Tape casting method for ultra-thin silicon nitride substrate with low energy consumption and low VOC
Through modified ethyl cellulose and planetary ball milling technology, the problems of poor fluidity and low solid content in the manufacturing of silicon nitride substrates are solved, and high-quality, low-energy consumption silicon nitride ultra-thin substrate production is achieved, satisfying nitriding Application requirements of silicon substrates in AMB.
Patent Information
- Application Number
- CN202410488526.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-04-23
AI Technical Summary
In the manufacturing of existing silicon nitride substrates, there are irregular powders, poor fluidity, poor surface quality, low solids content, high energy consumption and environmental protection problems, making it difficult to achieve high-quality and efficient casting.
Using suitable binders, modifiers, dispersants and sintering aids, mixed grinding and casting are carried out through modified ethyl cellulose and planetary ball milling technology to form a high-quality silicon nitride ultra-thin substrate.
It has achieved high quality, low energy consumption, and low VOC (absorbable harmful substances) production of silicon nitride ultra-thin substrates, with smooth surface, small thickness tolerance, high solid content, excellent thermal conductivity and bending strength.
Smart Images

Figure CN118459231B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicon nitride ceramic tape casting, and in particular belongs to a tape casting method for a low-energy-consumption and low-VOC silicon nitride ultra-thin substrate. Background Art
[0002] Silicon nitride substrate is one of the important materials in the third generation semiconductor. At present, silicon nitride ceramic substrate is widely used in SiCMOSFET.
[0003] There are some challenges in the manufacture of silicon nitride substrates, such as the irregular shape and poor fluidity of silicon nitride powder, which makes it difficult to perform tape casting. For the application of silicon nitride substrates in AMB, the substrates cannot be ground because the ground surface will fail with the metallization layer during the temperature cycle test. Therefore, the surface quality requirements of the tape-cast green porcelain are very high, and the thickness tolerance control requirements of the tape-cast green porcelain are also very high. Therefore, tape casting technology is one of the key factors in the production of silicon nitride substrates.
[0004] Patent document CN113149662B discloses a method for preparing a high thermal conductivity silicon nitride ceramic cast film and its application. The method selects DBP (dibutyl phthalate) plasticizer as a raw material, but the plasticizer has been banned in Europe. In the preparation method, homogenous stirring and primary ball milling are used instead of the traditional secondary ball milling to achieve the same dispersion effect as the secondary ball milling in the traditional method, but two mixing processes are still required to prepare the first slurry and the second slurry respectively. The solid content of the product obtained by this method is only 48.5~52%.
[0005] However, there are still some problems in the prior art. In terms of raw material selection, the commonly used plasticizer raw material phthalates are not environmentally friendly, and the commonly used dispersants such as triethyl phosphate, polyacrylic acid, castor oil or polyvinyl pyrrolidone have poor dispersibility. The binders used are polyvinyl butyral and polyvinyl alcohol with high thermal decomposition temperatures. In terms of preparation process, the mixed ball milling method in the prior art is complicated and inefficient, and often cannot obtain the required slurry in one go; the casting temperature is high and the temperature difference is large, so the surface quality of the prepared product is poor. Due to raw material and process defects, the corresponding silicon nitride sheet may face problems such as poor surface quality, large tolerance, low solid content, and high energy consumption.
[0006] In general, the production and application of silicon nitride substrates face some challenges, but by researching and improving preparation methods and processes, these problems can be overcome, the quality and performance of silicon nitride substrates can be improved, and domestic substitution and market competition can be achieved. Summary of the invention
[0007] The present invention overcomes the defects of raw material selection and preparation process in the prior art, and provides a tape casting method for low-energy consumption and low-VOC silicon nitride ultra-thin substrates. The technical solution provided by the present invention selects suitable binders, modifiers, dispersants and sintering aids, and proposes a new mixed grinding and tape casting process. Through this method, a silicon nitride ultra-thin substrate with high quality, good leveling and high solid content is finally obtained.
[0008] The present invention provides a tape casting method for a low-energy-consumption, low-VOC silicon nitride ultra-thin substrate, comprising the following steps:
[0009] S1. A modifier and ethyl cellulose are modified to form modified ethyl cellulose; the modifier is dioctyl terephthalate (DOTP);
[0010] S2. The grinding balls, silicon nitride powder, mixed sintering aid, dispersant, solvent and modified ethyl cellulose are mixed and ground to form a slurry;
[0011] S3. Degassing the slurry, and sequentially tape-casting at four temperature ranges of 23-27°C, 28-32°C, 33-37°C, and 38-42°C to obtain silicon nitride ultra-thin substrate green ceramics, and then debinding and sintering to obtain low-energy consumption and low-VOC silicon nitride ultra-thin substrates.
[0012] The mixed sintering aids are Ho2O3 and MgF2.
[0013] The dispersant is one or more of oleic acid, polyoxyethylene oleate, and Solsperse 17000.
[0014] The solvent is anhydrous ethanol and / or propylene glycol methyl ether.
[0015] The slurry includes 50 to 60 parts of silicon nitride powder, 5 to 7 parts of mixed sintering aid, 0.1 to 0.6 parts of dispersant, 15 to 24.4 parts of solvent and 10 to 15 parts of modified ethyl cellulose in parts by mass.
[0016] Furthermore, the solvent is 15 to 21.96 parts of ethanol and 2.44 to 9.24 parts of propylene glycol methyl ether.
[0017] Furthermore, the dispersant contains 0-0.4 parts of oleic acid, 0-0.4 parts of polyoxyethylene oleate, and 0.1-0.3 parts of Solsperse 17000.
[0018] Furthermore, the mixed sintering aid is 2 to 3 parts of Ho2O3 and 3 to 4 parts of MgF2.
[0019] The modification operation is to stir in a reactor at a temperature of 35-40° C. for 4-6 hours.
[0020] The mass ratio of the ethyl cellulose to the modifier is (75-80): (20-25); wherein, in the prior art, polyvinyl butyral and polyvinyl alcohol are used as binders, and the thermal decomposition temperature (200-240° C.) is high, while the thermal decomposition temperature of the ethyl cellulose used in the present invention is 200° C.
[0021] In the modification process of the present invention, the modification of ethyl cellulose mainly involves two aspects: first, the residual hydroxyl groups of ethyl cellulose can form hydrogen bonds with dioctyl phthalate, and the hydrogen bonds formed between these two polar molecules help reduce the surface energy between molecules. Secondly, the residual hydroxyl groups on ethyl cellulose can introduce benzene-containing functional groups on the ethyl cellulose chain when reacting with DOTP (a plasticizer), enhance the hydrophobic effect, and its dispersibility in the system can be regulated after modification. Dioctyl phthalate, as a commonly used plasticizer, can increase the flexibility of ethyl cellulose in the present invention. Through this modification reaction, the properties of ethyl cellulose are changed, including its solubility and toughness, thereby improving the fluidity of the slurry. In short, by adjusting the polarity between molecules, the adhesion and dispersibility of the modified ethyl cellulose are optimized in the system, which helps to reduce the defects that may occur during the molding process. Therefore, through the above-mentioned modification process, a silicon nitride ultra-thin substrate with a small thickness tolerance and extreme difference can be obtained, and the substrate surface is smooth, without cracks and pits.
[0022] The device used for the mixed ball milling is a planetary ball mill; if an ordinary ball mill is used, the ball milling time is relatively long (for example, the ball milling time of CN113149662B requires 24 hours), while the planetary ball mill can rotate and revolve simultaneously, and the grinding efficiency is higher.
[0023] The orbital speed in the mixing ball mill is 50-200 rpm, and the rotation speed is 100-400 rpm.
[0024] The mixing and grinding time is 5 to 6 hours.
[0025] The grinding balls are three times the weight of the silicon nitride powder.
[0026] The tape casting process is performed at each temperature for 4 to 6 hours.
[0027] The casting speed is 0.05-0.1 m / min.
[0028] The vacuum negative pressure of the degassing treatment is 0.05-0.1 MPa, the temperature of the degassing treatment is 35° C., and the time of the degassing treatment is 9-10 hours.
[0029] The viscosity of the slurry after the degassing treatment is controlled at 20000-30000 mPa·S.
[0030] The debinding temperature is 500-550° C., and the debinding time is 12-24 hours.
[0031] The sintering temperature is 1880-1930° C., and the sintering time is 2-10 hours.
[0032] In the present invention, the casting temperature changes slightly, which is not likely to cause problems such as product cracking and bubbling caused by a large temperature change; and the required temperature is low, so the energy consumption is low.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] 1. In terms of raw material selection, the present invention adopts low molecular weight ethyl cellulose, which has a lower thermal decomposition (200°C) and is therefore easier to debond; at the same time, an environmentally friendly plasticizer DOTP is used to better protect the environment; in addition, oleic acid, oleic acid polyoxyethylene ester and Solsperse 17000 are used as dispersants to provide good dispersibility effects, reduce the viscosity of the slurry, and achieve a high solid content.
[0035] 2. In terms of process, the present invention uses a planetary ball mill to mill the raw materials once to obtain a slurry, which can greatly shorten the grinding time, improve efficiency, and reduce energy consumption. In addition, the casting temperature changes less, avoiding the occurrence of problems such as product cracking and bubbling due to large temperature changes. Moreover, the maximum casting temperature is only 40°C, and the temperature required for casting molding is relatively low, thereby reducing energy consumption and further reducing production costs.
[0036] 3. In terms of product effects, the thermal conductivity of the silicon nitride ultra-thin substrate obtained by the present invention is 82~95W / (m·k), the bending strength is 708~810Mpa, the warpage is less than 2%, the thickness tolerance is less than ±0.03, the solid content can reach 60~65%, the substrate surface is smooth, without cracks or concave resistance; the substrate thickness tolerance is small, the single-piece extreme difference is small, and the leveling property is good. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a raw ceramic picture of the silicon nitride ultra-thin substrate prepared by the method of the present invention.
[0038] Figure 2 This is a surface picture of the raw ceramic of the silicon nitride ultra-thin substrate prepared by the method of the present invention.
[0039] Figure 3 This is a picture of the silicon nitride ultra-thin substrate prepared by the method of the present invention.
[0040] Figure 4 This is a picture of the raw ceramic of the silicon nitride ultra-thin substrate prepared in Comparative Example 1. DETAILED DESCRIPTION
[0041] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0042] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Example 1
[0043] S1. Use environmentally friendly plasticizer DOTP to modify ethyl cellulose, add 23% DOTP and 77% ethyl cellulose; stir in a reactor at 35-40°C for 5 hours to obtain low-viscosity modified ethyl cellulose;
[0044] S2. Add grinding balls to a planetary ball mill, the grinding balls are 3 times the weight ratio of silicon nitride powder, add 560g silicon nitride powder, 20gHo2O3, 40gMgF2, 4g oleic acid, 2gSolsperse 17000, add 219.6g anhydrous ethanol, 24.4g propylene glycol methyl ether, 130g modified ethyl cellulose, mix for 6 hours, the planetary mill revolution is 70rpm, rotation is 140rpm, to form a slurry;
[0045] S3. The silicon nitride slurry is subjected to degassing treatment at a vacuum negative pressure of 0.05~0.1MPa, a temperature of 35°C, and a treatment period of 10 hours. The viscosity is controlled at 20000~30000mPa·s. Tape casting is performed in sequence at four temperatures of 25°C, 30°C, 35°C, and 40°C, with a treatment period of 5 hours at each temperature, a casting speed of 0.05~0.1m / min, debinding at 500~550°C for 24 hours, and sintering at 1880~1930°C for 5 hours. The silicon nitride ultra-thin substrate can be obtained. Example 2
[0046] S1. Use environmentally friendly plasticizer DOTP to modify ethyl cellulose, add 20% DOTP and 80% ethyl cellulose; stir in a reactor at 35-40°C for 6 hours to obtain low-viscosity modified ethyl cellulose;
[0047] S2. Add grinding balls to a planetary ball mill, the grinding balls are 3 times the weight ratio of silicon nitride powder, add 560g silicon nitride powder, 20gHo2O3, 40gMgF2, 4g oleic acid, 2gSolsperse 17000, add 219.6g anhydrous ethanol, 24.4g propylene glycol methyl ether, 130g modified ethyl cellulose, mix for 6 hours to form a slurry, the planetary mill revolution is 100rpm, the rotation is 200rpm;
[0048] S3. The silicon nitride slurry is subjected to degassing treatment at a vacuum negative pressure of 0.05~0.1MPa, a temperature of 35°C, and a treatment time of 10 hours. The viscosity is controlled at 20000~30000mPa·s. Tape casting is performed in sequence at four temperatures of 25°C, 30°C, 35°C, and 40°C, with a treatment time of 5 hours at each temperature, a casting speed of 0.05~0.1m / min, debinding at 500~550°C for 20 hours, and sintering at 1880~1930°C for 4.5 hours. The silicon nitride ultra-thin substrate can be obtained. Example 3
[0049] S1. Use environmentally friendly plasticizer DOTP to modify ethyl cellulose, add 25% DOTP and 75% ethyl cellulose; stir in a reactor at 35-40°C for 6 hours to obtain low-viscosity modified ethyl cellulose;
[0050] S2. Add grinding balls to a planetary ball mill, the grinding balls are 3 times the weight ratio of silicon nitride powder, add 560g silicon nitride powder, 20gHo2O3, 40gMgF2, 4g oleic acid, 2gSolsperse 17000, add 219.6g anhydrous ethanol, 24.4g propylene glycol methyl ether, 130g modified ethyl cellulose, mix for 6 hours to form a slurry, the planetary mill revolution is 150rpm, rotation is 300rpm;
[0051] S3. The silicon nitride slurry is subjected to degassing treatment at a vacuum negative pressure of 0.05~0.1MPa, a temperature of 35°C, and a treatment time of 10 hours. The viscosity is controlled at 20000~30000mPa·s. Tape casting is performed in sequence at four temperatures of 25°C, 30°C, 35°C, and 40°C, with a treatment time of 5 hours at each temperature, a casting speed of 0.05~0.1m / min, debinding at 500~550°C for 18 hours, and sintering at 1880~1930°C for 5 hours. The silicon nitride ultra-thin substrate can be obtained. Example 4
[0052] S1. Use environmentally friendly plasticizer DOTP to modify ethyl cellulose, add 23% DOTP and 77% ethyl cellulose; stir in a reactor at 35-40°C for 5 hours to obtain low-viscosity modified ethyl cellulose;
[0053] S2. Add grinding balls to a planetary ball mill, the grinding balls are 3 times the weight ratio of silicon nitride powder, add 560g silicon nitride powder, 20gHo2O3, 40gMgF2, 4g polyoxyethylene oleate, 2gSolsperse 17000, add 219.6g anhydrous ethanol, 24.4g propylene glycol methyl ether, 130g modified ethyl cellulose, mix for 6 hours to form a slurry, the planetary mill revolution is 150rpm, rotation is 300rpm;
[0054] S3. The silicon nitride slurry is subjected to degassing treatment at a vacuum negative pressure of 0.05~0.1MPa, a temperature of 35°C, and a treatment time of 10 hours. The viscosity is controlled at 20000~30000mPa·s. Tape casting is performed in sequence at four temperatures of 25°C, 30°C, 35°C, and 40°C, with a treatment time of 5 hours at each temperature, a casting speed of 0.05~0.1m / min, debinding at 500~550°C for 18 hours, and sintering at 1880~1930°C for 5 hours. The silicon nitride ultra-thin substrate can be obtained. Example 5
[0055] S1. Use environmentally friendly plasticizer DOTP to modify ethyl cellulose, add 23% DOTP and 77% ethyl cellulose; stir in a reactor at 35-40°C for 5 hours to obtain low-viscosity modified ethyl cellulose;
[0056] S2. Add grinding balls to a planetary ball mill, the grinding balls are 3 times the weight ratio of silicon nitride powder, add 560g silicon nitride powder, 20gHo2O3, 40gMgF2, 2g oleic acid, 2g oleic acid polyoxyethylene ester, 2gSolsperse 17000, add 219.6g anhydrous ethanol, 24.4g propylene glycol methyl ether, 130g modified ethyl cellulose, mix for 6 hours to form a slurry, the planetary mill revolution is 150rpm, rotation is 300rpm;
[0057] S3. The silicon nitride slurry is subjected to degassing treatment at a vacuum negative pressure of 0.05~0.1MPa, a temperature of 35°C, and a treatment time of 10 hours. The viscosity is controlled at 20000~30000mPa·s. Tape casting is performed in sequence at four temperatures of 25°C, 30°C, 35°C, and 40°C, with a treatment time of 5 hours at each temperature, a casting speed of 0.05~0.1m / min, debinding at 500~550°C for 18 hours, and sintering at 1880~1930°C for 5 hours. The silicon nitride ultra-thin substrate can be obtained. Example 6
[0058] S1. Use environmentally friendly plasticizer DOTP to modify ethyl cellulose, add 23% DOTP and 77% ethyl cellulose; stir in a reactor at 35-40°C for 5 hours to obtain low-viscosity modified ethyl cellulose;
[0059] S2. Add grinding balls to a planetary ball mill, the grinding balls are 3 times the weight ratio of silicon nitride powder, add 560g silicon nitride powder, 30gHo2O3, 30gMgF, 4g oleic acid, 2gSolsperse 17000, add 219.6g anhydrous ethanol, 24.4g propylene glycol methyl ether, 130g modified ethyl cellulose, mix for 6 hours to form a slurry, the planetary mill revolution is 70rpm, the rotation is 140rpm;
[0060] S3. The silicon nitride slurry is subjected to degassing treatment at a vacuum negative pressure of 0.05~0.1MPa, a temperature of 35°C, and a treatment time of 10 hours. The viscosity is controlled at 20000~30000mPa·s. Tape casting is performed in sequence at four temperatures of 25°C, 30°C, 35°C, and 40°C, with a treatment time of 5 hours at each temperature, a casting speed of 0.05~0.1m / min, debinding at 500~550°C for 24 hours, and sintering at 1880~1930°C for 5 hours. The silicon nitride ultra-thin substrate can be obtained.
[0061] The test results of the silicon nitride ultra-thin substrates prepared in Examples 1 to 6 are shown in Table 1 below.
[0062]
[0063] In each of Examples 1 to 6, 9 silicon nitride ultra-thin substrates were randomly selected for range calculation, as shown in Table 2 below.
[0064]
[0065] The pictures of silicon nitride ultra-thin substrate green ceramic and silicon nitride ultra-thin substrate prepared in Examples 1 to 5 are as follows: Figures 1 to 3 . Comparative Example 1
[0066] In step S3. of this embodiment, tape casting is performed at four temperatures of 25°C, 35°C, 48°C and 55°C for 5 hours, and the other steps are the same as those in Example 1. The surface quality of the green ceramic of the silicon nitride ultra-thin substrate obtained in this comparative example is poor overall, and some green ceramics have pits and small hidden cracks. The green ceramic of the silicon nitride ultra-thin substrate obtained is shown in the figure below. Figure 4 After firing, the ultra-thin silicon nitride substrate has a large thickness difference, with the highest point thickness of 0.341mm, the lowest point thickness of 0.315mm, and the thickness difference of 0.026mm.
[0067] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods. The specific embodiments described above further describe the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A tape casting method for a low-energy, low-VOC silicon nitride ultra-thin substrate, characterized in that: The following steps are involved: S1. The modifier and ethyl cellulose are modified to become modified ethyl cellulose; The modifier is dioctyl terephthalate; The modification operation is to stir in a reaction kettle at a temperature of 35-40° C. for 4-6 hours; The mass ratio of the ethyl cellulose to the modifier is 75-80:20-25; S2. The grinding balls, silicon nitride powder, mixed sintering aid, dispersant, solvent and modified ethyl cellulose are mixed and ball-milled to form a slurry; The dispersant is one or more of oleic acid, polyoxyethylene oleate, and Solsperse 17000; The mixed sintering aids are Ho2O3 and MgF2; The slurry comprises, by weight, 50 to 60 parts of silicon nitride powder, 5 to 7 parts of a mixed sintering aid, 0.1 to 0.6 parts of a dispersant, 15 to 24.4 parts of a solvent and 10 to 15 parts of modified ethyl cellulose; S3. The slurry is degassed, and tape-casting is performed at four temperatures of 23-27°C, 28-32°C, 33-37°C, and 38-42°C to obtain a silicon nitride ultra-thin substrate green ceramic, and then the low-energy and low-VOC silicon nitride ultra-thin substrate is obtained by debinding and sintering; The tape casting process is performed at each temperature for 4 to 6 hours.
2. The tape casting method for a low-energy, low-VOC silicon nitride ultra-thin substrate according to claim 1, characterized in that: The solvent is anhydrous ethanol and / or propylene glycol methyl ether.
3. The tape casting method for a low-energy, low-VOC silicon nitride ultra-thin substrate according to claim 1, characterized in that: The solvent is 15-21.96 parts of anhydrous ethanol and 0-9.24 parts of propylene glycol methyl ether; The dispersant is 0-0.4 parts of oleic acid, 0-0.4 parts of polyoxyethylene oleate and 0.1-0.3 parts of Solsperse 17000; The mixed sintering aid is 2-3 parts of Ho2O3 and 3-4 parts of MgF2.
4. The tape casting method for a low-energy, low-VOC silicon nitride ultra-thin substrate according to claim 1, characterized in that: The device used for the mixed ball milling is a planetary ball mill; The mixing ball milling time is 5 to 6 hours; The orbital speed in the mixing ball mill is 50-200 rpm, and the rotation speed is 100-400 rpm; The weight of the grinding balls is three times the weight of the silicon nitride powder.
5. The tape casting method for low-energy consumption and low-VOC silicon nitride ultra-thin substrate according to claim 1, characterized in that: The tape casting speed is 0.05-0.1 m / min.
6. The tape casting method for low-energy consumption and low-VOC silicon nitride ultra-thin substrate according to claim 1, characterized in that: The vacuum negative pressure of the degassing treatment is 0.05-0.1 MPa, the temperature of the degassing treatment is 35°C, and the time of the degassing treatment is 9-10 hours; The viscosity of the slurry after the degassing treatment is controlled at 20000-30000 mPa·s.
7. The tape casting method for low-energy consumption and low-VOC silicon nitride ultra-thin substrate according to claim 1, characterized in that: The debinding temperature is 500-550°C and the debinding time is 12-24h; The sintering temperature is 1880-1930° C., and the sintering time is 2-10 hours.
8. The tape casting method for low-energy consumption and low-VOC silicon nitride ultra-thin substrate according to claim 1, characterized in that: The solid content of the silicon nitride ultra-thin substrate is 63-65%; The average thickness of the silicon nitride ultra-thin substrate is 0.314-0.320 mm, the thickness tolerance is less than ±0.03 mm, and the thickness extreme difference is less than 0.017 mm.