] (1) Take 100g of spent cesium fluoride ( Figure 1 ) was placed in a platinum crucible and calcined at 400°C for 3 h under air flow to obtain calcined cesium fluoride;

[0057] (2) adding ultrapure water to dissolve the calcined cesium fluoride obtained in step (1) at a solid-liquid mass ratio of 1:4 to obtain a cesium fluoride mixed solution containing a large amount of black slag;

[0058] (3) The mixed solution obtained in step (2) is first coarsely filtered using filter paper with a pore size of 1 μm, and then finely filtered using a filter membrane with a pore size of 0.2 μm to obtain a light yellow cesium fluoride aqueous solution;

[0059] (4) The cesium fluoride aqueous solution obtained in step (3) is transferred into a platinum crucible, and then calcined under air flow at 200° C. for 3 h, and then calcined under air flow at 400° C. for 4 h. After the calcination, the temperature is cooled to room temperature to obtain a light yellow cesium fluoride solid;

[0060] (5) the cesium fluoride solid obtained in step (4) is further dissolved in ultrapure water at a solid-liquid mass ratio of 1:3 to obtain a secondary aqueous solution of cesium fluoride mixed with small black residues, the secondary aqueous solution of cesium fluoride is first coarsely filtered using a filter paper with a pore size of 1 μm, and then finely filtered using a filter membrane with a pore size of 0.2 μm to obtain a clear and transparent aqueous solution of cesium fluoride;

[0061] (6) placing the clear and transparent cesium fluoride aqueous solution obtained in step (5) in a platinum crucible, calcining it at 200° C. for 3 h under air flow, then raising the temperature to 400° C. and calcining it for 4 h under nitrogen flow until white cesium fluoride crystals are obtained;

[0062] (7) The blocky cesium fluoride crystals obtained in step (6) are crushed in a closed space to obtain white powdery cesium fluoride crystals that can be used as a catalyst. The full element analysis results are shown in Table 2.

[0063]

[0064] The complete analysis results of the 99.5% cesium fluoride standard sample are shown in Table 3.

[0065]

[0066] It can be seen from the data in Tables 1 to 3 that the spent cesium fluoride treated by the method of the present invention was subjected to full element analysis. The results showed that the content of impurity ions (mainly sodium ions and potassium ions) therein was only increased by about 2000ppm compared with the purchased standard cesium fluoride sample with a purity of 99.5%, and the catalytic effect was almost the same as that of the standard sample.

[0067] Example 3

[0068] The other steps of Example 3 are the same as those of Example 1, except that the calcination temperature in step (1) is changed from 400°C to 450°C. After calcination at 450°C, a pale yellow solution is still obtained, and the color is similar to that after calcination at 400°C. Considering the problem of calcination energy consumption, the calcination temperature is preferably selected as 400°C.

[0069] Example 4

[0070] The other steps of Example 4 are the same as those of Example 1, except that the calcination time in step (1) is changed from 3 h to 4 h. After calcination for 4 h, a pale yellow solution is still obtained, and the color is similar to that of calcination for 3 h. Considering the problem of calcination energy consumption, the calcination time is preferably selected as 3 h.

[0071] Example 5

[0072] The other steps of Example 5 are the same as those of Example 1, except that the solid-liquid mass ratio of the dissolution in step (2) is changed from 1:3 to 1:5. Both the solid-liquid mass ratio of 1:3 and 1:5 can dissolve the deactivated cesium fluoride after high temperature treatment. Considering the problem of liquid volume, the dissolution solid-liquid mass ratio of 1:3 is preferably selected.

[0073] Example 6

[0074] Example 6 is the same as Example 1 in other steps, except that the first calcination temperature in step (4) is changed from 200°C to 250°C. After calcination at 200°C and 250°C for 3h, the water can be completely evaporated to obtain a light yellow amorphous state. Considering the energy consumption problem, the first calcination temperature is preferably selected as 200°C.

[0075] Example 7

[0076] Example 7 is the same as the other steps of Example 7, except that the first calcination time in step (4) is changed from 3 hours to 4 hours. After calcination for 3 hours and 4 hours, the water can be completely evaporated to obtain a light yellow amorphous state. Considering the problem of energy consumption, the first calcination time is preferably selected as 3 hours.

[0077] Example 8

[0078] Example 8 is the same as Example 1 in other steps, except that the second step calcination temperature in step (4) is changed from 400°C to 450°C. After calcination at 400°C and 450°C, a colorless and transparent cesium fluoride aqueous solution can be obtained. Considering the problem of energy consumption, the second step calcination temperature is preferably selected to be 400°C.

[0079] Example 9

[0080] Example 9 is the same as Example 1 in other steps, except that the second step calcination time in step (4) is changed from 4 hours to 3 hours. When the calcination time is 3 hours, a colorless and transparent cesium fluoride aqueous solution cannot be obtained, and the obtained cesium fluoride solution is slightly yellow. Considering the color and purity of the obtained cesium fluoride, the second step calcination time is preferably selected to be 4 hours.

[0081] Example 10

[0082] The other steps of Example 10 are the same as those of Example 1, except that the solid-liquid mass ratio of the dissolution in step (5) is changed from 1:3 to 1:5. Both the solid-liquid mass ratio of 1:3 and 1:5 can dissolve the deactivated cesium fluoride after high temperature treatment. Considering the problem of liquid volume, the dissolution solid-liquid mass ratio of 1:3 is preferably selected.

[0083] Embodiment 11

[0084] Example 11 is the same as Example 1 in other steps, except that the first calcination temperature in step (6) is changed from 200°C to 250°C. After calcination at 200°C and 250°C for 3h, the water can be completely evaporated to obtain a white amorphous state. Considering the energy consumption problem, the first calcination temperature is preferably selected as 200°C.

[0085] Example 12

[0086] Example 12 is the same as Example 1 in other steps, except that the first calcination time in step (6) is changed from 3 hours to 4 hours. After calcination for 3 hours and 4 hours, the water can be completely evaporated to obtain a white amorphous state. Considering the problem of energy consumption, the first calcination time is preferably selected as 3 hours.

[0087] Example 13

[0088] Example 13 is the same as Example 1 in other steps, except that the second step calcination temperature in step (6) is changed from 400°C to 450°C. After calcination at 400°C and 450°C, white blocky cesium fluoride crystals can be obtained after being dissolved in water. Considering the problem of energy consumption, the second step calcination temperature is preferably selected to be 400°C.

[0089] Embodiment 14

[0090] Example 14 is the same as Example 1 in other steps, except that the second step calcination time in step (6) is changed from 4 hours to 3 hours. When the calcination time is 3 hours, the cesium fluoride crystals cannot be completely transformed into blocky white crystals, so the second step calcination time is preferably 4 hours.

Claims

1. A method for recovering spent catalyst cesium fluoride produced in the synthesis process of perfluorohexanone, characterized in that: The steps include: (1) placing the spent catalyst cesium fluoride in a platinum crucible and calcining it under air flow at 400-450° C. to obtain calcined cesium fluoride; (2) adding water to dissolve the calcined cesium fluoride obtained in step (1) to obtain a cesium fluoride mixed solution containing black slag; (3) The mixed solution obtained in step (2) is first coarsely filtered using filter paper, and then finely filtered using a filter membrane to obtain a light yellow cesium fluoride aqueous solution; (4) The cesium fluoride aqueous solution obtained in step (3) is transferred into a platinum crucible, and then calcined for 3-4 hours under air flow conditions of 200-250°C, and then calcined for 3-4 hours under air flow conditions of 400-450°C. After the calcination, the temperature is cooled to room temperature to obtain a cesium fluoride solid; (5) further adding water to dissolve the cesium fluoride solid obtained in step (4) to obtain a secondary aqueous solution of cesium fluoride, and the secondary aqueous solution of cesium fluoride is first coarsely filtered using filter paper and then finely filtered using a filter membrane to obtain a clear and transparent aqueous solution of cesium fluoride; (6) placing the clear and transparent cesium fluoride aqueous solution obtained in step (5) in a platinum crucible and calcining it under air flow at 200-250° C. for 3-4 hours, then raising the temperature to 400-450° C. and continuing calcining under nitrogen flow until blocky white cesium fluoride crystals are obtained; (7) The blocky cesium fluoride crystals obtained in step (6) are crushed in a closed space to obtain white powdery cesium fluoride crystals that can be used as a catalyst.

2. A method for recovering spent catalyst cesium fluoride produced in the synthesis process of perfluorohexanone as claimed in claim 1, characterized in that: In step (1), the calcination time is 3-4 hours.

3. A method for recovering spent catalyst cesium fluoride produced in the synthesis process of perfluorohexanone as claimed in claim 1, characterized in that: In step (2), the solid-liquid mass ratio of cesium fluoride to water after calcination is 1:3-5.

4. A method for recovering spent catalyst cesium fluoride produced in the synthesis process of perfluorohexanone as claimed in claim 1, characterized in that: In step (3) and step (5), the pore size of the filter paper for coarse filtration is 1 μm, and the pore size of the filter membrane for fine filtration is 0.2 μm.

5. A method for recovering spent catalyst cesium fluoride produced in the synthesis process of perfluorohexanone as claimed in claim 1, characterized in that: In step (5), the solid-liquid mass ratio of cesium fluoride solid to water is 1:3-5.

6. A method for recovering spent catalyst cesium fluoride produced in the synthesis process of perfluorohexanone as claimed in claim 1, characterized in that: In step (6), the calcination time under nitrogen flow conditions is 3-4 hours.

Citation Information

Patent Citations

  • Preparation method of perfluorethyl isopropyl ketone

    CN102992986A

  • Continuous production process of perfluor-2-methyl-3-pentanone

    CN107879912A

  • Method for continuously and controllably preparing hexafluoropropylene dimer / trimer

    CN112830863A

  • A purification method for perfluorohexanone

    CN116969825B

  • Use of fluorinated ketones in fire extinguishing compositions

    US6478979B1