A high-temperature solid acid impregnated NiO / YSZ composite electrolyte membrane and a preparation method thereof, and a preparation method of a solid acid fuel cell
The preparation of NiO/YSZ composite electrolyte membranes through high-temperature impregnation method solves the problem of insufficient proton conductivity and thermal stability of solid acid fuel cells under high temperature conditions, and achieves higher conductivity and mechanical strength, which is suitable for industrial production.
Patent Information
- Application Number
- CN202410933334.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The existing solid acid fuel cells have problems with insufficient proton conductivity and thermal stability under high temperature conditions, and the hydration characteristics of traditional electrolyte membrane materials affect their conductivity at operating temperature.
NiO/YSZ composite electrolyte membrane was prepared by high-temperature impregnation method, porous oxide membrane was prepared by casting method, and solid acid solution was immersed into the membrane at high temperature, combining nickel oxide and YSZ materials to improve proton conductivity and thermal stability .
It significantly improves the temperature range of proton conductivity and the thermal stability of the material, enhances the mechanical strength, and provides a medium-temperature fuel cell composite electrolyte membrane preparation method with low production cost and simple process, suitable for industrial production.
Smart Images

Figure CN118472335B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of proton conductor fuel cells, and more specifically, to a NiO / YSZ composite electrolyte membrane impregnated with solid acid at high temperature, a preparation method thereof, and a preparation method of a solid acid fuel cell. More specifically, the present invention relates to a preparation method of a proton conductor composite electrolyte membrane material by immersing a prepared NiO / YSZ membrane material in a solid acid solution using a high temperature impregnation method. Background Art
[0002] A fuel cell is a device that converts the chemical energy of a fuel directly into electrical energy. Fuel cells have the advantages of high efficiency, no pollution, and light weight. Fuel cells can not only convert the chemical energy of a fuel into electrical energy, but also realize the process of converting electrical energy into certain gaseous fuels. For example, hydrogen and ammonia are ideal energy storage materials. Their use and synthesis in proton conductor solid oxide electrochemical devices can achieve efficient and clean power generation and energy storage. Solid acid is a class of inorganic compounds that undergo superproton phase transition at high temperatures and have good proton conductivity. It has good proton conductivity and phase transition characteristics. Solid acid fuel cells (SAFCs) have the properties of low methanol permeability, high electrode catalytic activity, and resistance to carbon monoxide poisoning. As a research direction in the field of fuel cells, they have good development prospects. Solid acid has become an electrolyte material for fuel cells due to its high proton conductivity and stability between 100℃ and 250℃.
[0003] Solid acids have been widely studied due to their high proton conductivity and high-temperature phase change behavior. However, most solid acids are not considered as electrolyte membranes for fuel cells because of their water solubility and high-temperature ductility. In 2001, Haile and his colleagues at the California Institute of Technology first used solid acid CsHSO4 in fuel cells. They used CsHSO4 as an electrolyte membrane to assemble a hydrogen-oxygen fuel cell. The operating temperature of the battery was 150~160℃, and the open circuit voltage reached 1.11V. Since the operating temperature of the battery exceeded 100℃, it was proved that the performance of solid acid electrolytes would not be affected by the humidity of the working environment, thus proving the possibility of solid acids as electrolyte materials. Ponomareva studied the performance of CsHSO4 and CsH2PO4 / SiO2 composite electrolytes and found that by doping with different types of SiO2, the conductivity of CsH2PO4 could be increased to 10 at 130~250℃. -3 ~10 -2S / cm. Otomo et al. studied the conductivity of CsHSO4 / SiO2 composite membranes. By impregnating CsHSO4 solution into microporous SiO2 membranes, the proton conductivity of CsHSO4 / SiO2 composite membranes can be increased by 2 orders of magnitude compared with pure CsHSO4 at a temperature below the superproton conductor phase transition temperature of 60-140°C. Boysen et al. prepared composite membranes by combining CsHSO4 and thermoplastic polymer PVDF. The results showed that the highest conductivity was obtained when the PVDF volume fraction was 20% at 100°C. Yang et al. also prepared CsHSO4 / PVDF composite membranes. The results showed that the composite membranes were suitable for fuel cells, but the stability was poor. Replacing SO4 with PO4 can improve the stability of the composite membranes. Kim et al. studied the performance of ionic liquid-doped CsHSO4 composite membranes. The results showed that ionic liquid / CsHSO4 composite membranes had high conductivity at 80-180°C, reaching (1~2) 10 -3 S / cm. In the medium temperature range, the ion transport mechanism in solid electrolytes is similar to that in liquids.
[0004] Since solid acid materials have a reversible dehydration process, the gas needs to be humidified before being passed into the electrode side of the fuel cell to ensure the stability of the battery under operating temperature conditions. Relevant researchers have measured the superproton phase transition temperature of the material under different humidity and pressure gas atmospheres. Increasing the ambient humidity and gas pressure can reduce the temperature of the proton phase transition, thereby improving the material's high conductivity temperature range and thermal stability. By impregnating the solid acid material into the oxide material and using the porous oxide material as the supporting structure, the thermal stability of the material is improved and the temperature range of the conductivity is increased. Since the structure of the material affects the hydration characteristics of the solid acid material, it will affect the conductivity of the composite material at the operating temperature. Summary of the invention
[0005] According to the technical problems raised above, a NiO / YSZ composite electrolyte membrane impregnated with solid acid at high temperature and a preparation method thereof as well as a preparation method of a solid acid fuel cell are provided. The present invention adopts a method of high temperature impregnation of porous oxide materials, prepares a composite oxide membrane material by a tape casting method, removes carbon-based materials by high temperature calcination to prepare a porous oxide membrane material, and prepares an inorganic composite electrolyte membrane by high temperature impregnation of a solid acid solution, and a solid acid with high proton conductivity and a nickel oxide and YSZ composite material with thermal stability and mechanical strength.
[0006] The technical means adopted by the present invention are as follows:
[0007] A method for preparing a NiO / YSZ composite electrolyte membrane impregnated with solid acid at high temperature comprises the following steps: preparing slurry, ball milling, degassing, casting, calcining, and drying. Specifically, the method comprises the following steps:
[0008] Yttria-stabilized zirconium oxide powder, nickel oxide, a pore former, a dispersant, a binder, and water are prepared into a slurry;
[0009] After ball milling and drying the slurry to remove air, the prepared slurry is cast into a NiO / YSZ film material in a mold;
[0010] The NiO / YSZ porous membrane material is prepared by sintering the cast NiO / YSZ membrane material at a high temperature;
[0011] Preparation of solid acid solution: reacting metal salt and acid in a certain molar ratio to prepare solid acid material;
[0012] The prepared porous membrane material is immersed in a solid acid solution at a preset high temperature;
[0013] The immersion is repeated for a certain number of times, and vacuum drying is performed after the immersion is completed to obtain a NiO / YSZ composite electrolyte membrane material.
[0014] Furthermore, the slurry is calculated by mass ratio, and the proportions of yttria-stabilized zirconia powder, nickel oxide, pore-forming agent, dispersant, and binder are 34.9~38.8%, 11.6~19.4%, 14.1~17.4%, 1.7~2.4%, 4.7~5.8%, and the rest is water.
[0015] Furthermore, the specific steps of preparing the slurry are as follows: preparing the slurry by mixing NiO and YSZ powders with a pore former in distilled water and a dispersant, stirring the mixture for a period of time, adding a binder to the slurry, and then stirring for another 9 to 12 hours.
[0016] Furthermore, the mass ranges of yttria-stabilized zirconia, nickel oxide, dispersant, adhesive, graphite or starch used to prepare the NiO / YSZ membrane material are 30~40g, 10~20g, 10.5~14.5g, 1.5~2.5g, and 4~6g.
[0017] Furthermore, the prepared slurry is cast into a NiO / YSZ film material in a mold by evacuating the slurry, forming it on a casting machine, and then demolding it, and the thickness of the ceramic sheet is 0.4-0.6 mm.
[0018] Furthermore, the preparation of NiO / YSZ porous membrane material is specifically as follows: high temperature sintering is programmed temperature firing. When the NiO / YSZ film is programmed temperature fired, the heating rate from room temperature to 400±10°C is 1~2°C / min. After being kept constant at 400±10°C for 2±0.5h, the heating rate from 400±10°C to 1300~1600°C is 1~3°C / min. After being kept constant at 1300~1600°C for 4±0.5h, the temperature is finally dropped to room temperature at a rate of 1~2°C / min.
[0019] Furthermore, the sintered NiO / YSZ film is immersed in a solid acid solution at 150-200° C. for 4-6 hours.
[0020] Furthermore, the solid acid is MH x One or more combinations of XO4, wherein M is Cs, Rb, K or NH4, and X is S or P. x Correspondence is based on specific elements.
[0021] Furthermore, the molar ratio of nickel oxide, yttria-stabilized zirconium oxide, and solid acid material is used to calculate the content of the solid acid material in the composite material based on the actual weighed mass.
[0022] The present invention also claims to protect the NiO / YSZ composite electrolyte membrane impregnated with solid acid at high temperature prepared based on the above method.
[0023] The present invention also discloses a method for preparing a solid acid fuel cell based on the NiO / YSZ composite electrolyte membrane impregnated with solid acid at high temperature, comprising:
[0024] The Pt / C sheet and the impregnated composite electrolyte film were stacked and maintained at a constant temperature and pressure of 80±5° C. and 15±1 MPa for 30±5 min to prepare a solid acid fuel cell.
[0025] Compared with the prior art, the present invention has the following advantages:
[0026] 1. The tape casting process is simple, low-cost, pollution-free, and by changing the content of the pore-forming agent in the slurry, the porosity of the material can be adjusted, further increasing the doping amount of the solid acid material;
[0027] 2. Compared with pure solid acid electrolyte, the inorganic composite electrolyte membrane not only improves the temperature range of proton conductivity, but also improves the thermal stability and mechanical strength of the material;
[0028] 3. The present invention provides a method for preparing a medium-temperature fuel cell composite electrolyte membrane with low production cost, simple process and strong operability, which can be suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0030] Figure 1The graphs show the relationship between the conductivity and temperature of electrolyte materials with three different solid acid material doping amounts in Examples 1-3.
[0031] Figure 2 It shows Example 4, and the figure shows the voltage and power density change curve of a battery prepared with an electrolyte material with a doping amount of 30% and a Pt / C electrode under a water partial pressure of 0.3atm. DETAILED DESCRIPTION
[0032] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention.
[0033] A method for preparing a NiO / YSZ composite electrolyte membrane impregnated with solid acid at high temperature comprises the following steps: preparing slurry, ball milling, degassing, casting, calcining, and drying. Specifically, the method comprises the following steps:
[0034] Yttria-stabilized zirconium oxide powder, nickel oxide, a pore former, a dispersant, a binder, and water are prepared into a slurry;
[0035] Calculated by mass ratio, the slurry includes yttria-stabilized zirconia powder, nickel oxide, pore-forming agent, dispersant, and binder in proportions of 34.9~38.8%, 11.6~19.4%, 14.1~17.4%, 1.7~2.4%, 4.7~5.8%, and the rest is water, specifically 34.9~38.8%.
[0036] Further, as a specific implementation manner, the mass range of yttria-stabilized zirconia, nickel oxide, dispersant, adhesive, graphite or starch used to prepare NiO / YSZ film material is 30~40g, 10~20g, 10.5~14.5g, 1.5~2.5g, 4~6g.
[0037] The specific steps of preparing the slurry are as follows: preparing the slurry by mixing NiO and YSZ powders with a pore former in distilled water and a dispersant, stirring the mixture for a period of time, adding a binder to the slurry, and then stirring for another 9 to 12 hours. In this embodiment, the standing time is about one day, i.e., 24±5h.
[0038] After ball milling and drying the slurry to remove air, the prepared slurry is cast into a NiO / YSZ film material in a mold;
[0039] Furthermore, the prepared slurry is cast into a NiO / YSZ film material in a mold by evacuating the slurry, forming it on a casting machine, and then demolding it, and the thickness of the ceramic sheet is 0.4-0.6 mm.
[0040] The NiO / YSZ porous membrane material is prepared by sintering the cast NiO / YSZ membrane material at a high temperature;
[0041] Furthermore, the preparation of NiO / YSZ porous membrane material is specifically as follows: high temperature sintering is programmed temperature firing. When the NiO / YSZ film is programmed temperature fired, the heating rate from room temperature to 400°C is 1~2°C / min. After maintaining the temperature at 400°C for 2h, the heating rate from 400°C to 1300~1600°C is 1~3°C / min. The temperature is maintained at 1300~1600°C for 4h, and finally the temperature is dropped to room temperature at a rate of 1~2°C / min.
[0042] Preparation of solid acid solution: reacting metal salt and acid in a certain molar ratio to prepare solid acid material;
[0043] Furthermore, the solid acid is MH x One or more combinations of XO4, wherein M is Cs, Rb, K or NH4, and X is S or P.
[0044] The solid acid can be prepared by itself. Specifically, it can be one or more combinations of CsH2PO4, RbH2PO4, K2HPO4, NH4H2PO4, CsHSO4, RbHSO4, KHSO4, and NH4HSO4.
[0045] Corresponding to the mass of the above slurry, the mass of the solid acid is 40-50 g.
[0046] Furthermore, the sintered NiO / YSZ film is immersed in a solid acid solution at 150-200° C. for 4-6 hours.
[0047] The prepared porous membrane material is immersed in a solid acid solution at a preset high temperature;
[0048] The immersion is repeated for a certain number of times, and vacuum drying is performed after the immersion is completed to obtain a NiO / YSZ composite electrolyte membrane material.
[0049] Furthermore, the molar ratio of nickel oxide, yttria-stabilized zirconium oxide, and solid acid material is calculated based on the actual weighed mass to calculate the content of the solid acid material in the composite material, and can be adjusted according to actual conditions.
[0050] Example 1
[0051] This embodiment relates to a method for preparing a NiO / YSZ composite electrolyte membrane impregnated with solid acid at high temperature. In the composite electrolyte membrane, the mass ratio of yttria-stabilized zirconium oxide, nickel oxide, and solid acid material is 5:3:3; the method specifically comprises the following steps:
[0052] Step 1: nickel oxide, yttria-stabilized zirconium oxide, pore-forming agent, dispersant and water are prepared into a slurry; in this embodiment, 30 g of zirconium oxide powder, 18 g of nickel oxide, 10.5 g of dispersant, 1.5 g of binder, and 5 g of graphite or starch pore-forming agent are selected as the pore-forming agent;
[0053] Step 2: After ball milling the mixed slurry for 24 hours, a binder was added, stirred, and ball milled for 9 hours;
[0054] Step 3: After drying and degassing, the slurry is molded on a casting machine and demolded to form a NiO / YSZ film with a thickness of 0.42 mm;
[0055] Step 4: sintering the NiO / YSZ film at high temperature, wherein the high temperature sintering is programmed temperature firing. When the NiO / YSZ film is programmed temperature fired, the heating rate from room temperature to 400°C is 2°C / min, after being kept constant at 400°C for 2h, the heating rate from 400°C to 1400°C is 2°C / min, and the temperature is kept constant at 1400°C for 4h, and finally the temperature is lowered to room temperature at 2°C / min to prepare a NiO / YSZ porous film;
[0056] Step 5: After mixing 40 g of the prepared solid acid CsH2PO4 material with a small amount of distilled water, the solution is heated to 200°C;
[0057] Step 6: Vacuum the NiO / YSZ porous film to remove the air in its pores, put it into a heated solid acid solution, and immerse it at a constant temperature for 4 hours. Repeat the above process 8 to 10 times, and weigh 0.116g after drying at room temperature;
[0058] Step 7: Take out the immersed composite electrolyte film material and heat-treat it under water vapor at 150° C., and weigh 0.145 g after drying at room temperature.
[0059] Example 2
[0060] This embodiment relates to a method for preparing a NiO / YSZ composite electrolyte membrane impregnated with solid acid at high temperature. In the composite electrolyte membrane, the total mass ratio of yttria-stabilized zirconium oxide, nickel oxide, and solid acid material is 6:3:1. The method specifically comprises the following steps:
[0061] Step 1: Yttria-stabilized zirconium oxide, nickel oxide, pore-forming agent, dispersant and water are prepared into a slurry; in this embodiment, 32g of zirconium oxide powder, 16g of nickel oxide, 11g of dispersant, 2g of binder, and 6g of graphite or starch pore-forming agent are selected as the pore-forming agent;
[0062] Step 2: After ball milling the mixed slurry for 12 hours, a binder was added, and the mixture was stirred and ball milled for 9 hours;
[0063] Step 3: After drying and degassing, the slurry is molded on a casting machine and demolded to form a NiO / YSZ film with a thickness of 0.6 mm;
[0064] Step 4: sintering the NiO / YSZ film at high temperature, wherein the high temperature sintering is programmed temperature firing. When the NiO / YSZ film is programmed temperature fired, the heating rate from room temperature to 405°C is 2°C / min, after being kept at 405°C for 2h, the heating rate from 405°C to 1500°C is 3°C / min, and the temperature is kept at 1500°C for 4h, and finally the temperature is cooled to room temperature at 2°C / min to prepare a NiO / YSZ porous film;
[0065] Step 5: Mix 45g of the prepared solid acid CsH2PO4 and RbH2PO4 mixture with a small amount of distilled water, and heat the solution to 200°C;
[0066] Step 6: Vacuum the NiO / YSZ porous film to remove the air in its pores, put it into a heated solid acid solution, and immerse it at a constant temperature for 4 hours. Repeat the above process 8 to 10 times, and weigh 0.12g after drying at room temperature;
[0067] Step 7: Take out the immersed composite electrolyte film material and heat-treat it under water vapor conditions at 150° C., and weigh 0.133 g after drying at room temperature.
[0068] Example 3
[0069] This embodiment relates to a method for preparing a NiO / YSZ composite electrolyte membrane impregnated with solid acid at high temperature. In the composite electrolyte membrane, the total mass ratio of yttria-stabilized zirconium oxide, nickel oxide, and solid acid material is 6:2:2; specifically, the following steps are included:
[0070] Step 1: nickel oxide, yttria-stabilized zirconium oxide, pore former, dispersant and water are prepared into a slurry; in this embodiment, 30 g of zirconium oxide powder, 10 g of nickel oxide, 10.5 g of dispersant, 1.5 g of binder, and 5 g of graphite or starch pore former are selected as the pore former;
[0071] Step 2: After ball milling the mixed slurry for 12 hours, a binder was added, and the mixture was stirred and ball milled for 9 hours;
[0072] Step 3: After drying and degassing, the slurry is molded on a casting machine and demolded to form a NiO / YSZ film with a thickness of 0.5 mm;
[0073] Step 4: sintering the NiO / YSZ film at high temperature, wherein the high temperature sintering is programmed temperature firing. When the NiO / YSZ film is programmed temperature fired, the heating rate from room temperature to 400°C is 1°C / min, after being kept constant at 400°C for 2h, the heating rate from 400°C to 1600°C is 2°C / min, and the temperature is kept constant at 1600°C for 4h, and finally the temperature is reduced to room temperature at 2°C / min to prepare a NiO / YSZ porous film;
[0074] Step 5: Mix 50g of the prepared solid acid CsHSO4 and KHSO4 mixture with a small amount of distilled water, and heat the solution to 150°C;
[0075] Step 6: Vacuum the NiO / YSZ porous film to remove the air in its pores, put it into a heated solid acid solution, and immerse it at a constant temperature for 6 hours. Repeat the above process 8 to 10 times, and weigh 0.118g after drying at room temperature;
[0076] Step 7: Take out the immersed composite electrolyte film material and heat-treat it under water vapor conditions at 150° C., and weigh 0.147 g after drying at room temperature.
[0077] Example 4
[0078] This embodiment relates to a method for preparing a solid acid fuel cell, using Pt / C as an electrode material, using the above-mentioned high-temperature solid acid impregnated NiO / YSZ composite electrolyte membrane as a composite electrolyte film, including nickel oxide, yttria-stabilized zirconium oxide, and solid acid material in a total mass ratio of 5:3:3; specifically comprising the following steps:
[0079] Step 1: Prepare a slurry by mixing nickel oxide, yttria-stabilized zirconium oxide, a pore former, a dispersant and water; 30 g zirconium oxide powder, 18 g nickel oxide, 10.5 g dispersant, 1.5 g binder and 5 g graphite or starch pore former;
[0080] Step 2: After ball milling the mixed slurry for 24 hours, a binder was added, and the mixture was stirred and ball milled for 9 hours;
[0081] Step 3: After drying and degassing, the slurry is molded on a casting machine and demolded to form a NiO / YSZ film with a thickness of 0.42 mm;
[0082] Step 4: sintering the NiO / YSZ film at high temperature, wherein the high temperature sintering is programmed temperature firing. When the NiO / YSZ film is programmed temperature fired, the heating rate from room temperature to 400°C is 2°C / min, after being kept constant at 400°C for 1.85h, the heating rate from 400°C to 1300°C is 2°C / min, and the temperature is kept constant at 1300°C for 4.25h, and finally the temperature is reduced to room temperature at 1.5°C / min to prepare a NiO / YSZ porous film;
[0083] Step 5: After mixing 40g of the prepared solid acid CsH2PO4 or K2HPO4 and other materials with distilled water, the solution is heated to 200°C;
[0084] Step 6: Vacuum the NiO / YSZ porous film to remove the air in its pores, put it into a heated solid acid solution, and immerse it at a constant temperature for 4 hours. Repeat the above process 8 to 10 times, and weigh 0.116g after drying at room temperature;
[0085] Step 7: Take out the impregnated composite electrolyte film material and heat-treat it under water vapor conditions at 150° C., and weigh 0.145 g after drying at room temperature;
[0086] Step 8: stack the Pt / C sheet and the impregnated composite electrolyte film, and maintain constant temperature and pressure at 80° C. and 15 MPa for 30 minutes to prepare a solid acid fuel cell.
[0087] Example 5
[0088] This embodiment relates to a method for preparing a solid acid fuel cell, using Pt / C as an electrode material, using the above-mentioned high-temperature solid acid impregnated NiO / YSZ composite electrolyte membrane as a composite electrolyte film, including nickel oxide, yttria-stabilized zirconium oxide, and solid acid material in a total mass ratio of 6:3:1; specifically comprising the following steps:
[0089] Step 1: nickel oxide, yttria-stabilized zirconium oxide, pore former, dispersant and water are prepared into a slurry; in this embodiment, 32g of zirconium oxide powder, 16g of nickel oxide, 11g of dispersant, 2g of binder, and 6g of graphite or starch pore former are selected as the pore former;
[0090] Step 2: After ball milling the above mixed slurry for 24 hours, add the binder, stir and ball mill for 12 hours;
[0091] Step 3: After drying and degassing, the slurry is molded on a casting machine and demolded to form a NiO / YSZ film with a thickness of 0.6 mm;
[0092] Step 4: sintering the NiO / YSZ film at high temperature, wherein the high temperature sintering is programmed temperature firing. When the NiO / YSZ film is programmed temperature fired, the heating rate from room temperature to 400°C is 2°C / min, after being kept constant at 400°C for 2h, the heating rate from 400°C to 1500°C is 1°C / min, and the temperature is kept constant at 1500°C for 4h, and finally the temperature is reduced to room temperature at 1°C / min to prepare a NiO / YSZ porous film;
[0093] Step 5: After mixing 45 g of the prepared solid acid CsH2PO4 or RbH2PO4 and other materials with distilled water, the solution is heated to 200°C;
[0094] Step 6: Vacuum the NiO / YSZ porous film to remove the air in its pores, put it into a heated solid acid solution, and immerse it at a constant temperature for 4 hours. Repeat the above process 8 to 10 times, and weigh 0.12g after drying at room temperature;
[0095] Step 7: Take out the impregnated composite electrolyte film material and heat-treat it under water vapor conditions at 150° C., and weigh 0.133 g after drying at room temperature;
[0096] Step 8: stack the Pt / C sheet and the impregnated composite electrolyte film, and maintain constant temperature and pressure at 85° C. and 16 MPa for 30 minutes to prepare a solid acid fuel cell.
[0097] Example 6
[0098] This embodiment relates to a method for preparing a solid acid fuel cell, using Pt / C as an electrode material, using the above-mentioned high-temperature solid acid impregnated NiO / YSZ composite electrolyte membrane as a composite electrolyte film, including nickel oxide, yttria-stabilized zirconium oxide, and solid acid material in a total mass ratio of 6:2:2; specifically comprising the following steps:
[0099] Step 1: nickel oxide, yttria-stabilized zirconium oxide, pore former, dispersant and water are prepared into a slurry; in this embodiment, 30 g of zirconium oxide powder, 10 g of nickel oxide, 10.5 g of dispersant, 1.5 g of binder, and 5 g of graphite or starch pore former are selected as the pore former;
[0100] Step 2: After ball milling the above mixed slurry for 24 hours, add the binder, stir and ball mill for 12 hours;
[0101] Step 3: After drying and degassing, the slurry is molded on a casting machine and demolded to form a NiO / YSZ film with a thickness of 0.5 mm;
[0102] Step 4: sintering the NiO / YSZ film at high temperature, wherein the high temperature sintering is programmed temperature firing. When the NiO / YSZ film is programmed temperature fired, the heating rate from room temperature to 400°C is 2°C / min, after being kept constant at 400°C for 2h, the heating rate from 400°C to 1600°C is 2°C / min, and the temperature is kept constant at 1600°C for 4h, and finally the temperature is lowered to room temperature at 2°C / min to prepare a NiO / YSZ porous film;
[0103] Step 5: Add 50g of solid acid CsHSO4 or KHSO4 and other materials to distilled water, and heat the solution to 200℃;
[0104] Step 6: Vacuum the NiO / YSZ porous film to remove the air in its pores, put it into a heated solid acid solution, and immerse it at a constant temperature for 4 hours. Repeat the above process 8 to 10 times, and weigh 0.118g after drying at room temperature;
[0105] Step 7: Take out the impregnated composite electrolyte film material and heat-treat it under water vapor conditions at 150° C., and weigh 0.147 g after drying at room temperature;
[0106] Step 8: stack the Pt / C sheet and the impregnated composite electrolyte film, and maintain constant temperature and pressure at 80° C. and 15 MPa for 30 minutes to prepare a solid acid fuel cell.
[0107] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a NiO / YSZ composite electrolyte membrane impregnated with solid acid at high temperature, characterized in that: The method comprises the following steps: preparing slurry, ball milling, degassing, casting, calcining and drying, and specifically comprises the following steps: Yttria-stabilized zirconium oxide powder, nickel oxide, pore former, dispersant, binder and water are configured into a slurry. The slurry is calculated by mass ratio. The proportions of yttria-stabilized zirconium oxide powder, nickel oxide, pore former, dispersant and binder are 34.9-38.8%, 11.6-19.4%, 14.1-17.4%, 1.7-2.4%, 4.7-5.8% respectively, and the rest is water. After ball milling and drying the slurry to remove air, the prepared slurry is cast into a NiO / YSZ film material in a mold; The NiO / YSZ porous membrane material is prepared by sintering the cast NiO / YSZ membrane material at a high temperature; obtaining a solid acid solution; The prepared porous membrane material is immersed in a solid acid solution at 150-200°C for 4-6 hours; The impregnation is repeated for 8-10 times, and vacuum drying is performed after the impregnation is completed to obtain a NiO / YSZ composite electrolyte membrane material.
2. The method according to claim 1, characterized in that The specific steps of preparing the slurry are as follows: preparing the slurry by mixing NiO and YSZ powders with a pore former in distilled water and a dispersant, stirring the mixture for a period of time, adding a binder to the slurry, and then stirring for another 9 to 12 hours.
3. The method according to claim 1, characterized in that The prepared slurry is cast into a NiO / YSZ film material in a mold by evacuating the slurry, forming it on a casting machine, and then demolding it. The thickness of the ceramic sheet is 0.4-0.6 mm.
4. The method according to claim 1, characterized in that: The specific preparation process of NiO / YSZ porous membrane material is as follows: high temperature sintering is programmed temperature firing. When programmed temperature firing of NiO / YSZ film, the heating rate from room temperature to 400±10℃ is 1~2℃ / min. After maintaining a constant temperature at 400±10℃ for 2±0.5h, the heating rate from 400±10℃ to 1300~1600℃ is 1~3℃ / min. After maintaining a constant temperature at 1300~1600℃ for 4±0.5h, the temperature is finally reduced to room temperature at a rate of 1~2℃ / min.
5. The method according to claim 1, characterized in that The solid acid is MH x One or more combinations of XO4, wherein M is Cs, Rb, K or NH4, and X is S or P.
6. The method according to claim 1, characterized in that The molar ratio of nickel oxide, yttria-stabilized zirconium oxide, and solid acid material is used to calculate the content of the solid acid material in the composite material based on the actual weighed mass.
7. A NiO / YSZ composite electrolyte membrane impregnated with solid acid at high temperature prepared by the method according to any one of claims 1 to 6.
8. A method for preparing a solid acid fuel cell, characterized in that: A NiO / YSZ composite electrolyte membrane impregnated with solid acid at high temperature prepared by the method according to any one of claims 1 to 6 is prepared, a Pt / C sheet is stacked with the impregnated composite electrolyte membrane, and a solid acid fuel cell is prepared by maintaining a constant temperature and pressure at 80±5°C and 15±1Mpa for 30±5min.