A gas shielded welding wire with functional coating and preparation method thereof

By coating the gas shielded welding wire with functional coatings of graphene, polythiophene and other materials, the problem of welding instability caused by defects in the copper plating layer is solved, the welding quality and efficiency are improved, and the purity and conductivity of the weld are achieved. sex.

CN118492745BActive Publication Date: 2024-10-29TIANJIN GOLDEN BRIDGE WELDING MATERIALS GRP CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410744234.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-29
Estimated Expiration
2044-06-11

AI Technical Summary

Technical Problem

Defects in the copper-plated layer during gas shielded welding can easily lead to fluctuations in the contact resistance between the welding wire and the contact tip, causing arc instability, affecting welding quality and work efficiency, and easily causing metal spatter and an increase in inclusions.

Method used

Use gas shielded welding wire with functional coating. The coating is composed of materials such as graphene, polythiophene, potassium oleate, sodium oleate and triethanolamine borate. It improves the density and adhesion of the surface of the welding wire through conductivity and lubricity. The connection effect stabilizes the arc and reduces spatter.

Benefits of technology

It improves arc stability and weld purity during the welding process, reduces spatter and inclusions, and improves welding quality and work efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention provides a gas shielded welding wire with a functional coating, comprising a welding wire, wherein the surface of the welding wire is provided with a functional coating; the functional coating is made of the following raw materials in parts by weight: 1-15 parts of potassium oleate, 2-15 parts of sodium oleate, 1-10 parts of triethanolamine borate, and 60-96 parts of a carrier. The gas shielded welding wire with a functional coating of the present invention is subjected to a coating treatment on the surface of the copper-plated welding wire, wherein the coating has a deoxidation effect during the welding process, optimizes the purity of molten iron, and enhances the fluidity of molten iron, and the special coating also has the effects of improving the conductivity of the welding wire, stabilizing the arc, and reducing spatter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of welding wires, and in particular relates to a gas shielded welding wire with a functional coating. Background Art

[0002] Gas shielded welding is an efficient welding technology. It has been rapidly developed at home and abroad due to its advantages of high production efficiency, strong process adaptability and low welding cost. At present, it has become one of the most important welding methods for metal materials such as low carbon steel, low alloy steel, copper and nickel. It is widely used in many industries such as shipbuilding, pressure vessels, vehicles, construction engineering, mining machinery, steel structure, petrochemicals, bridges, etc., and has achieved good social and economic benefits. However, there are still some problems that need to be solved in the production and use of gas shielded welding, such as defects in the copper plating layer, the surface copper layer is not dense and uniform, causing the steel welding wire matrix to be exposed and directly contacted with the outside world, which will cause the contact resistance between the welding wire and the conductive nozzle to fluctuate. In severe cases, it will cause arc instability, affect the gas protection effect, increase the oxygen content in the weld, increase the inclusions in the weld, and cause more metal spatter, affecting the welding quality and work efficiency. Summary of the invention

[0003] In view of this, the present invention aims to overcome the defects in the prior art and provides a gas shielded welding wire with a functional coating.

[0004] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0005] A gas shielded welding wire with a functional coating, comprising a welding wire, wherein the surface of the welding wire is provided with a functional coating;

[0006] The functional coating is made of the following raw materials in parts by weight:

[0007]

[0008] Furthermore, the coating amount of the functional coating is 0.4-2.0 g / m 2 .

[0009] Furthermore, the carrier is made of the following raw materials in parts by weight: 2-8 parts of graphene, 1-7 parts of polythiophene, and 45-93 parts of water. The carrier is made of a mixture of graphene, polythiophene and water.

[0010] Furthermore, the particle size of the graphene is less than or equal to 10 nanometers; and the particle size of the polythiophene is less than or equal to 300 nanometers.

[0011] Furthermore, the welding wire is a copper-plated welding wire.

[0012] Furthermore, the diameter of the welding wire is 0.8-1.6 mm.

[0013] The method for preparing the gas shielded welding wire with a functional coating comprises the following steps: coating the functional coating on the surface of the welding wire.

[0014] The graphene in the carrier is an allotrope of carbon with excellent electrical conductivity. Polythiophene is a conductive polymer, a high molecular compound formed by the polymerization of thiophene, so the carrier has a good conductive effect. Countless tiny molecular tentacles will be generated in the carrier, so that they are firmly and quickly distributed on the surface of the steel wire, forming a dense conductive network on the surface of the coating, so it has a good bonding effect with the welding wire, and the composition is uniform and the structure is stable, so it can be evenly coated on the surface of the welding wire. However, if the amount added is too large, the coating will form a slag shell attached to the surface of the welding wire, resulting in poor bonding with the welding wire.

[0015] Potassium and sodium elements can make the arc transition to openness, increase the axial electromagnetic force, facilitate the smooth detachment of the molten droplet from the end of the welding wire, and improve the effective ionization degree of the arc, so that the arc remains soft and smooth, stabilize the arc, reduce spatter, and ensure welding quality. Additives potassium oleate and sodium oleate contain certain potassium and sodium elements, which have been proven to have the above functions through a large number of experiments. In addition to the above functions, potassium oleate is a surface-active compound, and sodium oleate is an excellent emulsifier. The combination of these two substances on the surface of the welding wire also has good lubricity. However, if the content is too high, the welding smoke will increase accordingly, so it should be controlled within a certain range.

[0016] Triethanolamine borate contains boron, which can improve the strength and hardness of weld metal when entering the weld metal. It also has the effect of reducing the surface tension of molten iron and improving the fluidity of molten iron. At the same time, it can effectively absorb oxygen, reduce the impurity content in the weld, and improve the welding quality. Triethanolamine boric acid is also an excellent lubricant. However, while boron improves the strength of weld metal, it also reduces its toughness. In order to balance the strength and toughness of welding materials, its content needs to be properly controlled.

[0017] During welding, the functional coating is continuously brought into the welding area along with the welding wire, playing a role in deoxidation, optimizing the purity of molten iron, and enhancing the fluidity of molten iron, thereby achieving the effect of improving the conductivity of the welding wire, stabilizing the arc, and reducing spatter.

[0018] Compared with the prior art, the present invention has the following advantages:

[0019] The gas shielded welding wire with functional coating described in the present invention is coated on the surface of the copper-plated welding wire. The coating has a deoxidation effect during the welding process, and can optimize the purity of molten iron and enhance the fluidity of molten iron. The special coating also has the effects of improving the conductivity of the welding wire, stabilizing the arc, and reducing spatter. DETAILED DESCRIPTION

[0020] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0021] The present invention will be described in detail below with reference to the embodiments.

[0022] Example 1

[0023] A method for preparing a gas shielded welding wire with a functional coating comprises the following steps: applying the functional coating to the surface of the copper-plated gas shielded welding wire, wherein the copper-plated gas shielded welding wire model is ER70S-6, the welding wire specification is 1.2 mm, and the coating amount is 0.8 g / m 2 .

[0024] The functional coating is made of the following raw materials in parts by weight: 5 parts of potassium oleate, 8 parts of sodium oleate, 4 parts of triethanolamine borate, 3 parts by weight of graphene, 2 parts by weight of polythiophene, and 78 parts by weight of water.

[0025] Example 2

[0026] A method for preparing a gas shielded welding wire with a functional coating comprises the following steps: applying the functional coating to the surface of the copper-plated gas shielded welding wire, wherein the copper-plated gas shielded welding wire model is ER70S-6, the welding wire specification is 1.2 mm, and the coating amount is 1.3 g / m 2 .

[0027] The functional coating is made of the following raw materials in parts by weight: 7 parts of potassium oleate, 9 parts of sodium oleate, 6 parts of triethanolamine borate, 3 parts by weight of graphene, 2 parts by weight of polythiophene, and 73 parts by weight of water.

[0028] Example 3

[0029] A method for preparing a gas shielded welding wire with a functional coating comprises the following steps: applying the functional coating to the surface of the copper-plated gas shielded welding wire, wherein the copper-plated gas shielded welding wire model is ER70S-6, the welding wire specification is 1.2 mm, and the coating amount is 1.7 g / m 2 .

[0030] The functional coating is made of the following raw materials in parts by weight: 11 parts of potassium oleate, 13 parts of sodium oleate, 8 parts of triethanolamine borate, 3 parts by weight of graphene, 2 parts by weight of polythiophene, and 63 parts by weight of water.

[0031] Example 4

[0032] A method for preparing a gas shielded welding wire with a functional coating comprises the following steps: applying the functional coating to the surface of the copper-plated gas shielded welding wire, wherein the copper-plated gas shielded welding wire model is ER70S-6, the welding wire specification is 1.0 mm, and the coating amount is 1.2 g / m 2 .

[0033] The functional coating is made of the following raw materials in parts by weight: 6 parts of potassium oleate, 10 parts of sodium oleate, 3 parts of triethanolamine borate, 3 parts of graphene, 2 parts of polythiophene, and 76 parts of water.

[0034] Example 5

[0035] A method for preparing a gas shielded welding wire with a functional coating comprises the following steps: applying the functional coating to the surface of the copper-plated gas shielded welding wire, wherein the copper-plated gas shielded welding wire model is ER70S-6, the welding wire specification is 1.6 mm, and the coating amount is 0.9 g / m 2 .

[0036] The functional coating is made of the following raw materials in parts by weight: 7 parts of potassium oleate, 12 parts of sodium oleate, 8 parts of triethanolamine borate, 6 parts by weight of graphene, 4 parts by weight of polythiophene, and 63 parts by weight of water.

[0037] Comparative Example 1

[0038] The only difference from Example 1 is that: a common copper-plated gas shielded welding wire model ER70S-6 is used, the welding wire specification is 1.2 mm, and there is no functional coating.

[0039] Comparative Example 2

[0040] The difference from Example 1 is only that: 17 parts of potassium oleate.

[0041] Comparative Example 3

[0042] The difference from Example 1 is only that: 18 parts of sodium oleate.

[0043] Comparative Example 4

[0044] The only difference from Example 1 is that: 12 parts of triethanolamine borate.

[0045] Comparative Example 5

[0046] The only difference from Example 1 is that the weight parts of graphene are 9 parts, the weight parts of polythiophene are 8 parts, and the weight parts of water are 66 parts.

[0047] Comparative Example 6

[0048] The only difference from Example 1 is that the coating amount is 2.4 g / m 2 .

[0049] The welding wires obtained in each embodiment and each comparative example were tested, as follows:

[0050] Welding material model: G49A4UC1S6.

[0051] Welding specifications: welding speed 5-6mm / s; gas flow 15-25L / min; current: 280-300A; voltage: 28-32V, shielding gas: 100% CO2.

[0052] The mechanical properties of the deposited metal are shown in Table 1.

[0053] Table 1 Mechanical properties of deposited metal

[0054]

[0055]

[0056] The performance of all the 11 groups of products except Comparative Example 4# meets the requirements. The low impact value and elongation value of Comparative Example 4 are mainly due to the high boron content in the coating composition, which increases the brittle and hard phase of the weld metal and leads to poor plasticity and toughness.

[0057] A comparative analysis of the 11 welding wire groups was conducted in terms of arc stability, spatter volume, inclusion content, molten iron fluidity and welding fume. The experimental results are shown in Table 2.

[0058] Table 2 Welding process performance

[0059]

[0060]

[0061] Note:

[0062] 1. Arc stability: The current and voltage stability is evaluated through the feedback of the high-speed photography system, and the grades are divided into excellent, good, qualified and unqualified.

[0063] 2. Spatter amount: The welding time is 2 minutes, and the copper box is used to collect the welding spatter and weigh it.

[0064] 3. Inclusions: Conduct radiographic testing to determine the number of inclusions.

[0065] 4. Molten iron fluidity: The molten iron fluidity is evaluated by measuring the surface width of the weld.

[0066] 5. Welding fume: The fume of the sample is collected and weighed by a vacuum fume collector, and the percentage of its weight to the mass of the sample is calculated.

[0067] Compared with the ordinary product of Comparative Example 1, the product of Example 5 has more ideal welding process performance in all aspects, with stable welding arc, small spatter, level I radiographic flaw detection, good molten iron fluidity, and small welding smoke. Comparative Examples 2, 3, and 6 have significantly increased welding smoke because the coating composition or coating amount is not within the appropriate range. Comparative Example 5 has poor bonding between the coating and the surface of the welding wire due to the excessively high content of graphene and polythiophene, resulting in poor welding processability.

[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A gas shielded welding wire with a functional coating, Features: It comprises a welding wire, the surface of which is provided with a functional coating; The functional coating is made of the following raw materials in parts by weight: 1-15 parts of potassium oleate, 2-15 parts of sodium oleate, 1-10 parts of triethanolamine borate, and 60-96 parts of a carrier; The carrier is made of raw materials including the following parts by weight: 2-8 parts of graphene, 1-7 parts of polythiophene, and 45-93 parts of water.

2. The gas shielded welding wire with functional coating according to claim 1, Features: The coating amount of the functional coating is 0.4-2.0g / m 2 .

3. The gas shielded welding wire with functional coating according to claim 1, Features: The particle size of the graphene is less than or equal to 10 nanometers; the particle size of the polythiophene is less than or equal to 300 nanometers.

4. The gas shielded welding wire with functional coating according to claim 1, Features: The welding wire is a copper-plated welding wire.

5. The gas shielded welding wire with functional coating according to claim 1, Features: The diameter of the welding wire is 0.8-1.6 mm.

6. A method for preparing a gas shielded welding wire with a functional coating according to any one of claims 1 to 5, Features: The method comprises the following steps: coating the functional coating on the surface of the welding wire.

Citation Information

Patent Citations

  • Welding electrode with functional coatings

    CA3175022A1

  • Gas protecting welding wire with nano-coating

    CN101407004A