A modified spherical silicon powder for copper clad laminate and preparation method thereof

Through carboxylation treatment and surface modification of silicon micropowder, the modified spherical silicon micropowder is formed, which solves the problem of deterioration of material density and dielectric properties caused by the interface effect of silicon micropowder in epoxy resin, and improves the mechanical and mediation of copper clad plates Electrical performance.

CN118460017BActive Publication Date: 2024-11-05广州豫顺新材料科技有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410583019.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-11
Publication Date
2024-11-05
Estimated Expiration
2044-05-11

AI Technical Summary

Technical Problem

The existing silicon micropowders produce interfacial effects in epoxy resins, resulting in a decrease in the density of the material and a decrease in dielectric properties.

Method used

Silicon powder is treated by carboxylation, and surface activation and modification is carried out using chemical substances such as DL-1-(1-naphthyl)ethylamine, N,N'-carbonyldiimidazole, p-formylphenylboric acid, etc. to form modified spherical silicon Micropowder improves its compatibility and bonding strength with epoxy resin.

Benefits of technology

The mechanical and dielectric properties of composite materials are improved, the water absorption and linear expansion rate are reduced, the heat resistance and conductivity of copper clad plates are improved, and the problem of poor dielectric properties is solved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GHA0000007258820000091
    Figure GHA0000007258820000091
  • Figure GHA0000007258820000101
    Figure GHA0000007258820000101
Patent Text Reader

Abstract

The present invention discloses a modified spherical silicon powder for copper-clad laminate and a preparation method thereof, and relates to the technical field of silicon powder materials. The present invention discloses a preparation method of modified spherical silicon powder for copper-clad laminate, comprising the following steps: S1: reacting carboxylated silicon powder with DL-1-(1-naphthyl)ethylamine to obtain component one; S2: brominating component one to obtain component two; S3: subjecting component two to a substitution reaction with p-formylphenylboronic acid to obtain component three; S4: carboxylating component three to obtain modified spherical silicon powder. The modified spherical silicon powder prepared in the present application is compounded with epoxy resin in the copper-clad laminate base material as a filler, effectively improving the dielectric properties and mechanical properties of the copper-clad laminate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon micropowder materials, and in particular to modified spherical silicon micropowder for copper-clad plates and a preparation method thereof. Background Art

[0002] With the advent of the information automation era, modern electronic products have developed rapidly. The integrated circuit industry has become a basic and strategic industry supporting social development. Copper clad laminates, as the main carrier in integrated circuits, serve as industrial basic materials on integrated circuits. Copper clad laminates are plate-shaped materials made by impregnating resins with different properties with reinforcing materials, adding different fillers (such as silicon powder), drying, and covering one or both sides with copper foil, and then hot pressing. With the emergence and vigorous promotion of integrated circuits, electronic products are gradually moving towards miniaturization, low energy consumption and safety. Printed circuit boards are constantly developing in the direction of multi-layer and high-density installation. The high reliability of copper clad laminates faces increasingly severe challenges. In order to reduce the cost of circuit boards and improve their mechanical properties, heat resistance, dispersion and conductivity, inorganic fillers such as silicon powder, talc, aluminum hydroxide, etc. are usually added to copper clad laminate substrates.

[0003] As a typical inorganic filler, silicon micropowder has the excellent characteristics of "three highs" (high insulation, high thermal conductivity, high thermal stability), "three lows" (low thermal expansion coefficient, low dielectric constant, low raw material cost) and "two resistances" (acid and alkali resistance, wear resistance). It is widely used in copper clad laminates and is the main inorganic filler in copper clad laminates. It improves the mechanical strength and thermal stability of printed circuit boards, prevents deformation and cracking of printed circuit boards, strengthens heat resistance and improves chemical resistance. Silicon micropowder is a polar, hydrophilic substance with a Mohs hardness of 7 and a melting point of 1750℃. Silicon micropowder has small particles, large specific surface area, and is mostly spherical or oval in shape. When silicon micropowder filler is dispersed in organic polymer resins with low polarity, its compatibility is poor, which affects the processing performance and quality of the material. With the addition of silicon micropowder, many micropores are introduced into the matrix, which reduces the density of the material and the insulation of the material. Moreover, the composite process of silicon micropowder and epoxy resin is prone to cause interface effect, attracting space charge and generating voids, which increases the dielectric constant of the composite material and reduces the dielectric properties of the material. Summary of the invention

[0004] The purpose of the present invention is to provide a modified spherical silicon powder for copper clad laminate and a preparation method thereof, so as to solve the following technical problems:

[0005] When the existing silicon micropowder is added to the epoxy resin, the epoxy resin and the silicon micropowder produce an interface effect, and the density of the material decreases, and the dielectric properties of the material decrease.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing modified spherical silicon powder for copper clad laminates comprises the following steps:

[0008] S1: Add carboxylated silicon powder, N,N-dimethylformamide, DL-1-(1-naphthyl)ethylamine and N,N'-carbonyldiimidazole into reactor A and disperse them evenly. Control the temperature to 80-90°C, keep the temperature for 24-48 hours, centrifuge, wash and dry to obtain component 1.

[0009] S2: Add component 1 and tetrachloromethane to reactor B and disperse evenly, add liquid bromine, react at room temperature in the dark for 24-36 hours, filter, wash and dry to obtain component 2;

[0010] S3: In a nitrogen atmosphere, component 2, p-formylphenylboronic acid, potassium carbonate, and 1,4-dioxane are added to reaction kettle C and dispersed evenly, deionized water and tetrakis(triphenylphosphine)palladium are added, the temperature is controlled at 70-80°C, the reaction is kept warm for 24-48 hours, and filtered and chromatographed to obtain component 3;

[0011] S4: In a nitrogen atmosphere, component three, cyanoacetic acid and tetrahydrofuran are added into reactor D and dispersed evenly, piperidine is added and dispersed evenly, the temperature is controlled to reflux for reaction for 9-12 hours, filtered, washed and dried to obtain modified spherical silicon powder.

[0012] As a further solution of the present invention: the addition ratio of carboxylated silicon powder, N,N-dimethylformamide, DL-1-(1-naphthyl)ethylamine and N,N'-carbonyldiimidazole in S1 is 10g:100-200mL:2-5g:2-5g.

[0013] As a further solution of the present invention: the addition ratio of component 1, tetrachloromethane and liquid bromine in S2 is 10g:100-200mL:0.5-2g.

[0014] As a further scheme of the present invention: the addition ratio of component 2, p-formylphenylboric acid, potassium carbonate, 1,4-dioxane, deionized water, and tetrakis(triphenylphosphine)palladium in S3 is 1g: 0.05-0.15g: 0.2-0.4g: 10-20mL: 0.3-1mL: 0.01-0.02g.

[0015] As a further embodiment of the present invention: the addition ratio of component three, cyanoacetic acid, tetrahydrofuran and piperidine in S4 is 10 g: 1-1.5 g: 100-200 mL: 1-1.5 mL.

[0016] As a further scheme of the present invention: the preparation method of carboxylated silicon micropowder comprises the following steps: adding γ-aminopropyltriethoxysilane, succinic anhydride and N,N-dimethylformamide into a reaction kettle and dispersing them evenly, adding silicon micropowder and deionized water and dispersing them evenly, controlling the temperature at 60-80°C, keeping warm and stirring for 3-6 hours, washing and drying to obtain carboxylated silicon micropowder.

[0017] As a further solution of the present invention: the addition ratio of γ-aminopropyltriethoxysilane, succinic anhydride, N,N-dimethylformamide, silicon micropowder and deionized water is 0.2-0.5g: 0.1-0.2g: 50-200mL: 10g: 5-10mL.

[0018] A modified spherical silicon powder for copper-clad laminates is prepared by any one of the above-mentioned preparation methods.

[0019] Beneficial effects of the present invention:

[0020] The present application utilizes succinic anhydride and γ-aminopropyltriethoxysilane to undergo a ring-opening reaction, grafts a carboxyl group onto a silane coupling agent, and utilizes the hydrolyzable group of γ-aminopropyltriethoxysilane to hydrolyze to generate silanol, which reacts with the surface hydroxyl group of silicon micropowder to form siloxane, thereby obtaining carboxylated silicon micropowder. This step realizes the surface organic treatment of silicon micropowder, improves the dispersibility of silicon micropowder in the resin system, improves the compatibility between silicon micropowder and resin, and improves the mechanical properties and mechanical properties of the composite material. The present invention uses N,N'-carbonyldiimidazole as an activator to activate the carboxyl groups on the surface of carboxylated silicon micropowder, and then uses the amino group of DL-1-(1-naphthyl)ethylamine to react with the carboxyl groups on the surface of silicon micropowder to undergo an amide reaction, and grafts a naphthalene aromatic ring on the surface of the silicon micropowder to obtain component one; the component one is mixed with liquid bromine for reaction, and halogenated on the naphthalene aromatic ring to obtain component two; and component two and p-formylphenylboric acid are used as raw materials, and tetrakis(triphenylphosphine)palladium is used as a catalyst to obtain component three through a Suzuki coupling reaction; finally, the aldehyde groups on the surface of component three and cyanoacetic acid are reacted with piperidine through a Knoevenage l condensation reaction to obtain modified spherical silicon micropowder.

[0021] When the silicon powder prepared by the present application is mixed with the epoxy resin of the copper-clad laminate base material, the carboxyl group contained on the surface of the silicon powder reacts with the epoxy group of the epoxy resin to form a ring-opening reaction, and the silicon powder is organically connected to the epoxy resin through a molecular chain, thereby improving the interface compatibility of the two materials, thereby improving the comprehensive performance of the composite material and increasing the bonding strength. Moreover, with the cross-linking of silicon powder and epoxy resin, the introduction of naphthalene aromatic rings in the epoxy resin structure molecule not only improves the heat resistance of the epoxy resin, but also the introduction of naphthalene molecular structure in the epoxy resin system can reduce the linear expansion rate of the epoxy resin; more non-absorbent structural units and more hydrophobic hydroxyl structures are introduced into the epoxy resin, and the water absorption rate of the epoxy resin system can be reduced; the silicon powder prepared by the present application is added in the copper-clad laminate base material and organically combined with the epoxy resin, effectively solving the defects of poor moisture and heat resistance of ordinary epoxy resin and high linear expansion coefficient.

[0022] The silicon micropowder prepared in the present application is added as a filler in the epoxy resin of the copper clad laminate. The silicon micropowder not only has groups and organic molecular chains that occupy a large space volume, but also introduces double bond compounds to improve the dielectric properties of the epoxy resin, giving the copper clad laminate a small and stable dielectric constant (Dk) and dielectric loss (Df), effectively solving the poor dielectric properties of the epoxy resin and the problem that general epoxy resins are not suitable for rapid transmission of signals under high frequency and high speed conditions, thereby improving the integrity of signal transmission in the medium. DETAILED DESCRIPTION

[0023] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Embodiment 1 A method for preparing modified spherical silicon powder for copper clad laminate comprises the following steps:

[0025] S1: Add 0.5g of γ-aminopropyltriethoxysilane, 0.2g of succinic anhydride, and 100mL of N,N-dimethylformamide into the reaction kettle and disperse them evenly, add 10g of silicon micropowder and 10mL of deionized water and disperse them evenly, control the temperature to 80°C, keep warm and stir for 3h, wash and dry to obtain carboxylated silicon micropowder;

[0026] S2: 10 g of carboxylated silicon powder, 100 mL of N,N-dimethylformamide, 2 g of DL-1-(1-naphthyl)ethylamine, and 2 g of N,N'-carbonyldiimidazole were added to reactor A and dispersed evenly. The temperature was controlled at 80°C and kept warm for 24 h. The mixture was centrifuged, washed, and dried to obtain component 1.

[0027] S3: Add 10g of component 1 and 100mL of tetrachloromethane into reactor B and disperse evenly, add 0.5g of liquid bromine, react at room temperature for 24h in the dark, filter, wash and dry to obtain component 2;

[0028] S4: In a nitrogen atmosphere, 10 g of component 2, 0.5 g of p-formylphenylboronic acid, 2 g of potassium carbonate, and 100 mL of 1,4-dioxane were added to reactor C and dispersed evenly, 3 mL of deionized water and 0.1 g of tetrakis(triphenylphosphine)palladium were added, the temperature was controlled at 70°C, the reaction was kept warm for 24 h, and component 3 was obtained by filtration and chromatography;

[0029] S5: In a nitrogen atmosphere, 10 g of component three, 1.5 g of cyanoacetic acid, and 200 mL of tetrahydrofuran were added to reactor D and dispersed evenly, and 1.5 mL of piperidine was added and dispersed evenly. The temperature was controlled to reflux for 12 h, and the reaction was filtered, washed, and dried to obtain modified spherical silicon powder.

[0030] Embodiment 2 A method for preparing modified spherical silicon powder for copper clad laminate comprises the following steps:

[0031] S1: Add 0.5g of γ-aminopropyltriethoxysilane, 0.2g of succinic anhydride, and 100mL of N,N-dimethylformamide into the reaction kettle and disperse them evenly, add 10g of silicon micropowder and 10mL of deionized water and disperse them evenly, control the temperature to 80°C, keep warm and stir for 3h, wash and dry to obtain carboxylated silicon micropowder;

[0032] S2: 10 g of carboxylated silicon powder, 150 mL of N,N-dimethylformamide, 3.5 g of DL-1-(1-naphthyl)ethylamine, and 3.4 g of N,N'-carbonyldiimidazole were added to reactor A and dispersed evenly. The temperature was controlled at 85°C and kept warm for 36 h. The mixture was centrifuged, washed, and dried to obtain component 1.

[0033] S3: Add 10g of component 1 and 150mL of tetrachloromethane into reactor B and disperse evenly, add 1.2g of liquid bromine, react at room temperature for 30h in the dark, filter, wash and dry to obtain component 2;

[0034] S4: In a nitrogen atmosphere, 10 g of component 2, 1 g of p-formylphenylboronic acid, 3 g of potassium carbonate, and 150 mL of 1,4-dioxane were added to reactor C and dispersed evenly, 6 mL of deionized water and 0.15 g of tetrakis(triphenylphosphine)palladium were added, the temperature was controlled at 75°C, the reaction was kept warm for 36 hours, and then filtered and chromatographed to obtain component 3;

[0035] S5: In a nitrogen atmosphere, 10 g of component three, 1.2 g of cyanoacetic acid, and 150 mL of tetrahydrofuran were added to reactor D and dispersed evenly, and 1.2 mL of piperidine was added and dispersed evenly. The temperature was controlled to reflux for 9 h, and the modified spherical silica powder was obtained by filtering, washing, and drying.

[0036] Embodiment 3 A method for preparing modified spherical silicon powder for copper clad laminate comprises the following steps:

[0037] S1: Add 0.5g of γ-aminopropyltriethoxysilane, 0.2g of succinic anhydride, and 100mL of N,N-dimethylformamide into the reaction kettle and disperse them evenly, add 10g of silicon micropowder and 10mL of deionized water and disperse them evenly, control the temperature to 80°C, keep warm and stir for 3h, wash and dry to obtain carboxylated silicon micropowder;

[0038] S2: 10 g of carboxylated silicon powder, 200 mL of N,N-dimethylformamide, 5 g of DL-1-(1-naphthyl)ethylamine, and 5 g of N,N'-carbonyldiimidazole were added to reactor A and dispersed evenly. The temperature was controlled at 90°C and kept warm for 48 hours. The mixture was centrifuged, washed, and dried to obtain component 1.

[0039] S3: Add 10g of component 1 and 200mL of tetrachloromethane into reactor B and disperse evenly, add 2g of liquid bromine, react at room temperature for 36h in the dark, filter, wash and dry to obtain component 2;

[0040] S4: In a nitrogen atmosphere, 10 g of component 2, 1.5 g of p-formylphenylboronic acid, 4 g of potassium carbonate, and 200 mL of 1,4-dioxane were added to reactor C and dispersed evenly, and 10 mL of deionized water and 0.2 g of tetrakis(triphenylphosphine)palladium were added. The temperature was controlled at 80°C, and the reaction was kept warm for 48 hours. Filtering and chromatography were performed to obtain component 3;

[0041] S5: In a nitrogen atmosphere, 10 g of component three, 1.5 g of cyanoacetic acid, and 200 mL of tetrahydrofuran were added to reactor D and dispersed evenly, and 1.5 mL of piperidine was added and dispersed evenly. The temperature was controlled to reflux for 12 h, and the reaction was filtered, washed, and dried to obtain modified spherical silicon powder.

[0042] Embodiment 4 The preparation method of copper clad laminate comprises the following steps:

[0043] a: Preparation of glue: 25 g of tetrabromobisphenol A epoxy resin (Changchun resin) and 7.5 g of the silicon powder prepared in Example 1 were added into a reaction kettle, the temperature was controlled at 120-150° C., and the mixture was obtained by stirring while keeping warm;

[0044] b: Add 0.25g of curing agent (dicyandiamide) and N,N-dimethylformamide to the reaction bottle, stir until completely dissolved, add to the mixture and disperse evenly, add 0.4g of accelerator (dimethylimidazole) and disperse evenly to obtain glue (resin content 50%);

[0045] c: Gluing: The above glue solution is glued with electronic grade 7628 glass fiber cloth, and the gap between the clamping shafts is set to 0.35 mm. After gluing the glass cloth, it is first left to air at room temperature, and then baked in an oven at 170°C for 8 minutes to obtain a prepreg;

[0046] d: Lamination: The aluminum plate / semi-cured sheet / copper foil are stacked and placed on a hot oil test small press for vacuum lamination. The pressing procedure is: control the heating rate to 7℃ / min, heat to 130℃, and press at a pressure of 100bar for 30min; control the heating rate to 7℃ / min, heat to 150℃, and press at a pressure of 125bar for 30min; control the heating rate to 7℃ / min, heat to 210℃, and press at a pressure of 180bar for 120min; obtain the copper clad laminate.

[0047] Example 5 Compared with Example 4, Example 5 only replaces an equal amount of the silicon micropowder prepared in Example 1 added in Example 4 with the silicon micropowder prepared in Example 2, and the other components and preparation methods are exactly the same as those in Example 4.

[0048] Example 6 Compared with Example 4, Example 6 only replaces an equal amount of the silicon micropowder prepared in Example 1 added in Example 4 with the silicon micropowder prepared in Example 3, and the other components and preparation methods are exactly the same as those in Example 4.

[0049] Comparative Example 1 A method for preparing modified spherical silicon micropowder for copper clad laminates comprises the following steps: adding 0.5 g of γ-aminopropyltriethoxysilane, 0.2 g of succinic anhydride, and 100 mL of N,N-dimethylformamide into a reaction kettle and dispersing them evenly, adding 10 g of silicon micropowder and 10 mL of deionized water and dispersing them evenly, controlling the temperature to 80°C, keeping the mixture warm and stirring for 3 hours, washing, and drying to obtain modified spherical silicon micropowder.

[0050] Comparative Example 2 A method for preparing modified spherical silicon powder for copper clad laminate comprises the following steps:

[0051] S1: Add 0.5g of γ-aminopropyltriethoxysilane, 0.2g of succinic anhydride, and 100mL of N,N-dimethylformamide into the reaction kettle and disperse them evenly, add 10g of silicon micropowder and 10mL of deionized water and disperse them evenly, control the temperature to 80°C, keep warm and stir for 3h, wash and dry to obtain carboxylated silicon micropowder;

[0052] S2: Add 10 g of carboxylated silicon micropowder, 150 mL of N,N-dimethylformamide, 3.5 g of DL-1-(1-naphthyl)ethylamine, and 3.4 g of N,N'-carbonyldiimidazole into reactor A and disperse them evenly. Control the temperature at 85°C and keep it warm for 36 hours. Centrifuge, wash, and dry to obtain modified spherical silicon micropowder.

[0053] Comparative Example 3 A method for preparing modified spherical silicon powder for copper clad laminate comprises the following steps:

[0054] S1: Add 0.5g of γ-aminopropyltriethoxysilane, 0.2g of succinic anhydride, and 100mL of N,N-dimethylformamide into the reaction kettle and disperse them evenly, add 10g of silicon micropowder and 10mL of deionized water and disperse them evenly, control the temperature to 80°C, keep warm and stir for 3h, wash and dry to obtain carboxylated silicon micropowder;

[0055] S2: 10 g of carboxylated silicon powder, 150 mL of N,N-dimethylformamide, 3.5 g of DL-1-(1-naphthyl)ethylamine, and 3.4 g of N,N'-carbonyldiimidazole were added to reactor A and dispersed evenly. The temperature was controlled at 85°C and kept warm for 36 h. The mixture was centrifuged, washed, and dried to obtain component 1.

[0056] S3: Add 10g of component 1 and 150mL of tetrachloromethane into reactor B and disperse evenly, add 1.2g of liquid bromine, react at room temperature for 30h in the dark, filter, wash and dry to obtain component 2;

[0057] S4: In a nitrogen atmosphere, 10 g of component 2, 1 g of p-formylphenylboric acid, 3 g of potassium carbonate, and 150 mL of 1,4-dioxane were added to reactor C and dispersed evenly. 6 mL of deionized water and 0.15 g of tetrakis(triphenylphosphine)palladium were added. The temperature was controlled at 75°C, and the reaction was kept warm for 36 hours. The mixture was filtered and chromatographed to obtain modified spherical silica powder.

[0058] Comparative Example 4 Compared with Example 4, only the silicon micropowder prepared in Example 1 added in Example 4 is replaced by the silicon micropowder prepared in Comparative Example 1 in an equal amount, and the other components and preparation method are exactly the same as those in Example 4.

[0059] Comparative Example 5 Compared with Example 4, only the silicon micropowder prepared in Example 1 added in Example 4 is replaced by the silicon micropowder prepared in Comparative Example 2 in an equal amount, and the other components and preparation method are exactly the same as those in Example 4.

[0060] Comparative Example 6 Compared with Example 4, Example 6 only replaces an equal amount of the silicon micropowder prepared in Example 1 added in Example 4 with the silicon micropowder prepared in Comparative Example 3, and the remaining components and preparation method are exactly the same as those in Example 4.

[0061] Performance Testing

[0062] (1) Dielectric properties: The dielectric constant (Dk) and dielectric loss (Df) of the test specimens were tested according to IPC-TM-6502.5.5.9. The test was performed using the E4491 A impedance analyzer from Keysight Technologies. The test conditions were: 25°C, operating frequency 10 GHz, test size 50 mm × 50 mm × 1.6 mm. The dielectric constant and dielectric loss were tested. The test results are shown in Table 1.

[0063] (2) Peel strength: The peel strength of the sample was tested according to IPC-TM-6502.4.8. The peel strength tester was used to record the minimum value during the peeling process when the length was not less than 25 mm. The minimum load required per unit width was taken as the peel strength. The test results are shown in Table 1.

[0064] (3) Water absorption: The water absorption of the sample was tested according to IPC-TM-6502.6.2.1. During the test, the CCL copper clad laminate was immersed in distilled water for 24 hours. The test results are shown in Table 1.

[0065] Table 1: Statistical table of performance test data of Examples 4-6 and Comparative Examples 4-6

[0066]

[0067] As shown in Table 1, the silicon powder prepared in this application is used in combination with epoxy resin to prepare copper clad laminate glue, which gives the copper clad laminate low dielectric loss and low dielectric constant, and has good dielectric properties. In addition, it has good bonding effect and low water absorption, and during use, it gives the material stable physical and chemical properties.

[0068] (4) Thermal expansion coefficient: The thermal expansion coefficient of the sample was tested according to IPC-TM-6502.4.24 using a TMA instrument. The test results are shown in Table 2.

[0069] (5) High-pressure cooking test: The high-pressure cooking resistance of the sample was tested according to IPC-TM-6502.6.16. The sample size was 100 mm × 100 mm × 1.6 mm. The test conditions were: 260°C, cooking for 180 min in a pressure cooker, and a pressure of 105±3 KPa. After the sample was cooled, it was placed in a tin furnace (288°C, 10 s) to test the heat resistance limit time. The test results are shown in Table 2.

[0070] (6) Heat resistance limit (thermal stress): According to IPC-TM-6502.4.13.1, the thermal stress of the sample is tested, with tinning for 10S+1 / -0 and cooling at room temperature for 10S+1 / -0 as one test cycle, and the number of limit cycles is examined. The test results are shown in Table 2;

[0071] (7) Thermal conductivity: Refer to ASTM D5470-2006 and use DRL-3 thermal conductivity tester for testing. The test results are shown in Table 2.

[0072] Table 2: Statistical table of heat resistance test data of Examples 4-6 and Comparative Examples 4-6

[0073]

[0074] As can be seen from Table 2, the silicon micropowder prepared in the present application is added to the epoxy resin to prepare the glue. Due to the high compatibility and strong bonding between the silicon micropowder and the epoxy resin, the heat resistance of the material is greatly improved; and the material is given the advantages of low thermal expansion coefficient and high thermal conductivity.

[0075] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing modified spherical silicon powder for copper clad laminate, characterized in that: The steps include: S1: Add carboxylated silicon powder, N,N-dimethylformamide, DL-1-(1-naphthyl)ethylamine and N,N'-carbonyldiimidazole into reactor A and disperse them evenly. Control the temperature to 80-90°C, keep the temperature for 24-48 hours, centrifuge, wash and dry to obtain component 1. S2: Add component 1 and tetrachloromethane to reactor B and disperse evenly, add liquid bromine, react at room temperature in the dark for 24-36 hours, filter, wash and dry to obtain component 2; S3: In a nitrogen atmosphere, component 2, p-formylphenylboronic acid, potassium carbonate, and 1,4-dioxane are added to reaction kettle C and dispersed evenly, deionized water and tetrakis(triphenylphosphine)palladium are added, the temperature is controlled at 70-80°C, the reaction is kept warm for 24-48 hours, and filtered and chromatographed to obtain component 3; S4: In a nitrogen atmosphere, component three, cyanoacetic acid, and tetrahydrofuran are added to the reaction kettle D and dispersed evenly, piperidine is added and dispersed evenly, the temperature is controlled to reflux for 9-12 hours, filtered, washed, and dried to obtain modified spherical silicon powder; The addition ratio of carboxylated silicon powder, N,N-dimethylformamide, DL-1-(1-naphthyl)ethylamine, and N,N'-carbonyldiimidazole in S1 is 10 g: 100-200 mL: 2-5 g: 2-5 g; The addition ratio of component 1, tetrachloromethane, and liquid bromine in S2 is 10g:100-200mL:0.5-2g; The addition ratio of component 2, p-formylphenylboric acid, potassium carbonate, 1,4-dioxane, deionized water, and tetrakis(triphenylphosphine)palladium in S3 is 1 g: 0.05-0.15 g: 0.2-0.4 g: 10-20 mL: 0.3-1 mL: 0.01-0.02 g; The addition ratio of component three, cyanoacetic acid, tetrahydrofuran, and piperidine in S4 is 10 g: 1-1.5 g: 100-200 mL: 1-1.5 mL; The preparation method of carboxylated silicon micropowder comprises the following steps: adding γ-aminopropyltriethoxysilane, succinic anhydride and N,N-dimethylformamide into a reaction kettle and dispersing them uniformly, adding silicon micropowder and deionized water and dispersing them uniformly, controlling the temperature at 60-80° C., keeping the temperature and stirring for 3-6 hours, washing and drying to obtain carboxylated silicon micropowder; The addition ratio of γ-aminopropyltriethoxysilane, succinic anhydride, N,N-dimethylformamide, silicon micropowder and deionized water is 0.2-0.5g: 0.1-0.2g: 50-200mL: 10g: 5-10mL.

2. A modified spherical silicon powder for copper clad laminate, characterized in that: Prepared by the preparation method described in claim 1.