A raw material mixing method for preparing ultra-low expansion quartz glass

By uniformly mixing silicon tetrachloride and titanium tetrachloride gas in the gas mixing chamber, and adjusting the proportion using the protective gas and neural network model, the problems of insufficient mixing and insufficient expansion coefficient in the preparation of quartz glass in the prior art are solved. The effect of ultra-low expansion coefficient and large-size preparation is achieved.

CN118459058BActive Publication Date: 2024-11-12INNER MONGOLIA JINSHABUDI HENGTONG PHOTOELECTRIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410919531.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-12
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

In the preparation of ultra-low expansion quartz glass, silicon tetrachloride and titanium tetrachloride raw materials are insufficiently mixed, making it difficult to achieve the requirements of ultra-low expansion coefficient. The temperature resistance of the product decreases, the thermal expansion coefficient increases, and the sintered ingots. The material diameter is small, making it difficult to make large-sized blanks.

Method used

By mixing the gasified silicon tetrachloride gas with titanium tetrachloride gas in the gas mixing chamber, the gas flow direction and flow rate are detected using sensors, the mixing ratio and circulating mixing are adjusted, the mixing uniformity is ensured, and the protective gas control is used Gas phase reaction, combined with neural network model to adjust the deposition value, and adjust the ratio of silicon tetrachloride to titanium tetrachloride in real time.

Benefits of technology

The ultra-low thermal expansion coefficient of quartz glass is achieved, the diameter of the lump is increased, the large size preparation is ensured, the hydroxyl content is reduced, and the production stability and deposition efficiency are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118459058B_ABST
    Figure CN118459058B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of quartz glass production, and in particular to a raw material mixing method for preparing ultra-low expansion quartz glass, comprising: gasifying silicon tetrachloride raw material and titanium tetrachloride raw material respectively; passing the gasified silicon tetrachloride gas and titanium tetrachloride gas into a gas mixing chamber; determining the gas mixing degree according to the gas flow direction and flow rate at each position in the gas mixing chamber to determine whether to circulate and mix the mixed raw material gas; passing the mixed raw material gas whose gas mixing degree meets the preset standard into a protective gas chamber and controlling the ratio of the protective gas to the mixed raw material gas; passing the gas mixed in the protective gas chamber into a deposition furnace to prepare a quartz glass ingot, and determining the deposition value of the glass ingot according to the shrinkage change degree of the ingot size during the cooling process; and adjusting the mixing ratio of the silicon tetrachloride gas and the titanium tetrachloride gas according to the deposition value. The present invention can improve the mixing efficiency of the prepared quartz glass raw materials and improve production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of quartz glass production, and in particular to a raw material mixing method for preparing ultra-low expansion quartz glass. Background Art

[0002] In recent years, due to the special needs of certain fields, quartz glass is required to maintain its original high purity and heat resistance, and also has the requirement of ultra-low thermal expansion coefficient. For example, the fields of aerospace, astronomy, and EUV lithography require reflective optical components to have both a high lightweight rate and an extremely low thermal expansion coefficient to ensure that the optical components can maintain their surface accuracy when the temperature fluctuates. Large-sized ultra-low expansion quartz glass has good weldability and can be used to make honeycomb lightweight structures. It also has an extremely low thermal expansion coefficient and high deformation resistance, making it an ideal optical material in the field of high-end reflective optics.

[0003] At present, the existing technology mainly adopts "hydrogen-oxygen flame hydrolysis chemical vapor deposition (CVD) process" or "vapor axial deposition (VAD), also known as two-step method or SOOT method, which refers to low-temperature chemical vapor deposition to obtain loose body and then secondary high-temperature sintering", and doping titanium-containing compounds in the deposition process to prepare ultra-low expansion quartz glass. When the CVD method dopes titanium dioxide (mostly, doped with titanium tetrachloride hydrolysis), because the melting point of titanium dioxide is as high as 1870℃, which is about 200℃ higher than the melting point of silicon dioxide (formed by hydrolysis of silicon tetrachloride) of 1670℃, in order to melt titanium dioxide in quartz glass, the deposition temperature must be increased. However, too high a deposition temperature will cause the main quartz glass to soften severely and be difficult to form; in addition, because the hydrogen-oxygen flame atmosphere contains a large amount of water, the hydroxyl content of the product is as high as 1200ppm, which reduces the temperature resistance of the product and increases the thermal expansion coefficient (higher than 1×10 -7 / ℃). Although the SOOT method can increase the temperature and remove most of the hydroxyl groups (hydroxyl content is less than 5ppm) during the second sintering, the diameter of the sintered ingot is often very small (maximum 200mm) due to the limitation of the loose body diameter, making it difficult to make large-sized green sheets; at the same time, the stress is large and difficult to completely eliminate; in addition, there are many steps, the environment requires a thousand-level clean room, and the cost is high. Therefore, the use of anhydrous plasma flame chemical vapor deposition silicon tetrachloride method (PCVD) and doping with titanium tetrachloride can produce ideal large-size, low-hydroxyl, ultra-low expansion quartz glass in one step, which has great advantages.

[0004] Chinese patent publication number CN117645406A discloses a method and device for producing a low expansion coefficient quartz glass ingot, comprising: using concentrated hydrochloric acid as a solvent and SiCl 4 and TiCl 4The mixed raw material solution is prepared as a solute, and the mixed raw material solution in the mixing box is gasified into an evaporator through a branch pipe through an oxyhydrogen burner to form a raw material gas, and the raw material gas enters the feed pipe of the oxyhydrogen burner through a feed pipe and is ejected, and is melted at the focus of the oxyhydrogen flame and deposited in a crucible to form a quartz glass loose body; the prepared quartz glass loose body is vitrified under a high temperature condition of 1700-1750°C to obtain a finished quartz glass ingot with a low expansion coefficient.

[0005] It can be seen that the production method and production device of the low expansion coefficient quartz glass ingot provided by the above invention have the following problems: the hydrogen-oxygen flame atmosphere contains a large amount of water, which leads to a high hydroxyl content in the product, which reduces the temperature resistance of the product and increases the thermal expansion coefficient. In addition, due to the limitation of the diameter of the loose body, the sintered ingot is often very small in diameter, making it difficult to make large-sized quartz glass blanks and difficult to achieve the requirements of ultra-low expansion coefficient. Summary of the invention

[0006] To this end, the present invention provides a raw material mixing method for preparing ultra-low expansion quartz glass, which is used to overcome the problem in the prior art that the prepared quartz glass is difficult to achieve an ultra-low expansion coefficient due to insufficient mixing of silicon tetrachloride raw materials and titanium tetrachloride raw materials.

[0007] To achieve the above object, the present invention provides a raw material mixing method for preparing ultra-low expansion quartz glass, comprising:

[0008] Step S1, preheating and gasifying the silicon tetrachloride raw material and the titanium tetrachloride raw material in corresponding evaporators respectively;

[0009] Step S2, introducing the gasified silicon tetrachloride gas and titanium tetrachloride gas into a gas mixing chamber for gas mixing; wherein the interior of the gas mixing chamber is a cylindrical cavity extending in a horizontal direction;

[0010] Step S3, determining the gas mixing degree according to the gas flow direction and flow rate at several positions in the gas mixing chamber to determine whether to circulate and mix the mixed raw material gas;

[0011] Wherein, the sensors for detecting the gas flow direction and flow velocity in the gas mixing chamber are evenly arranged in the cylindrical cavity along the horizontal direction;

[0012] Step S4, introducing the mixed raw material gas whose gas mixing degree meets the preset standard into the protective gas chamber and controlling the ratio of the protective gas to the mixed raw material gas;

[0013] Step S5, passing the gas mixed in the protective gas chamber into the deposition furnace to react with oxygen to prepare a quartz glass ingot, and determining the deposition value of the glass ingot according to the shrinkage change degree of the ingot size during the cooling process;

[0014] Step S6, adjusting the mixing ratio of silicon tetrachloride gas and titanium tetrachloride gas according to the deposition value.

[0015] Further, in step S2, the titanium tetrachloride gas is introduced into the gas mixing chamber at the lower end of the gas mixing chamber input port along a first preset direction; the silicon tetrachloride gas is introduced into the gas mixing chamber at the upper end of the gas mixing chamber input port along a second preset direction; and the component of the first preset direction along the transverse direction of the input port cross section is parallel to and in opposite directions to the component of the second preset direction along the transverse direction of the input port cross section.

[0016] Furthermore, in step S3, the mixed raw material gas is circulated and mixed, including: outputting the mixed raw material gas within a preset range from the output port of the gas mixing chamber, and re-inputting the mixed raw material gas into the gas mixing chamber at the input port of the gas mixing chamber at a first gas flow rate; the gas mixing chamber is provided with an output branch, which is connected to the input branch of the gas mixing chamber input port.

[0017] Furthermore, in step S3, if the gas flow directions within the preset range of the gas mixing chamber from the output port are different and / or the change in gas flow rate per unit time is not within a preset change threshold, it is determined that the gas mixing degree does not meet the preset standard, and the mixed raw material gas is circulated and mixed.

[0018] Furthermore, in step S3, if the gas flow direction within the preset range of the gas mixing chamber from the output port is the same and the change in gas flow rate per unit time is less than a preset change threshold, it is determined that the gas mixing degree meets the preset standard.

[0019] Furthermore, the first gas flow rate is determined according to the gas flow rate at each position in the gas mixing chamber.

[0020] Furthermore, the first gas flow rate V is calculated by the following formula:

[0021] V=(a 1 ×v 1 +a 2 ×v 2 +…+a i ×v i +…+a n ×v n ) / (∑ n i=1 v i );

[0022] Wherein, i=1, 2, ..., n; n is the number of sensors for detecting gas flow rate in the gas mixing chamber, n≥2; v i is the gas flow rate detected by the i-th gas flow rate detecting sensor; a i v iThe corresponding weight coefficient.

[0023] Furthermore, in step S5, the step of determining the deposition value of the glass ingot according to the shrinkage change degree of the ingot size during the cooling process includes:

[0024] Step S51, obtaining the size of the block corresponding to each preset temperature point during the cooling process;

[0025] Step S52, inputting the size of each ingot into the target neural network model to obtain the deposition value of the glass ingot output by the target neural network model;

[0026] The target neural network model is obtained by the following steps:

[0027] Step S511, obtaining initial data of each quartz glass ingot in the historical data; the initial data includes the ingot size corresponding to each preset temperature point during the cooling process of each quartz glass ingot, and the deposition value corresponding to each quartz glass ingot;

[0028] Step S512, screening each quartz glass ingot according to a preset deposition value range;

[0029] Step S513, using the ingot size corresponding to each preset temperature point in the cooling process of each quartz glass ingot after screening as a training sample to obtain a training sample set, and using the deposition value corresponding to each quartz glass ingot as a sample label of the corresponding training sample;

[0030] Step S514: training the initial neural network model according to the training sample set to obtain a target neural network model.

[0031] Furthermore, in the step S6, the deposition value is inversely proportional to the amount of titanium tetrachloride gas introduced, and the mixing ratio of silicon tetrachloride gas to titanium tetrachloride gas is in the range of 15:1 to 10:1.

[0032] Furthermore, the preset range is a range of a length in the gas mixing chamber from the output port that is 1 / 4 to 1 / 5 of the length of the gas mixing chamber.

[0033] Compared with the prior art, the beneficial effect of the present invention is that the present invention can ensure that the two gases can be mixed evenly by passing the gasified silicon tetrachloride gas and titanium tetrachloride gas into a gas mixing chamber for gas mixing. Passing the mixed gas into the protective gas chamber and controlling the ratio of the protective gas to the mixed raw material gas can ensure the uniformity of the gas phase reaction, reduce the hydroxyl content, and ensure the deposition efficiency. Passing the gas mixed in the protective gas chamber into a deposition furnace to prepare a quartz glass ingot can increase the diameter of the ingot, thereby ensuring that larger-sized quartz glass can be prepared later. Determining the deposition value of the glass ingot according to the degree of shrinkage change of the ingot size during the cooling process, and adjusting the mixing ratio of the silicon tetrachloride gas and the titanium tetrachloride gas according to the deposition value, production stability can be ensured through real-time adjustment, and the prepared quartz glass can meet the requirements of ultra-low thermal expansion coefficient.

[0034] Furthermore, the present invention can improve the mixing efficiency of the two gases and ensure mixing uniformity by passing titanium tetrachloride gas into the gas mixing chamber at the lower end of the gas mixing chamber input port along a first preset direction, and passing silicon tetrachloride gas into the gas mixing chamber at the upper end of the gas mixing chamber input port along a second preset direction.

[0035] Furthermore, circulating and mixing the mixed raw material gas can ensure the uniformity of the mixing of the two gases, and can improve the gas mixing efficiency without excessively affecting the mixing process of the two gases passing into the gas mixing chamber.

[0036] Furthermore, the present invention determines whether it is necessary to circulate and mix the mixed raw material gas through the gas flow direction and flow rate within a preset range of the gas mixing chamber from the output port. If the two gases are mixed evenly, the gas flow direction near the output port should be uniform and the flow rate should be gentle, meeting the preset standard, and no circulated mixing is required. Otherwise, the two gases have not been mixed evenly near the output port, and the efficiency of relying solely on the natural mixing of the two gases is relatively low. Therefore, the mixed raw material gas is circulated and mixed to improve the mixing efficiency.

[0037] Furthermore, the cyclic mixing of the present invention is achieved by re-inputting a first gas flow rate into the gas mixing chamber at the input port of the gas mixing chamber, and by controlling the flow rate of the mixed gas to ensure that the circulating mixed gas does not excessively affect the mixing process of the two gases entering the gas mixing chamber during the cyclic mixing, thereby avoiding a reduction in the mixing efficiency of the two gases. The first gas flow rate is determined by the gas flow rate at each position in the gas mixing chamber, and can be adjusted in time according to the real-time mixing situation.

[0038] Furthermore, the present invention obtains the deposition value of the glass ingot by training the target neural network model, which can accurately characterize the degree of shrinkage change of the ingot size during the cooling process and improve the efficiency of data processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 A schematic diagram of the steps of the raw material mixing method for preparing ultra-low expansion quartz glass according to the present invention;

[0040] Figure 2 A flow chart of a raw material mixing method for preparing ultra-low expansion quartz glass according to the present invention;

[0041] Figure 3 A logic judgment diagram of a raw material mixing method for preparing ultra-low expansion quartz glass according to the present invention;

[0042] Figure 4 It is a schematic diagram of the structure of the gas mixing chamber of the present invention;

[0043] In the figure: 1. Gas mixing chamber; 2. Titanium tetrachloride gas branch; 3. Silicon tetrachloride gas branch; 4. Circulation mixing branch; 5. Valve for controlling the output of mixed raw material gas that meets preset standards; 6. Valve for controlling the circulation and mixing output of mixed raw material gas; 7. Protective gas branch; 8. Valve for controlling the output of gas after mixing in the protective gas chamber; 9. Protective gas chamber; 10. Gas output branch after mixing in the protective gas chamber; 11. Mixed raw material gas output branch. DETAILED DESCRIPTION

[0044] In order to make the objects and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0045] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.

[0046] It should be noted that, in the description of the present invention, terms such as "up", "down", "left", "right", "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is merely for the convenience of description and does not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present invention.

[0047] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be a connection between the two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. It can also be a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be a connection between the two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances.

[0048] See also Figure 1 , Figure 2 as well as Figure 3 As shown, Figure 1 A schematic diagram of the steps of the raw material mixing method for preparing ultra-low expansion quartz glass according to the present invention; Figure 2 A flow chart of a raw material mixing method for preparing ultra-low expansion quartz glass according to the present invention; Figure 3 The present invention is a logic judgment diagram of the raw material mixing method for preparing ultra-low expansion quartz glass.

[0049] The embodiment of the present invention provides a raw material mixing method for preparing ultra-low expansion quartz glass, comprising:

[0050] Step S1, preheating and gasifying the silicon tetrachloride raw material and the titanium tetrachloride raw material in corresponding evaporators respectively;

[0051] In practice, the silicon tetrachloride raw material is in liquid state and is preheated to above 60°C in the evaporator to become gaseous state, and the density of silicon tetrachloride gas is 7.58 g / L. The titanium tetrachloride raw material is in liquid state and is preheated to above 140°C in the evaporator to become gaseous state, and the density of titanium tetrachloride gas is 8.48 g / L.

[0052] See also Figure 4As shown, it is a schematic diagram of the structure of the gas mixing chamber of the present invention, the gas mixing chamber 1 input port is provided with a titanium tetrachloride gas branch 2, a silicon tetrachloride gas branch 3, and a circulating mixing branch 4, the titanium tetrachloride gas branch 2 is used to pass the preheated titanium tetrachloride gas into the gas mixing chamber 1, the silicon tetrachloride gas branch 3 is used to pass the preheated silicon tetrachloride gas into the gas mixing chamber 1; the gas mixing chamber 1 output port is provided with a mixed raw material gas output branch 11, which is used to output the mixed raw material gas, the mixed raw material gas output branch 11 is provided with a valve 5 for controlling the output of the mixed raw material gas that meets the preset standard, and a valve 6 for controlling the mixed raw material gas to be circulated and mixed and outputted, the valve 5 for controlling the output of the mixed raw material gas that meets the preset standard is normally closed and the valve 6 for controlling the mixed raw material gas to be circulated and mixed and outputted is opened, and the mixed raw material gas that meets the preset standard is controlled to be discharged. The valve 5 for controlling the output of the mixed raw material gas and the valve 6 for controlling the circulating mixed output of the mixed raw material gas are not opened at the same time. When the mixed raw material gas meets the preset standard, the valve 5 for controlling the output of the mixed raw material gas that meets the preset standard is opened, and when the mixed raw material gas does not meet the preset standard, the valve 6 for controlling the circulating mixed output of the mixed gas is opened; the protective gas chamber 9 is provided with a protective gas branch 7 and a gas output branch 10 after mixing through the protective gas chamber. The protective gas branch 7 is used to pass the protective gas into the protective gas chamber 9, and the gas output branch 10 after mixing through the protective gas chamber is used to output the gas mixed through the protective gas chamber. The gas output branch 10 after mixing through the protective gas chamber is provided with a valve 8 for controlling the output of the gas mixed through the protective gas chamber. The valve 8 for controlling the output of the gas mixed through the protective gas chamber is normally closed, and is opened when the mixed raw material gas and the protective gas are evenly mixed.

[0053] Step S2, introducing the gasified silicon tetrachloride gas and titanium tetrachloride gas into a gas mixing chamber 1 for gas mixing; wherein the interior of the gas mixing chamber 1 is a cylindrical cavity extending in a horizontal direction;

[0054] In practice, since the initial temperatures of silicon tetrachloride gas and titanium tetrachloride gas are inconsistent, in order to avoid liquefaction of titanium tetrachloride gas, the temperature inside the gas mixing chamber is maintained above 140°C, and the silicon tetrachloride raw material is preheated to above 140°C in the evaporator.

[0055] Specifically, in step S2, the titanium tetrachloride gas is introduced into the gas mixing chamber at the lower end of the gas mixing chamber input port along a first preset direction; the silicon tetrachloride gas is introduced into the gas mixing chamber at the upper end of the gas mixing chamber input port along a second preset direction; the component of the first preset direction along the transverse direction of the input port section is parallel to and opposite to the component of the second preset direction along the transverse direction of the input port section.

[0056] In implementation, silicon tetrachloride gas and titanium tetrachloride gas are introduced into the gas mixing chamber at corresponding flow rates respectively. Since the density of silicon tetrachloride gas is smaller than that of titanium tetrachloride gas, silicon tetrachloride gas is introduced at the upper end of the gas mixing chamber input port. After the introduction, the silicon tetrachloride gas sinks under the action of the initial flow rate, but due to its small density, it has a tendency to float. Titanium tetrachloride gas is introduced at the lower end of the gas mixing chamber input port. After the introduction, the titanium tetrachloride gas floats under the action of the initial flow rate, but due to its large density, it has a tendency to sink. Silicon tetrachloride gas and titanium tetrachloride gas will be mixed inside the gas mixing chamber, which can increase the mixing speed of silicon tetrachloride gas and titanium tetrachloride gas and make them mix faster and more evenly.

[0057] It should be noted that in actual application scenarios, actual implementers can determine the first preset direction and the second preset direction based on the actual situation and the specific length (extension direction) size and diameter size of the gas mixing chamber to obtain the best mixing effect through a limited number of tests. Preferably, the components of the first preset direction and the second preset direction along the cross-section of the gas mixing chamber are 30°~45° to the horizontal direction, and the components of the first preset direction and the second preset direction along the extension direction of the gas mixing chamber are related to the length size of the gas mixing chamber.

[0058] The present invention can improve the mixing efficiency of the two gases and ensure mixing uniformity by passing titanium tetrachloride gas into the gas mixing chamber at the lower end of the gas mixing chamber input port along a first preset direction and passing silicon tetrachloride gas into the gas mixing chamber at the upper end of the gas mixing chamber input port along a second preset direction.

[0059] Step S3, determining the gas mixing degree according to the gas flow direction and flow rate at several positions in the gas mixing chamber to determine whether to circulate and mix the mixed raw material gas;

[0060] Wherein, the sensors for detecting the gas flow direction and flow velocity in the gas mixing chamber are evenly arranged in the cylindrical cavity along the horizontal direction;

[0061] It should be noted that those skilled in the art know that any sensor capable of detecting the gas flow direction and flow rate in the prior art falls within the protection scope of the present invention and will not be described in detail herein.

[0062] Specifically, in step S3, the mixed raw material gas is circulated and mixed, including: outputting the mixed raw material gas within a preset range from the output port of the gas mixing chamber, and re-inputting the mixed raw material gas into the gas mixing chamber at the input port of the gas mixing chamber at a first gas flow rate; the gas mixing chamber is provided with an output branch, which is connected to the input branch of the gas mixing chamber input port.

[0063] In actual application scenarios, the branch for transporting the circulating mixed gas can be set at the center of the gas mixing chamber input port to avoid affecting the direction and flow rate of silicon tetrachloride gas and titanium tetrachloride gas respectively entering the gas mixing chamber.

[0064] In practice, the mixed raw material gas is circulated and mixed, which can ensure the uniformity of the mixing of the two gases and improve the gas mixing efficiency without excessively affecting the mixing process of the two gases passing into the gas mixing chamber.

[0065] Specifically, in step S3, if the gas flow directions within the preset range of the gas mixing chamber from the output port are different and / or the change in gas flow rate per unit time is not within the preset change threshold, it is determined that the gas mixing degree does not meet the preset standard, and the mixed raw material gas is circulated and mixed.

[0066] Specifically, in step S3, if the gas flow direction within the preset range of the gas mixing chamber from the output port is the same and the change in gas flow rate per unit time is less than a preset change threshold, it is determined that the gas mixing degree meets the preset standard.

[0067] In implementation, the preset range is generally set to be within a range of 1 / 4 to 1 / 5 of the length of the gas mixing chamber from the outlet, and at least two sensors are arranged within the preset range to detect the gas flow direction and gas flow rate at the corresponding position. In actual application scenarios, the actual implementer can set the preset range according to actual conditions. By setting the preset range, it can be detected in real time whether the two gases are mixed evenly near the outlet, so as to avoid uneven mixing of silicon tetrachloride gas and titanium tetrachloride gas, resulting in poor quality of the prepared quartz glass and non-compliant thermal expansion coefficient.

[0068] In actual application scenarios, the gas flow direction of each corresponding position is determined according to the detection results of each sensor within the preset range, and the change in gas flow rate per unit time is determined according to the average value of the change in gas flow rate at each corresponding position within the preset time period. For example, if there are three sensors for detecting gas flow rate within the preset range, the detected initial gas flow rates are 1mm / s, 2mm / s, and 3mm / s, respectively, and the target gas flow rates are 1mm / s, 1mm / s, and 2mm / s, respectively, and the preset time period is 2s, then the changes in gas flow rate per unit time at each corresponding position are 0 and 0.5mm / s, respectively. 2 , 0.5mm / s 2 , then the change of gas flow rate per unit time within the preset range is 1 / 3mm / s 2 .

[0069] Specifically, the actual implementer can set the preset change threshold according to the actual situation. The smaller the preset change threshold, the higher the requirement for the change of gas flow rate per unit time within the preset range. Preferably, the preset change threshold is set to 10 mm / s 2 -15mm / s 2 .

[0070] In implementation, the present invention determines whether it is necessary to circulate and mix the mixed raw material gas through the gas flow direction and flow rate within a preset range of the gas mixing chamber from the output port. If the two gases are mixed evenly, the gas flow direction near the output port should be uniform and the flow rate should be gentle, meeting the preset standard, and no circulated mixing is required. Otherwise, the two gases have not been mixed evenly near the output port, and the efficiency of relying solely on the natural mixing of the two gases is relatively low. Therefore, the mixed raw material gas is circulated and mixed to improve the mixing efficiency.

[0071] Specifically, the first gas flow rate is determined according to the gas flow rate at each position in the gas mixing chamber.

[0072] Specifically, the first gas flow rate V is calculated by the following formula:

[0073] V=(a 1 ×v 1 +a 2 ×v 2 +…+a i ×v i +…+a n ×v n ) / (∑ n i=1 v i );

[0074] Wherein, i=1, 2, ..., n; n is the number of sensors for detecting gas flow rate in the gas mixing chamber, n≥2; v i is the gas flow rate detected by the i-th gas flow rate detecting sensor; a i v i The corresponding weight coefficient.

[0075] Specifically, n i=1 a i=1, in the actual application scenario, the actual implementer can set the weight coefficient according to the actual situation. Generally, due to the different flow rates of the mixed raw gas at various positions, after the valve 6 for controlling the mixed gas to be circulated and mixed and outputted at the gas mixing chamber output port is opened, the mixed raw gas at the gas mixing chamber output port position is first outputted to the circulating mixing branch, which has a certain influence on the flow rate of the first gas. In order to avoid the mixed raw gas from affecting the mixing process of the two gases entering the gas mixing chamber too much when it is introduced into the gas mixing chamber input port, the flow rate of the first gas is also affected by the gas flow rate at the gas mixing chamber input port position. The gas flow rate at the middle position has little influence on the output flow rate of the mixed raw gas, and is also less affected by the mixed raw gas introduced into the circulating mixing branch, so it has little influence on the flow rate of the first gas. Thus, the weight coefficient corresponding to the sensor in the middle of the mixed gas chamber is smaller, and the weight coefficient corresponding to the sensor close to the input port and the output port is larger. For example, sensors A1, A2, A3, A4 and A5 are evenly distributed at the same height from the input port to the output port of the gas mixing chamber 1. The weight coefficients corresponding to sensors A1 and A5 are both set to 0.3, the weight coefficients corresponding to sensors A2 and A4 are set to 0.17, and the weight coefficient corresponding to sensor A3 is set to 0.06.

[0076] In practice, the cyclic mixing of the present invention is achieved by re-inputting a first gas flow rate into the gas mixing chamber at the input port of the gas mixing chamber, and by controlling the flow rate of the mixed gas to ensure that the circulating mixed gas does not excessively affect the mixing process of the two gases entering the gas mixing chamber during the cyclic mixing, thereby avoiding a reduction in the mixing efficiency of the two gases. The first gas flow rate is determined by the gas flow rate at each position in the gas mixing chamber, and can be adjusted in time according to the real-time mixing situation.

[0077] Step S4, introducing the mixed raw material gas whose gas mixing degree meets the preset standard into the protective gas chamber and controlling the ratio of the protective gas to the mixed raw material gas;

[0078] In practice, the protective gas may be any inert gas or a mixture of inert gases, for example, any one or more of the inert gases such as argon, neon, and nitrogen.

[0079] Specifically, the mixed gas is introduced into the protective gas chamber and the ratio of the protective gas to the mixed raw material gas is controlled to ensure the uniformity of the gas phase reaction. The protective gas can ensure that the gas phase reaction occurs uniformly, so as to achieve the addition of an appropriate amount of titanium dioxide into the prepared quartz glass lump, ensure the quality of the quartz glass, and reduce the hydroxyl content. In addition, by controlling the ratio of the protective gas to the mixed raw material gas, the production quality can be ensured while increasing the deposition rate.

[0080] Step S5, passing the gas mixed in the protective gas chamber into the deposition furnace to react with oxygen to prepare a quartz glass ingot, and determining the deposition value of the glass ingot according to the shrinkage change degree of the ingot size during the cooling process;

[0081] In actual application scenarios, the gas mixed in the protective gas chamber is introduced into the feeder on the deposition furnace, which is embedded in the top of the deposition furnace. A torch and a quartz matrix are set in the deposition furnace. The torch uses an inductively coupled plasma flame as a heat source, and a mixed gas of air and chlorine is used as a plasma ionization gas. The gas mixed in the protective gas chamber is introduced into the deposition furnace to react with oxygen to generate silicon dioxide doped with an appropriate amount of titanium dioxide, which is deposited on the quartz matrix inside the deposition furnace. The reaction chemical formula in the deposition furnace is: SiCl 4 +TiCl 4 +2O 2 =SiO 2 +TiO 2 +4Cl 2。

[0082] In practice, the size of the lump can be increased by adjusting the temperature in the deposition furnace. In actual application scenarios, the titanium tetrachloride gas flow rate is 3-10g / min, the silicon tetrachloride gas flow rate is 30-100g / min, the lump production speed is 500-1500g / h, the diameter is 200-350mm, and the plasma coil power is increased to increase the deposition temperature. The plasma coil power is 100KW and 200KW before and after the increase, respectively, and the deposition temperature (furnace wall temperature at the deposition surface) is 1400℃ and 1550℃ before and after. Increasing the power can use a large-diameter burner, increase the working ionized gas introduced, increase the flame diameter, increase the deposition surface, and reduce the gap between the side wall of the lump and the inner wall of the deposition furnace, resulting in an increase in furnace temperature and an increase in material discharge speed.

[0083] Specifically, the ingot is cylindrical, and the top deposition surface is approximately hemispherical. It is transparent because it is in a high-temperature zone and is covered by flames. An opaque slag layer of unmelted silicon dioxide (containing a small amount of titanium dioxide) is attached to the edge. The stably deposited ingot has equal diameters at the top and bottom. The mixed gas (a mixture of silicon tetrachloride gas, titanium tetrachloride gas, and protective gas) ejected from the feeder is oxidized into silicon dioxide (containing titanium dioxide) along the direction of the flame, covering and depositing on the entire upper surface of the ingot (approximately hemispherical surface), and melted into a glassy state under the action of the high-temperature flame. After the ingot is cut into ingots, it is placed in a trough sink furnace under vacuum or gas protection at a high temperature of 1900°C to soften naturally and spread into a flat billet.

[0084] Specifically, in step S5, the deposition value of the glass ingot is determined according to the shrinkage change degree of the ingot size during the cooling process, including:

[0085] Step S51, obtaining the size of the block corresponding to each preset temperature point during the cooling process;

[0086] Step S52, inputting the sizes of each glass ingot into the target neural network model to obtain the deposition value of the glass ingot output by the target neural network model.

[0087] The target neural network model is obtained by the following steps:

[0088] Step S511, obtaining initial data of each quartz glass ingot in the historical data; the initial data includes the ingot size corresponding to each preset temperature point during the cooling process of each quartz glass ingot, and the deposition value corresponding to each quartz glass ingot;

[0089] Step S512, screening each quartz glass ingot according to a preset deposition value range;

[0090] Step S513, using the ingot size corresponding to each preset temperature point in the cooling process of each quartz glass ingot after screening as a training sample to obtain a training sample set, and using the deposition value corresponding to each quartz glass ingot as a sample label of the corresponding training sample;

[0091] Step S514: training the initial neural network model according to the training sample set to obtain a target neural network model.

[0092] It should be noted that those skilled in the art know that any neural network model in the prior art that can determine the sedimentation value falls within the protection scope of the present invention and will not be described in detail here.

[0093] In actual application scenarios, actual implementers can set a preset deposition value range based on historical preparation data and preparation requirements according to actual conditions.

[0094] In implementation, the present invention obtains the deposition value of the glass ingot by training the target neural network model, which can accurately characterize the degree of shrinkage change of the ingot size during the cooling process and improve the efficiency of data processing.

[0095] Step S6, adjusting the mixing ratio of silicon tetrachloride gas and titanium tetrachloride gas according to the deposition value.

[0096] Specifically, in step S6, the deposition value is inversely proportional to the amount of titanium tetrachloride gas introduced, and the mixing ratio of silicon tetrachloride gas to titanium tetrachloride gas is in the range of 15:1 to 10:1.

[0097] Specifically, a preset comparison table is provided according to the inverse relationship between the deposition value and the amount of titanium tetrachloride gas introduced and the historical adjustment value, and the mixing ratio of silicon tetrachloride gas and titanium tetrachloride gas is adjusted according to the deposition value based on the preset comparison table.

[0098] In a specific embodiment, the comparison of the effects of adding different amounts of titanium tetrachloride on the thermal expansion coefficient is shown in Table 1:

[0099] Table 1 Effect of adding different amounts of titanium tetrachloride on the thermal expansion coefficient

[0100]

[0101] The present invention ensures that the two gases can be evenly mixed by passing the gasified silicon tetrachloride gas and titanium tetrachloride gas into a gas mixing chamber for gas mixing. Passing the mixed gas into a protective gas chamber and controlling the ratio of the protective gas to the mixed raw material gas can ensure the uniformity of the gas phase reaction, reduce the hydroxyl content, and ensure the deposition efficiency. Passing the mixed gas in the protective gas chamber into a deposition furnace to prepare a quartz glass ingot can increase the diameter of the ingot, thereby ensuring that larger-sized quartz glass can be prepared later. Determining the deposition value of the glass ingot according to the degree of shrinkage change of the ingot size during the cooling process, and adjusting the mixing ratio of the silicon tetrachloride gas and the titanium tetrachloride gas according to the deposition value, production stability can be ensured through real-time adjustment, and the prepared quartz glass can meet the requirements of ultra-low thermal expansion coefficient.

[0102] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

Claims

1. A raw material mixing method for preparing ultra-low expansion quartz glass, characterized in that: include: Step S1, preheating and gasifying the silicon tetrachloride raw material and the titanium tetrachloride raw material in corresponding evaporators respectively; Step S2, introducing the gasified silicon tetrachloride gas and titanium tetrachloride gas into a gas mixing chamber for gas mixing; wherein the interior of the gas mixing chamber is a cylindrical cavity extending in a horizontal direction; Step S3, determining the gas mixing degree according to the gas flow direction and flow rate at several positions in the gas mixing chamber to determine whether to circulate and mix the mixed raw material gas; Wherein, the sensors for detecting the gas flow direction and flow velocity in the gas mixing chamber are evenly arranged in the cylindrical cavity along the horizontal direction; Step S4, introducing the mixed raw material gas whose gas mixing degree meets the preset standard into the protective gas chamber and controlling the ratio of the protective gas to the mixed raw material gas; Step S5, passing the gas mixed in the protective gas chamber into the deposition furnace to react with oxygen to prepare a quartz glass ingot, and determining the deposition value of the glass ingot according to the shrinkage change degree of the ingot size during the cooling process; Step S6, adjusting the mixing ratio of silicon tetrachloride gas and titanium tetrachloride gas according to the deposition value.

2. The raw material mixing method for preparing ultra-low expansion quartz glass according to claim 1, characterized in that: In step S2, the titanium tetrachloride gas is introduced into the gas mixing chamber at the lower end of the gas mixing chamber input port along a first preset direction; the silicon tetrachloride gas is introduced into the gas mixing chamber at the upper end of the gas mixing chamber input port along a second preset direction; the component of the first preset direction along the transverse direction of the input port section is parallel to and opposite to the component of the second preset direction along the transverse direction of the input port section.

3. The raw material mixing method for preparing ultra-low expansion quartz glass according to claim 2, characterized in that: In step S3, the mixed raw material gas is circulated and mixed, including: outputting the mixed raw material gas within a preset range from the output port of the gas mixing chamber, and re-inputting the mixed raw material gas into the gas mixing chamber at the input port of the gas mixing chamber at a first gas flow rate; the gas mixing chamber is provided with an output branch, which is connected to the input branch of the gas mixing chamber input port.

4. The raw material mixing method for preparing ultra-low expansion quartz glass according to claim 3, characterized in that: In step S3, if the gas flow directions within the preset range of the gas mixing chamber from the output port are different and / or the change in gas flow rate per unit time is not within the preset change threshold, it is determined that the gas mixing degree does not meet the preset standard, and the mixed raw material gas is circulated and mixed.

5. The raw material mixing method for preparing ultra-low expansion quartz glass according to claim 4, characterized in that: In step S3, if the gas flow direction within the preset range of the gas mixing chamber from the output port is the same and the change in gas flow rate per unit time is less than a preset change threshold, it is determined that the gas mixing degree meets the preset standard.

6. The raw material mixing method for preparing ultra-low expansion quartz glass according to claim 5, characterized in that: The first gas flow rate is determined according to the gas flow rate at each position in the gas mixing chamber.

7. The raw material mixing method for preparing ultra-low expansion quartz glass according to claim 6, characterized in that: The first gas flow rate V is calculated by the following formula: V=(a1×v1+a2×v2+…+a i ×v i +…+a n ×v n ) / (∑ n i=1 in i ); Wherein, i=1, 2, ..., n; n is the number of sensors for detecting gas flow rate in the gas mixing chamber, n≥2; v i is the gas flow rate detected by the i-th gas flow rate detecting sensor; a i v i The corresponding weight coefficient.

8. The raw material mixing method for preparing ultra-low expansion quartz glass according to claim 1, characterized in that: In step S5, the step of determining the deposition value of the glass ingot according to the shrinkage change degree of the ingot size during the cooling process includes: Step S51, obtaining the size of the block corresponding to each preset temperature point during the cooling process; Step S52, inputting the size of each ingot into the target neural network model to obtain the deposition value of the glass ingot output by the target neural network model; The target neural network model is obtained by the following steps: Step S511, obtaining initial data of each quartz glass ingot in the historical data; the initial data includes the ingot size corresponding to each preset temperature point during the cooling process of each quartz glass ingot, and the deposition value corresponding to each quartz glass ingot; Step S512, screening each quartz glass ingot according to a preset deposition value range; Step S513, using the ingot size corresponding to each preset temperature point in the cooling process of each quartz glass ingot after screening as a training sample to obtain a training sample set, and using the deposition value corresponding to each quartz glass ingot as a sample label of the corresponding training sample; Step S514: training the initial neural network model according to the training sample set to obtain a target neural network model.

9. The raw material mixing method for preparing ultra-low expansion quartz glass according to claim 1, characterized in that: In the step S6, the deposition value is inversely proportional to the amount of titanium tetrachloride gas introduced, and the mixing ratio of silicon tetrachloride gas to titanium tetrachloride gas is in the range of 15:1 to 10:

1.

10. The raw material mixing method for preparing ultra-low expansion quartz glass according to claim 3, 4 or 5, characterized in that: The preset range is a range of lengths in the gas mixing chamber from the output port that is 1 / 4 to 1 / 5 of the length of the gas mixing chamber.