A rotary hearth furnace spiral blade with wear-resistant protrusions and a preparation method and application thereof

By inlaid wear-resistant protrusions on the upper edge of the rotary furnace spiral blade and designing their hardness and angle, the wear problem in high-temperature environment is solved, the scraping efficiency and service life are improved, and the wear resistance and mechanical strength are improved.

CN118482561BActive Publication Date: 2024-11-19HUAQINGPING WEAR RESISTANT TECH (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410939488.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-19
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The rotary bottom furnace spiral blades are prone to wear abrasive particles in high temperature environments, resulting in a decrease in wear resistance, short service life, and low efficiency when scraping off plates, which affects the operation of the equipment.

Method used

Wear-resistant protrusions are embedded on the upper edge of the blade base, and their hardness and angle distribution are specially designed to improve wear resistance and mechanical strength and extend service life.

Benefits of technology

It significantly improves the scraping efficiency of plate solids, reduces the wear rate of blades, extends service life, and maintains uniform wear in high-temperature environments, making it suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118482561B_ABST
    Figure CN118482561B_ABST
Patent Text Reader

Abstract

The present invention provides a rotary hearth furnace spiral blade with a wear-resistant protrusion, a preparation method and an application thereof, wherein the rotary hearth furnace spiral blade comprises a blade base, a wear-resistant protrusion embedded in the upper edge of the blade base, and a mounting portion penetrating the lower edge of the blade base; the hardness of the wear-resistant protrusion is greater than the hardness of the blade base; the upper edge of the blade base is a force-bearing part for the rotary hearth furnace spiral blade to scrape off the hardened material. The rotary hearth furnace spiral blade provided by the present invention significantly improves the wear resistance and mechanical strength of the blade by embedding the wear-resistant protrusion in the upper edge of the blade base, improves the scraping efficiency of the hardened material, and prolongs the service life of the blade, which is conducive to large-scale promotion and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel production equipment, and relates to a rotary hearth furnace spiral blade, and in particular to a rotary hearth furnace spiral blade with a wear-resistant protrusion, and a preparation method and application thereof. Background Art

[0002] The rotary hearth furnace is mainly used to process solid wastes such as ironmaking bag dust removal ash, ore trough dust removal ash, steelmaking coarse particles, sludge, etc. in steel plants, and has become an important device for the development of circular economy in the steel industry. Among them, the internal spiral discharger equipment needs to use high-temperature resistant, wear-resistant, and impact-resistant spiral blades when conveying high-temperature pellets. The equipment usually operates continuously in a high-temperature environment of 800-1200℃. The service life of the spiral blades of the rotary hearth furnace is generally about 2 months. They are often made of highly wear-resistant and high-temperature resistant nickel-chromium-tungsten series materials, such as Cr28Ni20W40. This type of material will anneal and crack when it is continuously operated at high temperatures, resulting in a decrease in the wear resistance of the material. After 2 months of use, the production capacity will decrease, and the blades must be replaced in time. Each shutdown for maintenance will cause economic losses of up to hundreds of thousands of yuan.

[0003] The spiral blades of the rotary hearth furnace must not only meet the wear resistance of continuous contact with metal materials when conveying materials, but also have the mechanical strength required for conveying pellets and cleaning the bottom of the furnace under high temperature conditions. The main failure form of the spiral blades of the rotary hearth furnace is abrasive wear in a high temperature environment. Since the powdered materials on the furnace bed cannot be discharged in time, they will form plated materials. When they accumulate to a certain height, they are scraped off and discharged by the spiral blades. In the process of scraping off these plated materials, since the upper end surface of the spiral blades of the rotary hearth furnace is worn very tilted, it is difficult to scrape off this plated material, which leads to serious wear on the upper end surface and affects the service life of the blades.

[0004] It can be seen that how to provide a rotary hearth furnace spiral blade and a preparation method to improve the wear resistance and mechanical strength of the blade, enhance the scraping efficiency of the compacted material, and extend the service life of the blade has become an urgent problem that technical personnel in this field need to solve. Summary of the invention

[0005] The purpose of the present invention is to provide a rotary hearth furnace spiral blade with a wear-resistant protrusion, a preparation method and an application thereof. By embedding the wear-resistant protrusion on the upper edge of the blade base and specially designing the angle distribution and material of the wear-resistant protrusion, the wear resistance and mechanical strength of the blade are significantly improved, the scraping efficiency of the compacted matter is improved, the service life of the blade is extended, and large-scale promotion and application are facilitated.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a rotary hearth furnace spiral blade having a wear-resistant protrusion, wherein the rotary hearth furnace spiral blade comprises a blade base, a wear-resistant protrusion embedded in the upper edge of the blade base, and a mounting portion penetrating the lower edge of the blade base.

[0008] The hardness of the wear-resistant protrusion is greater than the hardness of the blade base.

[0009] The upper edge of the blade base is the force-bearing part of the rotary hearth furnace spiral blade for scraping off the compacted matter.

[0010] The present invention embeds a wear-resistant protrusion on the upper edge of the blade base, and limits the hardness of the wear-resistant protrusion to be greater than the hardness of the blade base, so that during the spiral operation of the blade, the wear-resistant protrusion can scrape off the compacted material, which is beneficial to the full cracking and efficient removal of the compacted layer, thereby improving the scraping efficiency of the compacted material.

[0011] In addition, the wear-resistant protrusion isolates the blade base and the plated material from each other, protects the blade base, significantly reduces the wear rate of the blade base, thereby extending the service life of the blade, which is conducive to large-scale promotion and application.

[0012] On each rotary hearth furnace spiral blade, the number of the wear-resistant protrusions is at least 3, and they are arranged in sequence along the upper edge of the blade base, for example, 3, 4, 5, 6, 7, 8, 9 or 10, more preferably 4-6, but not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0013] The angle between the central axis symmetry line of the wear-resistant protrusion and the corresponding tangent line of the upper edge of the blade base is 30°-90°, for example, it can be 30°, 35°, 40°, 45°, 50°, 55°, 60°, 65°, 70°, 75°, 80°, 85° or 90°, but is not limited to the listed values, and other unlisted values ​​within this numerical range are also applicable.

[0014] Along the rotation direction of the spiral blade of the rotary hearth furnace, the angle increases successively, and the difference between the angles of adjacent wear-resistant protrusions is 5°-10°, for example, it can be 5°, 6°, 7°, 8°, 9° or 10°, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0015] In the present invention, the tangent corresponding to the upper edge of the blade base specifically refers to the tangent of the intersection of the central axis symmetry line of the wear-resistant protrusion and the upper edge of the blade base. The size of the above-mentioned angle directly affects the stress distribution when the wear-resistant protrusion contacts the material, and further determines its penetration ability and effect when scraping off the deposited materials on the bottom of the furnace. The present invention specifically limits the above-mentioned angle to the range of 30°-90°, which significantly improves the penetration of the wear-resistant protrusion on the deposited materials, thereby more effectively breaking and removing the deposited materials, while ensuring that the blade wears relatively evenly throughout the entire service life. If the above-mentioned angle is too small or too large, it will cause certain areas of the blade to wear faster, while other areas will wear more slowly, resulting in uneven wear.

[0016] In addition, too large an angle can easily cause the wear-resistant protrusion to break under high stress. The present invention can ensure that the wear-resistant protrusion has sufficient structural strength while providing sufficient wear resistance by limiting the angle range, thereby reducing the risk of breakage.

[0017] Furthermore, the present invention limits the angle between the central axis symmetry line of the wear-resistant protrusion and the corresponding tangent line of the upper edge of the blade base to increase successively along the rotation direction of the spiral blade of the rotary hearth furnace, and the difference between the angles of adjacent wear-resistant protrusions is 5°-10°, so that the wear-resistant protrusions subjected to greater force have higher angles, thereby further improving the wear uniformity of the wear-resistant protrusions.

[0018] The method for preparing the wear-resistant protrusion comprises the following steps:

[0019] (1) Mixing activated powder and hard particles and sintering at high temperature to obtain hard particles with surface metallization;

[0020] (2) Mixing the induction powder and the surface metallized hard particles obtained in step (1), preheating them in an oxygen-isolated environment, injecting alloy melt into them for sintering, and obtaining the wear-resistant protrusions.

[0021] Wherein, the activated powder in step (1) and the induced powder in step (2) both contain SiO2 powder.

[0022] In the present invention, the SiO2 powder contained in the activated powder and the induced powder can agglomerate with the hard particles during the sintering process and coat the surface of the hard particles to form a strong bonding interface, thereby improving the oxidation resistance and wear resistance of the wear-resistant protrusions in a high temperature environment (above 1000°C). In the subsequent blade casting process, SiO2 is coated on the surface of the wear-resistant protrusions in the form of particles, further enhancing the wear resistance of the wear-resistant protrusions.

[0023] Optionally, the wear-resistant protrusion is hidden inside the upper edge of the blade base, presenting a smooth curved edge.

[0024] In the present invention, the wear-resistant protrusion is hidden inside the upper edge of the blade base. In the initial scraping stage, the rotation speed and material thickness of the spiral blade of the rotary hearth furnace are controlled to make the blade base wear evenly. The wear-resistant protrusion is gradually exposed by utilizing the difference in wear resistance between the wear-resistant protrusion and the blade base.

[0025] Optionally, the wear-resistant protrusion is exposed outside the upper end edge of the blade base and presents a wavy edge or a serrated edge.

[0026] Preferably, the average height of the wavy edge or the serrated edge is 2-5 mm, for example, it can be 2 mm, 2.2 mm, 2.4 mm, 2.6 mm, 2.8 mm, 3 mm, 3.2 mm, 3.4 mm, 3.6 mm, 3.8 mm, 4 mm, 4.2 mm, 4.4 mm, 4.6 mm, 4.8 mm or 5 mm, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] In the present invention, the average height of the wavy edge or the serrated edge specifically refers to the height of the wear-resistant protrusion exposed to the upper end edge of the blade base.

[0028] Preferably, the wear-resistant protrusion has a shape of a cube and / or a frustum.

[0029] Preferably, the length of the cube is 30-50 mm, for example, it can be 30 mm, 32 mm, 34 mm, 36 mm, 38 mm, 40 mm, 42 mm, 44 mm, 46 mm, 48 mm or 50 mm, and the width and height are 10-30 mm respectively, for example, it can be 10 mm, 12 mm, 14 mm, 16 mm, 18 mm, 20 mm, 22 mm, 24 mm, 26 mm, 28 mm or 30 mm, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, the upper table surface of the truncated cone has a diameter of 20-40mm, for example, it can be 20mm, 22mm, 24mm, 26mm, 28mm, 30mm, 32mm, 34mm, 36mm, 38mm or 40mm, the lower table surface has a diameter of 30-50mm, for example, it can be 30mm, 32mm, 34mm, 36mm, 38mm, 40mm, 42mm, 44mm, 46mm, 48mm or 50mm, and the height is 30-50mm, for example, it can be 30mm, 32mm, 34mm, 36mm, 38mm, 40mm, 42mm, 44mm, 46mm, 48mm or 50mm, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the activated powder in step (1) comprises SiO2 powder, MnFe powder, La2O3 powder and adhesive powder, and is obtained by ball milling.

[0032] Preferably, the mass ratio of the SiO2 powder, MnFe powder, La2O3 powder and adhesive powder is (1-3):(6-10):1:1, for example, it can be 1:6:1:1, 1.5:7:1:1, 2:8:1:1, 2.5:9:1:1 or 3:10:1:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the ball milling is carried out in an industrial ball mill, and the ball milling time is 8-12 h, for example, 8 h, 8.5 h, 9 h, 9.5 h, 10 h, 10.5 h, 11 h, 11.5 h or 12 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the average particle size of the activated powder in step (1) is ≥ 400 mesh, for example, it can be 400 mesh, 500 mesh, 600 mesh, 700 mesh or 800 mesh, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0035] Preferably, the hard particles in step (1) include any one of Al2O3, ZrO2, TiC, WC, Cr3C2, TiB ceramics, BN ceramics or ZTA ceramics, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of Al2O3 and ZrO2, a combination of ZrO2 and TiC, a combination of TiC and WC, a combination of WC and Cr3C2, a combination of Cr3C2 and TiB ceramics, a combination of TiB ceramics and BN ceramics, or a combination of BN ceramics and ZTA ceramics.

[0036] Preferably, the average particle size of the hard particles in step (1) is 2-5 mm, for example, 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, 4.5 mm or 5 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0037] Preferably, the hard particles in step (1) are sequentially alkali washed and dried before mixing.

[0038] Preferably, the mixing time in step (1) is 6-10 h, for example, 6 h, 6.5 h, 7 h, 7.5 h, 8 h, 8.5 h, 9 h, 9.5 h or 10 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0039] Preferably, the temperature of the high temperature sintering in step (1) is 1300-1400°C, for example, it can be 1300°C, 1320°C, 1340°C, 1360°C, 1380°C or 1400°C, and the time is 1-2h, for example, it can be 1h, 1.2h, 1.4h, 1.6h, 1.8h or 2h, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0040] Preferably, the induced powder in step (2) comprises SiO2 powder and MnFe powder.

[0041] Preferably, the mixing volume ratio of the induced powder and the hard particles in step (2) is 1:(3-5), for example, it can be 1:3, 1:3.2, 1:3.4, 1:3.6, 1:3.8, 1:4, 1:4.2, 1:4.4, 1:4.6, 1:4.8 or 1:5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Preferably, in step (2), the oxygen-isolated environment is filled with argon gas.

[0043] Preferably, the temperature of the preheat treatment in step (2) is 900-1000°C, for example, it can be 900°C, 910°C, 920°C, 930°C, 940°C, 950°C, 960°C, 970°C, 980°C, 990°C or 1000°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0044] Preferably, the alloy melt in step (2) comprises the following components in parts by weight:

[0045]

[0046] The balance is Fe and inevitable impurities.

[0047] Wherein, the weight portion of Cr is 10-50 parts, for example, it can be 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts or 50 parts, the weight portion of Ni is 5-60 parts, for example, it can be 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts or 60 parts, the weight portion of Mo is 0-60 parts, for example, it can be 0 part, 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts or 60 parts, and the weight portion of Mn is 0-40 parts, for example, it can be 0 part, 2 parts, 4 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 17 parts 8 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts or 40 parts, the weight portion of W is 0-40 parts, for example, it can be 0 part, 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts or 40 parts, the weight portion of Si is 0-2 parts, for example, it can be 0 part, 0.2 parts, 0.4 parts, 0.6 parts, 0.8 parts, 1 part, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts or 2 parts, the weight portion of C is 0.1-3 parts, for example, it can be 0.1 part, 0.5 parts, 1 part, 1.5 parts, 2 parts, 2.5 parts or 3 parts, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0048] In the present invention, Cr in the alloy melt is crucial to improving the hardness, wear resistance and oxidation resistance of the wear-resistant protrusion; Ni can improve the toughness of the material and its strength and stability in a high-temperature environment; Mo, as a strong carbide-forming element, can significantly improve the hardness of the material; Mn can improve the strength and toughness of the material and help to reduce the brittle transition temperature of the material; W is a high-melting-point metal that can significantly improve the high-temperature strength and wear resistance of the material; an appropriate amount of C is an important element for forming carbides, which can significantly improve the hardness and wear resistance of the material.

[0049] The present invention optimizes the microstructure and macroscopic properties of the wear-resistant protrusions by rationally designing the chemical composition of the wear-resistant protrusions, so that the wear-resistant protrusions have excellent toughness, wear resistance, heat resistance and oxidation resistance in a high temperature environment (above 1000°C).

[0050] In a second aspect, the present invention provides a method for preparing a spiral blade of a rotary hearth furnace as described in the first aspect, the preparation method comprising the following steps:

[0051] (A) Make a foam model according to the blade drawing and embed the wear-resistant protrusions into the foam model;

[0052] (B) embedding the foam model inlaid with wear-resistant protrusions obtained in step (A) into a sand mold and vibrating it, injecting alloy melt after evacuation, and obtaining a cast blade after cooling;

[0053] (C) The as-cast blade obtained in step (B) is polished, quenched and air-cooled in sequence to obtain the rotary hearth furnace spiral blade.

[0054] Preferably, before the wear-resistant protrusions are embedded in step (A), a blind hole to be embedded is cut out at the upper edge of the foam model.

[0055] Preferably, the alloy melt in step (B) has the same composition as the alloy melt used in the process of preparing the wear-resistant protrusions.

[0056] Preferably, the quenching temperature in step (C) is 950-1000°C, for example, it can be 950°C, 955°C, 960°C, 965°C, 970°C, 975°C, 980°C, 985°C, 990°C, 995°C or 1000°C, and the holding time is 1-3h, for example, it can be 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, 2.2h, 2.4h, 2.6h, 2.8h or 3h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0057] Preferably, there are at least two temperings between the quenching and air cooling, and more preferably two temperings, so as to fully regulate the blade structure, so that the carbides are dispersed and precipitated to form secondary hardening. The resulting blades have high temperature strength and wear resistance, as well as excellent impact toughness, and are suitable for long-term service under high temperature and high wear resistance conditions.

[0058] Preferably, the tempering temperature is 400-500°C, for example, it can be 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C or 500°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0059] Preferably, the air cooling adopts a graded cooling method, and the wind speed is controlled to prevent the blades from cracking during the cooling process.

[0060] In a third aspect, the present invention provides an application of the spiral blade of a rotary hearth furnace as described in the first aspect, wherein the spiral blade of the rotary hearth furnace is used to transport materials and scrape off deposits on the furnace bottom.

[0061] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0062] Compared with the prior art, the present invention has the following beneficial effects:

[0063] (1) The present invention embeds a wear-resistant protrusion on the upper edge of the blade base, and limits the hardness of the wear-resistant protrusion to be greater than the hardness of the blade base, so that during the spiral operation of the blade, the wear-resistant protrusion can scrape off the compacted material, which is beneficial to the full cracking and efficient removal of the compacted layer, thereby improving the scraping efficiency of the compacted material; the wear-resistant protrusion isolates the blade base and the compacted material from each other, protects the blade base, significantly reduces the wear rate of the blade base, thereby extending the service life of the blade, and is beneficial to large-scale promotion and application.

[0064] (2) The present invention specifically limits the included angle of the wear-resistant protrusion to the range of 30°-90°, which significantly improves the penetration of the wear-resistant protrusion on the compacted material, thereby more effectively breaking and removing the compacted material, while ensuring that the blade wears relatively evenly throughout its entire service life; the included angle increases successively along the rotation direction of the spiral blade of the rotary hearth furnace, and the difference between the included angles of adjacent wear-resistant protrusions is 5°-10°, so that the included angle of the wear-resistant protrusion that is subjected to greater force is higher, thereby further improving the wear uniformity of the wear-resistant protrusion.

[0065] (3) The SiO2 powder contained in the activated powder and the induced powder can agglomerate with the hard particles during the sintering process and coat the surface of the hard particles, thereby forming a strong bonding interface, improving the oxidation resistance and wear resistance of the wear-resistant protrusions in high temperature environments (above 1000°C). In the subsequent blade casting process, SiO2 is coated on the surface of the wear-resistant protrusions in the form of particles, further enhancing the wear resistance of the wear-resistant protrusions. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] Figure 1 is a schematic diagram of the spiral blade structure of a rotary hearth furnace provided in Example 1;

[0067] Figure 2 is a schematic diagram of the spiral blade structure of the rotary hearth furnace provided in Examples 2 and 3;

[0068] Figure 3 is a comparison diagram of the wear of the spiral blades of the rotary hearth furnace provided by Example 1 and Comparative Example 1;

[0069] Figure 4 This is a comparison diagram of the spiral blades of the rotary hearth furnace obtained in Example 1 before and after wear;

[0070] Figure 5 is a scanning electron microscope photograph of a cross section of a wear-resistant protrusion in a spiral blade of a rotary hearth furnace provided in Example 1;

[0071] Figure 6This is a cross-sectional scanning electron microscope photograph of the wear-resistant protrusion in the spiral blade of the rotary hearth furnace provided in Example 1 and a comparison chart of the EDS component analysis.

[0072] Among them: 1-blade base; 2-wear-resistant protrusion; 3-installation part. DETAILED DESCRIPTION

[0073] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0074] Example 1

[0075] This embodiment provides a rotary hearth furnace spiral blade with a wear-resistant protrusion and a preparation method thereof, such as Figure 1 As shown, the rotary hearth furnace spiral blade comprises a blade base 1, a wear-resistant protrusion 2 embedded in the upper edge of the blade base 1, and a mounting portion 3 penetrating the lower edge of the blade base 1. The hardness of the wear-resistant protrusion 2 is greater than the hardness of the blade base 1; the upper edge of the blade base 1 is the force-bearing part of the rotary hearth furnace spiral blade for scraping off the hardened material; and the mounting portion 3 is a mounting hole.

[0076] In the present embodiment, the number of the wear-resistant protrusions 2 on each rotary hearth furnace spiral blade is 5, and they are arranged in sequence along the upper edge of the blade base; along the rotation direction of the rotary hearth furnace spiral blade, the angles between the central axis symmetry line of the wear-resistant protrusion 2 and the corresponding tangent line of the upper edge of the blade base 1 are 30°, 40°, 50°, 60°, and 70°, respectively; the wear-resistant protrusion 2 is hidden inside the upper edge of the blade base 1, presenting a smooth curved edge, and in the initial scraping stage, the rotation speed and material thickness of the rotary hearth furnace spiral blade are controlled to make the blade base 1 wear evenly, and the wear-resistant performance difference between the wear-resistant protrusion 2 and the blade base 1 is utilized to gradually expose the wear-resistant protrusion 2; the wear-resistant protrusion 2 is in the shape of a cube, and the length, width and height of the cube are all 30 mm.

[0077] In this embodiment, the method for preparing the wear-resistant protrusion 2 comprises the following steps:

[0078] (1) Mix 2 parts of SiO2 powder, 8 parts of MnFe powder, 1 part of La2O3 powder and 1 part of binder powder (paraffin), and ball mill them in an industrial ball mill for 10 hours to obtain an activated powder with an average particle size of 400 mesh;

[0079] (2) ZTA ceramics with an average particle size of 4 mm were selected as hard particles. After alkali washing and drying, the hard particles were added to the activated powder and mixed for 8 hours so that the activated powder was evenly coated on the surface of the hard particles. The hard particles were sintered at 1350°C for 1.5 hours to form a metallurgical bond between the activated powder and the surface of the hard particles, thereby obtaining hard particles with surface metallization.

[0080] (3) SiO2 powder and MnFe powder are used as induction powders. The induction powders and the surface metallized hard particles obtained in step (2) are mixed in a small crucible (diameter 45 mm) at a volume ratio of 1:4, nitrogen is filled into the crucible to isolate oxygen, the small crucible is preheated to 980°C, and alloy melt is injected for sintering to obtain the wear-resistant protrusion.

[0081] Wherein, the alloy melt in step (3) comprises the following components in parts by weight:

[0082]

[0083] The balance is Fe and inevitable impurities.

[0084] In this embodiment, the method for preparing the spiral blades of the rotary hearth furnace comprises the following steps:

[0085] (A) A foam model is made according to the blade drawing, a blind hole to be embedded is first cut on the upper edge of the foam model, and then the wear-resistant protrusion 2 is embedded in the foam model;

[0086] (B) embedding the foam model inlaid with the wear-resistant protrusion 2 obtained in step (A) into a sand mold and vibrating it, injecting an alloy melt after evacuation, and obtaining a cast blade after cooling; wherein the alloy melt has the same composition as the alloy melt used in the preparation process of the wear-resistant protrusion 2;

[0087] (C) The as-cast blade obtained in step (B) is taken out and polished, and then the blade is placed in a heat treatment furnace and slowly heated to 980°C for quenching. After keeping the temperature for 2 hours, it is cooled by graded air cooling, and tempered twice in this process, each tempering temperature is 450°C, and finally the rotary hearth furnace spiral blade is obtained.

[0088] Example 2

[0089] This embodiment provides a rotary hearth furnace spiral blade with a wear-resistant protrusion and a preparation method thereof, such as Figure 2 As shown, the rotary hearth furnace spiral blade comprises a blade base 1, a wear-resistant protrusion 2 embedded in the upper edge of the blade base 1, and a mounting portion 3 penetrating the lower edge of the blade base 1. The hardness of the wear-resistant protrusion 2 is greater than the hardness of the blade base 1; the upper edge of the blade base 1 is the force-bearing part of the rotary hearth furnace spiral blade for scraping off the hardened material; and the mounting portion 3 is a mounting hole.

[0090] In this embodiment, on each rotary hearth furnace spiral blade, the number of the wear-resistant protrusions 2 is 5, and they are arranged in sequence along the upper edge of the blade base; along the rotation direction of the rotary hearth furnace spiral blade, the angles between the central axis symmetry line of the wear-resistant protrusion 2 and the corresponding tangent line of the upper edge of the blade base 1 are 70°, 75°, 80°, 85°, and 90°, respectively; the wear-resistant protrusion 2 is exposed to the outside of the upper edge of the blade base 1, presenting a serrated edge, and the average height of the serrated edge is 3 mm; the wear-resistant protrusion 2 is in the shape of a cube, and the length, width and height of the cube are all 30 mm.

[0091] In this embodiment, the method for preparing the wear-resistant protrusion 2 comprises the following steps:

[0092] (1) Mix 1 part of SiO2 powder, 6 parts of MnFe powder, 1 part of La2O3 powder and 1 part of binder powder (paraffin), and ball mill them in an industrial ball mill for 8 hours to obtain an activated powder with an average particle size of 500 mesh;

[0093] (2) TiB ceramics with an average particle size of 2 mm were selected as hard particles. After alkali washing and drying, the hard particles were added to the activated powder and mixed for 6 hours so that the activated powder was evenly coated on the surface of the hard particles. The hard particles were sintered at 1300°C for 2 hours to form a metallurgical bond between the activated powder and the surface of the hard particles, thereby obtaining hard particles with surface metallization.

[0094] (3) SiO2 powder and MnFe powder are used as induction powders. The induction powders and the surface metallized hard particles obtained in step (2) are mixed in a small crucible (with a diameter of 45 mm) at a volume ratio of 1:3. Nitrogen is filled into the crucible to isolate oxygen. The small crucible is preheated to 900°C, and alloy melt is injected for sintering to obtain the wear-resistant protrusion.

[0095] Wherein, the alloy melt in step (3) comprises the following components in parts by weight:

[0096]

[0097] The balance is Fe and inevitable impurities.

[0098] In this embodiment, the method for preparing the spiral blades of the rotary hearth furnace comprises the following steps:

[0099] (A) A foam model is made according to the blade drawing, a blind hole to be embedded is first cut on the upper edge of the foam model, and then the wear-resistant protrusion 2 is embedded in the foam model;

[0100] (B) embedding the foam model inlaid with the wear-resistant protrusion 2 obtained in step (A) into a sand mold and vibrating it, injecting an alloy melt after evacuation, and obtaining a cast blade after cooling; wherein the alloy melt has the same composition as the alloy melt used in the preparation process of the wear-resistant protrusion 2;

[0101] (C) The as-cast blade obtained in step (B) is taken out and polished, and then the blade is placed in a heat treatment furnace and slowly heated to 950°C for quenching. After keeping the temperature for 3 hours, it is cooled by graded air cooling, and tempered twice in this process, each tempering temperature is 400°C, and finally the rotary hearth furnace spiral blade is obtained.

[0102] Example 3

[0103] This embodiment provides a rotary hearth furnace spiral blade with a wear-resistant protrusion and a preparation method thereof, such as Figure 2 As shown, the rotary hearth furnace spiral blade comprises a blade base 1, a wear-resistant protrusion 2 embedded in the upper edge of the blade base 1, and a mounting portion 3 penetrating the lower edge of the blade base 1. The hardness of the wear-resistant protrusion 2 is greater than the hardness of the blade base 1; the upper edge of the blade base 1 is the force-bearing part of the rotary hearth furnace spiral blade for scraping off the hardened material; and the mounting portion 3 is a mounting hole.

[0104] In this embodiment, on each rotary hearth furnace spiral blade, the number of the wear-resistant protrusions 2 is 5, and they are arranged in sequence along the upper edge of the blade base; along the rotation direction of the rotary hearth furnace spiral blade, the angles between the central axis symmetry line of the wear-resistant protrusion 2 and the corresponding tangent line of the upper edge of the blade base 1 are 50°, 60°, 70°, 80°, and 90°, respectively; the wear-resistant protrusion 2 is exposed to the outside of the upper edge of the blade base 1, presenting a serrated edge, and the average height of the serrated edge is 5 mm; the wear-resistant protrusion 2 is in the shape of a cube, and the length, width and height of the cube are all 30 mm.

[0105] In this embodiment, the method for preparing the wear-resistant protrusion 2 comprises the following steps:

[0106] (1) Mix 3 parts of SiO2 powder, 10 parts of MnFe powder, 1 part of La2O3 powder and 1 part of binder powder (paraffin), and ball mill them in an industrial ball mill for 12 hours to obtain an activated powder with an average particle size of 400 mesh;

[0107] (2) Al2O3 with an average particle size of 5 mm was selected as hard particles. After alkali washing and drying, the hard particles were added to the activated powder and mixed for 10 hours so that the activated powder was evenly coated on the surface of the hard particles. The particles were sintered at 1400°C for 1 hour to form a metallurgical bond between the activated powder and the surface of the hard particles, thereby obtaining hard particles with surface metallization.

[0108] (3) SiO2 powder and MnFe powder are used as induction powders. The induction powders and the surface metallized hard particles obtained in step (2) are mixed in a small crucible (with a diameter of 45 mm) at a volume ratio of 1:5, and nitrogen is filled into the crucible to isolate oxygen. The small crucible is preheated to 1000°C, and alloy melt is injected for sintering to obtain the wear-resistant protrusion.

[0109] Wherein, the alloy melt in step (3) comprises the following components in parts by weight:

[0110]

[0111] The balance is Fe and inevitable impurities.

[0112] In this embodiment, the method for preparing the spiral blades of the rotary hearth furnace comprises the following steps:

[0113] (A) A foam model is made according to the blade drawing, a blind hole to be embedded is first cut on the upper edge of the foam model, and then the wear-resistant protrusion 2 is embedded in the foam model;

[0114] (B) embedding the foam model inlaid with the wear-resistant protrusion 2 obtained in step (A) into a sand mold and vibrating it, injecting an alloy melt after evacuation, and obtaining a cast blade after cooling; wherein the alloy melt has the same composition as the alloy melt used in the preparation process of the wear-resistant protrusion 2;

[0115] (C) The as-cast blade obtained in step (B) is taken out and polished, and then the blade is placed in a heat treatment furnace and slowly heated to 1000°C for quenching. After keeping warm for 1 hour, it is cooled by graded air cooling, and tempered twice in this process, each tempering temperature is 500°C, and finally the rotary hearth furnace spiral blade is obtained.

[0116] Example 4

[0117] The present embodiment provides a rotary hearth furnace spiral blade with a wear-resistant protrusion and a preparation method thereof. Except that the angle between the central axis symmetry line of the wear-resistant protrusion 2 and the corresponding tangent line of the upper edge of the blade base 1 is changed to 60°, the remaining structures and conditions are the same as those in Example 1, so they are not repeated here.

[0118] Example 5

[0119] The present embodiment provides a rotary hearth furnace spiral blade with a wear-resistant protrusion and a preparation method thereof. Except for the angles between the central axis symmetry line of the wear-resistant protrusion 2 and the corresponding tangent line of the upper edge of the blade base 1 along the rotation direction of the rotary hearth furnace spiral blade, the remaining structures and conditions are the same as those in Example 1, so they are not repeated here.

[0120] Example 6

[0121] The present embodiment provides a rotary hearth furnace spiral blade with a wear-resistant protrusion and a preparation method thereof. Except that the shape of the wear-resistant protrusion 2 is changed to a truncated cone, and the upper table diameter is 30 mm, the lower table diameter is 40 mm, and the height is 40 mm, the remaining structures and conditions are the same as those in Example 1, so they are not repeated here.

[0122] Comparative Example 1

[0123] This comparative example provides a rotary hearth furnace spiral blade and a preparation method thereof, except that the wear-resistant protrusion 2 is not embedded in the upper edge of the blade base 1, and the rotary hearth furnace spiral blade is directly cast using alloy melt, the rest of the structure and conditions are the same as those in Example 1, so they are not described here.

[0124] Performance Testing

[0125] The spiral blades of the rotary hearth furnace obtained in Example 1 and Comparative Example 1 were respectively installed in the spiral discharger inside the rotary hearth furnace, and the wear of the spiral blades was observed after continuous use for 2 months.

[0126] like Figure 3 As shown, the red arrows in Figure (a) and Figure (b) indicate the spiral blades of the rotary hearth furnace obtained in Example 1, and the black arrows indicate the spiral blades of the rotary hearth furnace obtained in Comparative Example 1. Comparison shows that the wear resistance of the spiral blades of the rotary hearth furnace obtained in Example 1 is significantly better than that of Comparative Example 1, and the service life of the blades is also significantly longer than that of Comparative Example 1.

[0127] like Figure 4 As shown, according to the comparison before and after wear of the spiral blades of the rotary hearth furnace obtained in Example 1, it can be seen that the wear thickness of the spiral blades of the rotary hearth furnace obtained in Example 1 is only about 1 cm after continuous use for 2 months, and can be continuously used for more than 6 months.

[0128] like Figure 5 As shown, the cross-sectional scanning electron microscope photograph of the wear-resistant protrusions in the spiral blade of the rotary hearth furnace obtained in Example 1 shows that the hard particles of the ZTA ceramic material are tightly fused with the high-temperature alloy, and granular SiO2 powder can be seen gathered and wrapped around the ZTA ceramic particles at the interface between the two.

[0129] like Figure 6 As shown, the cross-sectional scanning electron microscope photograph of the wear-resistant protrusion in the spiral blade of the rotary hearth furnace obtained in Example 1 and the EDS composition analysis comparison chart show that the interface between the ZTA ceramic particles and the alloy is mainly enriched with Si, O and Al elements, indicating that a crystal spinel structure of aluminum oxide and silicon oxide has been formed at this interface, that is, a strong bonding interface has been formed.

[0130] The wear resistance of the rotary hearth furnace spiral blades obtained in Examples 2-6 is similar to that in Example 1, but the wear uniformity of the wear-resistant protrusions in the rotary hearth furnace spiral blades obtained in Examples 4 and 5 is not as good as that in Example 1. This is mainly because the angular distribution of the wear-resistant protrusions in the rotary hearth furnace spiral blades obtained in Examples 4 and 5 is not optimized.

[0131] It can be seen that the present invention embeds a wear-resistant protrusion on the upper edge of the blade base, and limits the hardness of the wear-resistant protrusion to be greater than the hardness of the blade base, so that during the spiral operation of the blade, the wear-resistant protrusion can scrape the compacted material, which is beneficial to the full cracking and efficient removal of the compacted layer, thereby improving the scraping efficiency of the compacted material; the wear-resistant protrusion isolates the blade base and the compacted material from each other, protects the blade base, significantly reduces the wear rate of the blade base, thereby extending the service life of the blade, and is beneficial to large-scale promotion and application.

[0132] In addition, the present invention specifically limits the angle of the wear-resistant protrusion to the range of 30°-90°, which significantly improves the penetration of the wear-resistant protrusion on the compacted material, thereby more effectively breaking and removing the compacted material, while ensuring that the blade wears relatively evenly throughout its entire service life; the angle increases successively along the rotation direction of the spiral blade of the rotary hearth furnace, and the difference between the angles of adjacent wear-resistant protrusions is 5°-10°, so that the wear-resistant protrusion that is subjected to greater force has a higher angle, thereby further improving the wear uniformity of the wear-resistant protrusion.

[0133] Furthermore, the SiO2 powder contained in the activated powder and the induced powder can agglomerate with the hard particles during the sintering process and coat the surface of the hard particles to form a strong bonding interface, thereby improving the oxidation resistance and wear resistance of the wear-resistant protrusions in high temperature environments (above 1000°C). In the subsequent blade casting process, SiO2 is coated on the surface of the wear-resistant protrusions in the form of particles, further enhancing the wear resistance of the wear-resistant protrusions.

[0134] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A spiral blade of a rotary hearth furnace having a wear-resistant protrusion, characterized in that: The spiral blade of the rotary hearth furnace comprises a blade base, a wear-resistant protrusion embedded in the upper edge of the blade base, and a mounting portion penetrating the lower edge of the blade base; The hardness of the wear-resistant protrusion is greater than the hardness of the blade base; The upper edge of the blade base is the force-bearing part of the rotary hearth furnace spiral blade for scraping off the compacted matter; On each rotary hearth furnace spiral blade, the number of the wear-resistant protrusions is at least 3, and they are arranged in sequence along the upper edge of the blade base; The angle between the central axis symmetry line of the wear-resistant protrusion and the corresponding tangent line of the upper edge of the blade base is 30°-90°; along the rotation direction of the spiral blade of the rotary hearth furnace, the angle increases successively, and the difference between the angles of adjacent wear-resistant protrusions is 5°-10°; The method for preparing the wear-resistant protrusion comprises the following steps: (1) Mixing activated powder and hard particles and sintering at high temperature to obtain hard particles with surface metallization; (2) mixing the induction powder and the surface metallized hard particles obtained in step (1), preheating them in an oxygen-isolated environment, injecting alloy melt into them for sintering, and obtaining the wear-resistant protrusions; Wherein, the activated powder in step (1) and the induced powder in step (2) both contain SiO2 powder.

2. The rotary hearth furnace spiral blade according to claim 1, characterized in that: The wear-resistant protrusion is hidden inside the upper edge of the blade base and presents a smooth curved edge; Or, the wear-resistant protrusion is exposed outside the upper edge of the blade base body and presents a wavy edge or a serrated edge; The average height of the wavy edge or the serrated edge is 2-5 mm respectively.

3. The spiral blade of a rotary hearth furnace according to claim 1, characterized in that: The shape of the wear-resistant protrusion includes a cube and / or a frustum; The length of the cube is 30-50 mm, and the width and height are 10-30 mm respectively; The upper surface of the truncated table has a diameter of 20-40 mm, the lower surface has a diameter of 30-50 mm, and the height is 30-50 mm.

4. The spiral blade of a rotary hearth furnace according to claim 1, characterized in that: The activated powder in step (1) comprises SiO2 powder, MnFe powder, La2O3 powder and binder powder, and is obtained by ball milling and mixing; The mass ratio of the SiO2 powder, MnFe powder, La2O3 powder and binder powder is (1-3):(6-10):1:1; The ball milling is carried out in an industrial ball mill, and the ball milling time is 8-12 hours; The average particle size of the activated powder in step (1) is ≥400 mesh.

5. The rotary hearth furnace spiral blade according to claim 1, characterized in that: The hard particles in step (1) include any one of Al2O3, ZrO2, TiC, WC, Cr3C2, TiB ceramics, BN ceramics or ZTA ceramics, or a combination of at least two thereof; The average particle size of the hard particles in step (1) is 2-5 mm; The hard particles in step (1) are sequentially alkali washed and dried before mixing; The mixing time in step (1) is 6-10 hours; The high temperature sintering in step (1) is performed at a temperature of 1300-1400° C. and for a time of 1-2 hours.

6. The spiral blade of a rotary hearth furnace according to claim 1, characterized in that: The induced powder in step (2) includes SiO2 powder and MnFe powder; The mixing volume ratio of the induced powder and the hard particles in step (2) is 1:(3-5); In step (2), the oxygen-isolated environment is filled with argon gas; The temperature of the preheating treatment in step (2) is 900-1000°C; In terms of weight, the alloy melt in step (2) comprises the following components: The balance is Fe and inevitable impurities.

7. A method for preparing a spiral blade of a rotary hearth furnace according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (A) Make a foam model according to the blade drawing and embed the wear-resistant protrusions into the foam model; (B) embedding the foam model inlaid with wear-resistant protrusions obtained in step (A) into a sand mold and vibrating it, injecting alloy melt after evacuation, and obtaining a cast blade after cooling; (C) The as-cast blade obtained in step (B) is polished, quenched and air-cooled in sequence to obtain the rotary hearth furnace spiral blade.

8. The preparation method according to claim 7, characterized in that: Step (A) Before the wear-resistant raised portion is embedded, a blind hole to be embedded is cut on the upper edge of the foam model; The alloy melt in step (B) has the same composition as the alloy melt used in the process of preparing the wear-resistant protrusions.

9. The preparation method according to claim 7, characterized in that: The quenching temperature in step (C) is 950-1000°C and the holding time is 1-3h; The quenching and air cooling also include at least 2 temperings; The tempering temperature is 400-500°C; The air cooling adopts a graded cooling method.

10. An application of a spiral blade of a rotary hearth furnace as claimed in any one of claims 1 to 6, characterized in that: The spiral blades of the rotary hearth furnace are used to transport materials and scrape off the deposits on the furnace bottom.