A heterojunction composite material for piezoelectric photocatalysis and its preparation method and application

By constructing Cu9S5/Bi4O5Br2 heterojunction composite material, combining piezoelectric effect and photocatalysis, the problems of low photocatalyst efficiency and unutilized piezoelectric material potential are solved, and efficient organic pollutant degradation and good stability are achieved. .

CN118491539BActive Publication Date: 2024-11-19中国市政工程西北设计研究院有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410925364.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-19
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

The photocarrier recombination rate of existing photocatalysts is high during photocatalysis, resulting in low efficiency, and the potential of piezoelectric materials is not fully utilized, making it difficult to effectively degrade organic pollutants.

Method used

By constructing Cu9S5/Bi4O5Br2 heterojunction composite material, the unique layered structure and piezoelectric characteristics of Bi4O5Br2 are combined with the narrow band gap characteristics of Cu9S5 to form a photocatalytic system with piezoelectric effect to promote the separation of photogenerated charges and mass transfer.

Benefits of technology

The photocatalytic activity and pollutant degradation efficiency are significantly improved, the material is stable and reusable, covering the full visible spectrum, avoiding the electron-hole recombination problem in a single Cu9S5 material, and achieving efficient organic pollutant degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118491539B_ABST
    Figure CN118491539B_ABST
Patent Text Reader

Abstract

The invention discloses a heterojunction composite material for piezoelectric photocatalysis and a preparation method and application thereof, belonging to the field of photocatalysts. Preparation method: bismuth subsalicylate is dispersed in ethanol, and then potassium bromide is dissolved in ultrapure water; under stirring, potassium bromide solution is added dropwise to the bismuth subsalicylate dispersion, the pH value of the mixed solution is adjusted to 10.0-12.0, and a hydrothermal reaction is carried out after continuous stirring; after the reactant is cooled, it is filtered, washed, and dried to obtain a product Bi4O5Br2; Bi4O5Br2, copper acetylacetonate and polyvinyl pyrrolidone are dissolved in N,N-dimethylformamide and stirred; then ammonium sulfide is added to the mixture, and a crude product is obtained after continuous stirring; the crude product is centrifuged, washed, and dried to obtain a product Cu9S5 / Bi4O5Br2, i.e., a heterojunction composite material for piezoelectric photocatalysis. The application of the composite material in the degradation of organic pollutants in wastewater by piezoelectric photocatalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of photocatalysts, and in particular relates to a heterojunction composite material for piezoelectric photocatalysis and a preparation method and application thereof. Background Art

[0002] Based on copper sulfide (Cu x S y ) can effectively degrade organic pollutants. Although it has excellent optical absorption characteristics, its high photocarrier recombination rate limits its application. In order to improve its photocatalytic efficiency, researchers have carried out a series of screening, synthesis and modification of copper sulfide. However, simply modifying the photocatalyst is still not enough to effectively improve its photocatalytic effect. Therefore, it is possible to try to combine the photocatalyst with other technologies to stimulate their synergistic effect. Recently, researchers have found that piezoelectric catalysis induced by external mechanical stress can greatly improve the photocatalytic efficiency. Under the action of external mechanical stress, polarization occurs inside the piezoelectric material and a piezoelectric potential difference is generated. When the piezoelectric effect is combined with photocatalysis, the polarized charge in the piezoelectric material induces a polarized electric field, which can promote the migration and separation of photogenerated charges. At the same time, the piezoelectric effect can change the electronic state of the catalyst and the surrounding aqueous solution, prompting the charge in the catalyst to transfer to the solution at the solid-liquid interface, thereby enhancing the mass transfer in the piezoelectric photocatalytic system.

[0003] Bi4O5X2 (X = Br, I) from the layered Silleín structure family has a simple sandwich structure where [Bi4O5] 2+ There are strong ionic bonding interactions between the layers and the double halide ion plates, while there are van der Waals forces connecting the adjacent halide ion plates. Due to their unique layered crystal structure and narrow band gap, they have been widely used in photocatalytic applications. It is worth noting that Bi4O5X2 has an asymmetric crystal structure with a monoclinic space group P21 and has unique piezoelectric properties, which has the potential to convert mechanical energy into chemical energy through piezoelectric catalysis.

[0004] In recent years, photocatalysis has been considered as a promising and sustainable method to solve water pollution due to its advantages such as environmental protection and low cost. However, the efficiency of most photocatalysts is still low due to the poor light absorption ability of photocatalysts and the rapid recombination of photogenerated electron-hole pairs. Heterojunction engineering has become a promising strategy to improve the utilization capacity of photogenerated carriers and enhance photocatalytic activity. Heterojunction structure can regulate the band structure of materials, expand the light response range of materials, and promote the migration of carriers. It is one of the most effective ways to improve photocatalytic activity.

[0005] Copper sulfide (CuS, Cu2S, Cu9S5) powdered photocatalysts have narrow band gaps and excellent photoelectric response characteristics. Using Cu2O crystals as hard templates, Cu9S5 materials with various microstructures have been prepared based on ion exchange or Kirkendall effect, which have been used as core components of photocatalysts, batteries, supercapacitors and sensors. However, despite the highly active copper species and inherent stability of Cu9S5, its potential for application in advanced oxidation processes is often overlooked due to the rapid in-situ recombination of photogenerated carriers.

[0006] Among bismuth-rich bismuth oxybromide (Bi4O5Br2), it is regarded as an attractive photocatalytic material due to its unique sandwich structure, excellent chemical stability, good visible light harvesting ability and suitable band structure. The increase in Bi and O content will regulate the conductivity and valence band, which is beneficial to electron transport and improves the catalytic activity. In addition, it is expected to exhibit unique piezoelectric properties due to its non-centrosymmetric crystal structure (monoclinic system, space group P21). However, it is still challenging to develop efficient and stable catalysts. Therefore, constructing a heterojunction and combining the piezoelectric effect is a promising strategy to improve the catalytic performance. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing a heterojunction composite material for piezoelectric photocatalysis, so as to obtain a heterojunction catalytic material with piezoelectric effect, higher interface charge separation efficiency, simple preparation method, better stability, reusability, and capable of achieving piezoelectric photocatalytic degradation of organic pollutants.

[0008] Another object of the present invention is to provide a heterojunction composite material for piezoelectric photocatalysis.

[0009] The third object of the present invention is to provide an application of a heterojunction composite material for piezoelectric photocatalysis.

[0010] The technical solution of the present invention is: (one)

[0012] A method for preparing a heterojunction composite material for piezoelectric photocatalysis comprises the following steps:

[0013] A. First, bismuth subsalicylate (C7H5BiO4) is dispersed in ethanol by magnetic stirring, and then potassium bromide is dissolved in ultrapure water; under vigorous stirring, the potassium bromide solution is added dropwise to the bismuth subsalicylate dispersion, and the pH value of the mixed solution is adjusted to 10.0-12.0 by using HCl and NaOH, and after continuous stirring, the mixture is slowly transferred to a polytetrafluoroethylene-lined hydrothermal reactor for hydrothermal reaction; after the reactant is cooled, it is filtered, washed with deionized water and ethanol, and dried to obtain the product Bi4O5Br2;

[0014] B. Dissolve a certain amount of Bi4O5Br2, copper acetylacetonate and polyvinyl pyrrolidone in a certain volume of N,N-dimethylformamide and stir vigorously for several minutes; then add an appropriate amount of ammonium sulfide to the mixture, maintain a certain temperature and continue stirring to obtain a crude product; centrifuge the crude product, wash it with ethanol, acetone and deionized water for 3 to 6 times respectively, and dry it to obtain the product Cu9S5 / Bi4O5Br2, which is a heterojunction composite material for piezoelectric photocatalysis.

[0015] As a further improvement of the present invention, in step A, the molar ratio of bismuth subsalicylate to potassium bromide is 0.5-1:1.

[0016] As a further improvement of the present invention, in step A, the temperature of the hydrothermal reaction is 100-140° C., and the time of the hydrothermal reaction is 10-14 h.

[0017] As a further improvement of the present invention, in step A, the drying temperature is 60-80° C., and the drying time is 12-24 hours.

[0018] As a further improvement of the present invention, in step B, the mass ratio of Bi4O5Br2, copper acetylacetonate and polyvinyl pyrrolidone is 5-10:5:8.

[0019] As a further improvement of the present invention, in step B, the temperature is maintained at 160-180° C. during continuous stirring, and magnetic stirring is performed for 6-8 h.

[0020] As a further improvement of the present invention, in step B, the drying temperature is 40-60° C., and the drying time is 12-24 h. (two)

[0022] A heterojunction composite material for piezoelectric photocatalysis is prepared by the above-mentioned preparation method of a heterojunction composite material for piezoelectric photocatalysis. (three)

[0024] The invention discloses an application of a heterojunction composite material for piezoelectric photocatalysis in the piezoelectric photocatalytic degradation of organic pollutants in wastewater.

[0025] A further organic pollutant is bisphenol A.

[0026] The beneficial effects of the present invention are as follows: the present invention compounds Bi4O5Br2 and Cu9S5 by constructing a heterojunction, thereby constructing a photocatalytic nanocomposite material, Cu9S5 / Bi4O5Br2, which has piezoelectric effect, stronger interface carrier separation ability, light absorption range covering the entire visible spectrum, and higher catalytic activity. Cu9S5 is a semiconductor catalytic material with optical absorption in the near-infrared region and a narrow band gap, but the charge separation efficiency of a single material is low; the Bi4O5Br2 material has a unique layered crystal structure, good visible light absorption and a suitable energy band structure, and is considered to be a photocatalytic material with good application prospects, and the non-centrosymmetric structure of Bi4O5Br2 gives it unique piezoelectric properties, but this property is often ignored by researchers, resulting in its potential as a piezoelectric body not being fully utilized. By combining Bi4O5Br2 and Cu9S5, the photogenerated electron-hole pairs of Cu9S5 / Bi4O5Br2 composite photocatalytic nanomaterials were successfully separated at the heterogeneous interface, avoiding the electron-hole recombination problem in the band gap of single Cu9S5 catalytic nanomaterials. Under the action of external mechanical stress, the piezoelectric material Bi4O5Br2 was polarized and a piezoelectric potential difference was generated. When the piezoelectric effect was combined with photocatalysis, the polarized charges in the piezoelectric material induced the generation of a polarized electric field, which can promote the migration and separation of photogenerated charges. The construction of a heterojunction more effectively enhances the charge separation and electron transfer at the heterojunction interface, greatly improving the photocatalytic activity. Finally, the Cu9S5 / Bi4O5Br2 piezoelectric photocatalytic system achieved effective pollutant degradation, and was characterized by good stability and reusability. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a scanning electron microscope image of Cu9S5 / Bi4O5Br2 prepared in Example 1 of the present invention;

[0028] Figure 2 The ultraviolet diffuse reflectance spectra of Cu9S5 / Bi4O5Br2, Bi4O5Br2 and Cu9S5 prepared in Example 1 and Comparative Examples 1 and 2 of the present invention are shown;

[0029] Figure 3 Fourier diffuse reflectance infrared spectra of Cu9S5 / Bi4O5Br2, Bi4O5Br2, and Cu9S5 prepared in Example 1 and Comparative Examples 1 and 2 of the present invention;

[0030] Figure 4 The butterfly amplitude loop and phase hysteresis loop of Cu9S5 / Bi4O5Br2 prepared in Example 1 of the present invention;

[0031] Figure 5This is a performance comparison chart of the piezoelectric photocatalytic degradation of bisphenol A by Cu9S5 / Bi4O5Br2, Bi4O5Br2, and Cu9S5 prepared in Example 1 of the present invention and Comparative Examples 1 and 2;

[0032] Figure 6 This is a degradation diagram of the reusability experiment of the piezoelectric photocatalytic degradation of bisphenol A by Cu9S5 / Bi4O5Br2 prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0034] Embodiment 1,

[0035] A method for preparing a heterojunction composite material for piezoelectric photocatalysis comprises the following steps:

[0036] A. First, 0.5 mmol bismuth subsalicylate (C7H5BiO4) was dispersed in 40 mL ethanol by magnetic stirring, and then 1 mmol potassium bromide was dissolved in 40 mL ultrapure water; under 600 r / min magnetic stirring, the potassium bromide solution was added dropwise to the bismuth subsalicylate dispersion, and then the pH value of the mixture was adjusted to 11.0 using HCl and NaOH. After continuous stirring, the mixture was slowly transferred to a polytetrafluoroethylene-lined hydrothermal reactor for hydrothermal reaction at 120°C for 12 h; after the reactant was cooled, it was filtered, washed with deionized water and ethanol, and dried in an oven at 60°C for 12 h to obtain the product Bi4O5Br2.

[0037] B. Dissolve 100 mg Bi4O5Br2, 50 mg copper acetylacetonate and 80 mg polyvinylpyrrolidone in 10 ml N,N-dimethylformamide and stir vigorously at 600 r / min for 10 minutes. Then add 1 ml ammonium sulfide to the mixture and stir magnetically at 170 °C for 7 hours to obtain a crude product. Centrifuge the crude product, wash it with ethanol, acetone and deionized water for 3-6 times respectively, and dry it at 40 °C for 24 hours to obtain the product Cu9S5 / Bi4O5Br2, which is a heterojunction composite material for piezoelectric photocatalysis.

[0038] Figure 1 This is a scanning electron microscope image of Cu9S5 / Bi4O5Br2 prepared in Example 1 of the present invention. Figure 1 As shown, the Cu9S5 / Bi4O5Br2 composite photocatalytic nanomaterial is a layer-by-layer stacked nanosheet structure.

[0039] Embodiment 2,

[0040] A method for preparing a heterojunction composite material for piezoelectric photocatalysis comprises the following steps:

[0041] A. First, 1.0 mmol of bismuth subsalicylate (C7H5BiO4) was dispersed in 40 mL of ethanol by magnetic stirring, and then 1 mmol of potassium bromide was dissolved in 40 mL of ultrapure water. Under magnetic stirring at 600 r / min, the potassium bromide solution was added dropwise to the bismuth subsalicylate dispersion. Subsequently, the pH value of the mixture was adjusted to 10.0 using HCl and NaOH. After continuous stirring, the mixture was slowly transferred to a polytetrafluoroethylene-lined hydrothermal reactor for hydrothermal reaction at 100°C for 14 h. After the reactants were cooled, they were filtered, washed with deionized water and ethanol, and dried in an oven at 80°C for 12 h to obtain the product Bi4O5Br2.

[0042] B. Dissolve 50 mg Bi4O5Br2, 50 mg copper acetylacetonate and 80 mg polyvinylpyrrolidone in 20 ml N,N-dimethylformamide and stir vigorously at 600 r / min for 10 minutes; then add 2 ml ammonium sulfide to the mixture and magnetically stir at 160 °C for 8 hours to obtain a crude product; centrifuge the crude product, wash it with ethanol, acetone and deionized water for 3-6 times respectively, and dry it at 60 °C for 12 h to obtain the product Cu9S5 / Bi4O5Br2, which is a heterojunction composite material for piezoelectric photocatalysis.

[0043] Embodiment 3,

[0044] A method for preparing a heterojunction composite material for piezoelectric photocatalysis comprises the following steps:

[0045] A. First, 0.75 mmol bismuth subsalicylate (C7H5BiO4) was dispersed in 40 mL ethanol by magnetic stirring, and then 1 mmol potassium bromide was dissolved in 40 mL ultrapure water. Under magnetic stirring at 600 r / min, the potassium bromide solution was added dropwise to the bismuth subsalicylate dispersion. Subsequently, the pH value of the mixture was adjusted to 12.0 using HCl and NaOH. After continuous stirring, the mixture was slowly transferred to a polytetrafluoroethylene-lined hydrothermal reactor for hydrothermal reaction at 140°C for 10 h. After the reactants were cooled, they were filtered, washed with deionized water and ethanol, and dried in an oven at 80°C for 24 h to obtain the product Bi4O5Br2.

[0046] B. Dissolve 75 mg Bi4O5Br2, 50 mg copper acetylacetonate and 80 mg polyvinylpyrrolidone in 15 ml N,N-dimethylformamide and stir vigorously at 600 r / min for 10 minutes. Then add 1.5 ml ammonium sulfide to the mixture and magnetically stir at 180 °C for 6 hours to obtain a crude product. Centrifuge the crude product, wash it with ethanol, acetone and deionized water for 3-6 times respectively, and dry it at 50 °C for 18 hours to obtain the product Cu9S5 / Bi4O5Br2, which is a heterojunction composite material for piezoelectric photocatalysis.

[0047] Comparative Example 1

[0048] Only Bi4O5Br2 was prepared: first, 0.5 mmol bismuth subsalicylate (C7H5BiO4) was dispersed in 40 mL of ethanol by magnetic stirring, and then 1 mmol potassium bromide was dissolved in 40 mL of ultrapure water; under magnetic stirring at 600 r / min, the potassium bromide solution was added dropwise to the bismuth subsalicylate dispersion, and then the pH value of the mixture was adjusted to 11.0 using HCl and NaOH. After continuous stirring, the mixture was slowly transferred to a polytetrafluoroethylene-lined hydrothermal reactor for hydrothermal reaction at 120°C for 12 h; after the reactant was cooled, it was filtered, washed with deionized water and ethanol, and dried in an oven at 60°C for 12 h to obtain the product Bi4O5Br2.

[0049] Comparative Example 2

[0050] Preparation of Cu9S5 only: 50 mg of copper acetylacetonate and 80 mg of polyvinylpyrrolidone were dissolved in 10 ml of N,N-dimethylformamide and stirred vigorously at 600 r / min for 10 minutes; then 1 ml of ammonium sulfide was added to the mixture and the crude product was obtained after magnetic stirring at 170°C for 7 hours; the crude product was centrifuged and washed with ethanol, acetone and deionized water for 3-6 times respectively, and dried at 40°C for 24 hours to obtain the product Cu9S5.

[0051] 1. Evaluation of photocatalytic degradation performance

[0052] The photocatalytic degradation performance of the catalysts prepared in Example 1 and Comparative Examples 1 and 2 was evaluated as follows:

[0053] Mechanical vibration was provided by an ultrasonic cleaner (40 kHz, 100 W, Jielimei, Kunshan, China), and visible light irradiation (λ>420 nm, Beijing Zhongjiao Jinyuan Technology Co., Ltd.) was simulated by a 300 W xenon lamp. Before irradiation, a solution (100 mL) containing the catalyst (0.1 g / L) and the pollutant (5 mg / L) was placed in a beaker and mechanically stirred for 30 min in the dark to reach adsorption-desorption equilibrium. The beaker was then placed in an ultrasonic cleaner, and ultrasonic vibration (US) and simulated sunlight (SL) were turned on. Ice bags were placed in the ultrasonic cleaner to keep the temperature at around 25 ± 5 °C. At given time intervals, 1 mL of the solution was taken and immediately filtered with a 0.22 μm syringe filter for detection. The concentration of bisphenol A (BPA) was measured by HPLC (Shimadzu, LC-16) using an Agilent SB-C18 column (2.1 mm × 100 mm, 1.8 μm) with a UV detector at 278 nm. The mobile phase was acetonitrile and ultrapure water with a volume ratio of 50:50. The relative concentration (C / C0) was used to calculate the degradation efficiency.

[0054] Figure 2 The ultraviolet diffuse reflectance spectra of Cu9S5 / Bi4O5Br2, Bi4O5Br2, and Cu9S5 prepared in Example 1 and Comparative Examples 1 and 2 of the present invention are shown in FIG. Figure 2 As shown, Bi4O5Br2 exhibits light absorption in the ultraviolet and visible light regions with an absorption edge of ~450nm, while Cu9S5 has strong absorption throughout the entire visible spectrum. At the same time, for Cu9S5 / Bi4O5Br2, it can be seen that the composite of Cu9S5 effectively enhances the tail peak intensity of the material, indicating that the two form complementary light absorption, which is beneficial to improving the visible light capture efficiency.

[0055] Figure 3 Fourier diffuse reflectance infrared spectra of Cu9S5 / Bi4O5Br2, Bi4O5Br2, and Cu9S5 prepared in Example 1 and Comparative Examples 1 and 2 of the present invention. For Bi4O5Br2, at 446 cm -1 There is an absorption peak at 3425 cm −1 The peak corresponds to the stretching vibration of the hydroxyl group. For Cu9S5, 550 cm −1 The peak at 1072 cm is the stretching vibration peak of Cu-S. −1 The peaks at 1522 and 3427 cm-1 match the CO stretching vibrations. −1The two groups of spectral bands correspond to the stretching vibration and deformation vibration of hydroxyl groups, respectively. It is worth mentioning that the main typical absorption peaks of the original Bi4O5Br2 and Cu9S5 are present in the Cu9S5 / Bi4O5Br2 sample, which further indicates the successful synthesis of the Cu9S5 / Bi4O5Br2 composite catalyst.

[0056] Figure 4 The butterfly amplitude loop and phase hysteresis loop of Cu9S5 / Bi4O5Br2 prepared in Example 1 of the present invention. For Cu9S5 / Bi4O5Br2, the piezoelectric coefficient calculated from the amplitude-voltage curve is 34.33 pm / V, indicating that the material has certain piezoelectric properties.

[0057] Figure 5 The performance comparison diagram of the piezoelectric photocatalytic degradation of bisphenol A by Cu9S5 / Bi4O5Br2, Bi4O5Br2, and Cu9S5 prepared in Example 1 of the present invention and Comparative Examples 1 and 2. The experiment was carried out under the conditions of a catalyst dosage of 0.1 g / L, an initial concentration of bisphenol A of 5 mg / L, and an initial temperature of room temperature. The experimental results show that when only ultrasound is used to provide external mechanical stress to simulate piezoelectric catalysis (without light), the degradation efficiency of single Cu9S5 on bisphenol A is only 17.69%, which indicates that Cu9S5 has no piezoelectric effect, and the only degradation may be due to the complexation of Cu (II) with pollutants. The degradation rate of single Bi4O5Br2 on bisphenol A under piezoelectric catalysis is 37.11%, which indicates that the internal polarization electric field formed by the asymmetric center induced by external mechanical stress causes electrons to be quickly transferred to the surface of the pollutant, which means that single Bi4O5Br2 is a piezoelectric catalytic material with good performance. Under the action of piezoelectric and visible light, the degradation rates of bisphenol A by single Cu9S5 and Bi4O5Br2 were 38.01% and 59.57%, respectively, which indicates that photocatalysis can further induce the generation of photogenerated electron-hole pairs, thereby accelerating the degradation efficiency of pollutants, but the removal effect is poor due to the rapid in-situ recombination of carriers. Under the action of piezoelectric-visible light catalysis, the degradation efficiency of pollutants by Cu9S5 / Bi4O5Br2 composite material reached 91.07% within 30 min, which indicates that photogenerated electrons migrate rapidly across heterogeneous interfaces under the action of polarized electric fields, further accelerating the degradation efficiency of pollutants. At the same time, in the absence of light, the degradation efficiency of pollutants by Cu9S5 / Bi4O5Br2 composite material was only 25.67%, which means that piezoelectric catalysis alone cannot achieve good degradation of bisphenol A.

[0058] 2. Continuous degradation experiment

[0059] After the first degradation reaction of Cu9S5 / Bi4O5Br2 prepared in Example 1 is completed, the solution after the reaction is centrifuged and washed, and the recovered catalyst is dried in a freeze dryer for 48 h, and then put into the reactor again for the next degradation experiment. Except for the materials, the other degradation reaction conditions are consistent with the setting procedures of the first photocatalytic degradation performance evaluation experiment; after the second reaction is completed, the above steps are repeated to carry out three degradation experiments.

[0060] Figure 6 This is a degradation diagram of the reusability experiment of Cu9S5 / Bi4O5Br2 piezoelectric photocatalytic degradation of bisphenol A prepared in Example 1 of the present invention. In three consecutive degradation experiments, the degradation efficiency of bisphenol A was above 90%, which shows that the photocatalytic activity of Cu9S5 / Bi4O5Br2 photocatalytic nanomaterials remains good after three cycles.

[0061] The present invention synthesizes a Cu9S5 / Bi4O5Br2 S-type heterojunction, which degrades the pollutant bisphenol A under the assistance of ultrasonic vibration and visible light. Among them, Bi4O5Br2 has an asymmetric crystal structure and exhibits unique piezoelectric properties. The close contact between Bi4O5Br2 and Cu9S5 can construct an S-type heterojunction, further promoting the effective separation of photogenerated carriers.

[0062] Organic pollutants in wastewater include but are not limited to bisphenol A, carbamazepine, atrazine, tetracycline, rhodamine B, etc. Preferably, the Cu9S5 / Bi4O5Br2 of the present invention has an exceptionally excellent degradation effect on bisphenol A under piezoelectric photocatalytic conditions. On the one hand, under visible light irradiation, the photocatalytic materials Cu9S5 / Bi4O5Br2 are photoexcited to generate photogenerated electrons and photogenerated holes. The matching energy level positions enable the photogenerated electrons in the conduction band of Cu9S5 to transfer to the valence band of Bi4O5Br2 across the heterojunction interface. This S-type charge transfer mechanism not only promotes carrier separation, but also retains strong redox ability. On the other hand, under the mechanical stress of ultrasonic vibration, the piezoelectric catalytic material Bi4O5Br2 generates a unidirectional polarized electric field, resulting in the formation of a polarized charge layer at the contact interface with the photocatalytic material Cu9S5, and inducing the bending of the surface energy band of the piezoelectric catalytic material Bi4O5Br2, which further induces the migration of electrons from Cu9S5 to Bi4O5Br2. The transfer of electrons across the interface will effectively inhibit the recombination of electron-hole pairs, thereby significantly improving the charge separation efficiency. Finally, the pollutants are oxidized by surface active oxygen or hydroxyl groups and holes, and finally generate water and carbon dioxide.

[0063] The present invention prepares Cu9S5 / Bi4O5Br2 piezoelectric photocatalytic composite nanomaterials by a solvothermal method. The simple preparation method and excellent photocatalytic performance make the catalyst an effective material for wastewater purification. In addition, the prepared sample has good stability and can be recycled, and has potential application value in the field of wastewater purification.

Claims

1. A method for preparing a heterojunction composite material for piezoelectric photocatalysis, characterized in that The following steps are involved: A. First, bismuth subsalicylate is dispersed in ethanol, and then potassium bromide is dissolved in ultrapure water; under stirring, the potassium bromide solution is added dropwise to the bismuth subsalicylate dispersion, the pH value of the mixed solution is adjusted to 10.0-12.0, and a hydrothermal reaction is carried out after continuous stirring, the temperature of the hydrothermal reaction is 100-140° C., and the time of the hydrothermal reaction is 10-14 hours; after the reactant is cooled, it is filtered, washed, and dried to obtain the product Bi4O5Br2; B. Dissolve Bi4O5Br2, copper acetylacetonate and polyvinyl pyrrolidone in N,N-dimethylformamide and stir; then add ammonium sulfide to the mixture, maintain the temperature at 160-180°C, and magnetically stir for 6-8 hours to obtain a crude product; centrifuge the crude product, wash, and dry to obtain the product Cu9S5 / Bi4O5Br2, which is a heterojunction composite material for piezoelectric photocatalysis.

2. The method for preparing a heterojunction composite material for piezoelectric photocatalysis according to claim 1, characterized in that: In step A, the molar ratio of bismuth subsalicylate to potassium bromide is 0.5-1:

1.

3. The method for preparing a heterojunction composite material for piezoelectric photocatalysis according to claim 1, characterized in that: In step A, the drying temperature is 60-80°C and the drying time is 12-24h.

4. The method for preparing a heterojunction composite material for piezoelectric photocatalysis according to claim 1, characterized in that: In step B, the mass ratio of Bi4O5Br2, copper acetylacetonate and polyvinyl pyrrolidone is 5-10:5:

8.

5. The method for preparing a heterojunction composite material for piezoelectric photocatalysis according to claim 1, characterized in that: In step B, the drying temperature is 40-60°C and the drying time is 12-24h.

6. A heterojunction composite material for piezoelectric photocatalysis, characterized in that: The composite material is prepared by the method for preparing a heterojunction composite material for piezoelectric photocatalysis according to any one of claims 1 to 5.

7. Use of the heterojunction composite material for piezoelectric photocatalysis according to claim 6 in piezoelectric photocatalytic degradation of organic pollutants in wastewater.

8. The use of a heterojunction composite material for piezoelectric photocatalysis according to claim 7, characterized in that: The organic pollutant is bisphenol A.