A method for preparing graphene with controllable angle assisted by Raman

By combining Raman surface scanning with peak area imaging and mechanical exfoliation, the problems of insufficient resolution for graphene edge identification and uncontrollable rotation angle in traditional methods have been solved. This has enabled efficient and accurate preparation of graphene with controllable rotation angle, simplifying the preparation process and improving sample quality.

CN118495524BActive Publication Date: 2024-11-22SUN YAT SEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410765092.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-11-22
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

Existing technologies struggle to efficiently and accurately prepare controllable twisted graphene, especially in the preparation of large-area twisted graphene. Traditional methods are complex to operate and easily damage the crystal quality of the sample, and their resolution is insufficient when Raman spectroscopy is used to identify the edges of graphene.

Method used

The edges of graphene were identified by Raman surface scanning combined with peak area imaging. By combining mechanical exfoliation and transfer techniques and adjusting the Raman experimental conditions and substrate selection, efficient identification of graphene edges and precise control of rotation angles were achieved.

Benefits of technology

It enables efficient identification and precise rotation control of graphene sample edges, simplifies the preparation process, improves preparation efficiency and sample quality, is compatible with a variety of substrates, and reduces dependence on precision equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118495524B_ABST
    Figure CN118495524B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing graphene with controllable angle by Raman assistance, the method comprising the following steps: mechanically exfoliating on a substrate 2 and a PMMA / PVA / silicon oxide substrate to obtain graphene, the substrate 2 being a silicon oxide wafer or a silicon oxide wafer spin-coated with PVA; and identifying the crystallographic edge type of the obtained graphene sample by a Raman scanning peak area imaging method; dissolving PVA in PMMA / PVA / silicon oxide with deionized water to obtain a PMMA suspended film loaded with graphene; placing the PMMA suspended film loaded with graphene and the substrate 2 with graphene on the upper and lower sides of a two-dimensional material transfer sample stage; setting the angle of rotation by the sample stage, and fitting the two graphene samples to achieve the preparation of graphene samples with controllable angle. The present invention pre-judges the crystallographic edge of the graphene sample by selecting the graphene sample and adjusting the Raman experimental conditions, thereby improving the preparation efficiency and avoiding the cutting of the sample, which is helpful to obtain angle graphene with controllable angle and large sample area.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of Raman scanning and two-dimensional material transfer, and in particular to a method for preparing controllable angle graphene with Raman assistance. Background Art

[0002] Twisted graphene is composed of two layers of graphene. When the crystallographic edges of the upper and lower graphene layers are aligned and the deviation is small, the small-angle graphene system exhibits many novel physical properties, such as superconductivity, strongly correlated insulating state, etc. Therefore, it is of great significance to prepare controllable angle twisted graphene to explore its physical properties. The above novel physical properties are all based on mechanically exfoliated graphene samples. This is because compared with the original single-layer graphene prepared by chemical methods such as chemical vapor deposition, the graphene obtained by mechanical exfoliation has the advantages of larger single crystal area and fewer crystal defects. Therefore, mechanical exfoliation is the basic method for preparing raw materials in twisted graphene. After the raw materials are obtained by mechanical exfoliation, the edges of the graphene samples need to be further aligned and rotated. The traditional alignment method only targets the sharp edges in the upper and lower graphene samples. Since it is impossible to determine whether the edge is the same type of crystallographic edge, the angle of the obtained twisted graphene is random and uncontrollable. In recent years, in order to align graphene with the same crystallographic edges, researchers have developed a series of cutting methods to cut the same graphene single crystal to obtain two or more graphene components with the same type of crystallographic edges as the upper and lower layers of graphene. For example, graphene is cut using an atomic force microscope probe to split the graphene into two halves. Afterwards, two-dimensional materials such as boron nitride are used as a pick-up layer to pick up one half of the graphene and align, rotate and superimpose it with the other half of the graphene. Further, researchers have also developed other cutting methods, such as electron beam exposure-assisted etching technology or laser cutting, but these cutting methods are complicated to operate and easily damage the quality of the sample crystal. It is worth noting that the area of ​​the mechanically peeled sample is small and at the micron level, so further cutting cannot meet the needs of large-area corner graphene preparation.

[0003] Because graphene samples are too thin, the instrument resolution required to observe their edges is extremely high, making direct observation and analysis difficult. In addition, the influence of preparation methods and environmental factors also increase the complexity of edge type identification. Commonly used identification methods are:

[0004] (1) Transmission electron microscopy (TEM): It can achieve atomic-level resolution, but requires a more complicated sample preparation process. It is difficult to use identified samples for secondary transfer or for the preparation of twisted graphene.

[0005] (2) Conventional Raman technology: It is non-destructive to samples and has a theoretical basis for Raman identification of graphene edges. However, in practice, it often takes a long time to observe because the intensity of the graphene defect peak (D peak) is too low to be observed. Summary of the invention

[0006] The purpose of the present invention is to overcome the problems existing in the prior art, select the edge of the graphene sample through Raman characterization, and improve the traditional Raman identification technology of graphene edges, so as to make the process more efficient, facilitate the combination of mechanical exfoliation and transfer technology, so as to achieve simple and efficient, precise control of the angle, and the preparation of angled graphene with a large interface area.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] The present invention provides a method for preparing graphene with controllable angle assisted by Raman, comprising the following steps:

[0009] (1) Spin coating a PVA solution and a PMMA solution on a silicon oxide wafer in sequence, and drying to obtain PMMA / PVA / silicon oxide; taking another substrate 2, wherein the substrate 2 is a silicon oxide wafer or a silicon oxide wafer spin coated with PVA, and using a mechanical exfoliation method to exfoliate the substrate 2 and PMMA / PVA / silicon oxide to obtain a graphene sample;

[0010] (2) using Raman scanning combined with peak area imaging to identify the edge of graphene; selecting a suitable substrate 2 and a graphene sample on PMMA / PVA / silicon oxide through identification; using deionized water to dissolve the PVA in PMMA / PVA / silicon oxide, so that the PMMA film carrying the graphene sample floats on the water surface, and using a gasket with holes to pick up the PMMA with graphene, so that the graphene is located in the center of the hole as much as possible, and then inverting and drying, during which it is necessary to pay attention to the graphene surface not contacting with water;

[0011] (3) Place the dried PMMA sample with graphene on the upper sample stage of the two-dimensional transfer platform, and place the substrate 2 containing the graphene sample on the lower sample stage. With the help of an optical microscope, the identified edge is rotated and aligned at a certain angle, and the angle is set through the sample stage to achieve controllable angle. Then adjust the transfer stage knob to lower the upper sample stage. During this process, attention should be paid to angle alignment. Then, fit the two samples together and keep them still for a period of time so that the sample interface can be tightly bonded. During this period, heating can be performed to accelerate the process, thereby achieving the preparation of angle graphene with controllable angle.

[0012] The present invention uses Raman surface scanning technology to scan the sample point by point Raman spectrum to obtain chemical and structural information with high spatial resolution. Combined with the peak area imaging method of the D peak, the resolution and resolution of the graphene edge type can be effectively improved, thereby identifying and distinguishing different edge types with high precision.

[0013] In some specific embodiments of the present invention, the oxidized silicon wafer is a 285nm oxide layer silicon wafer.

[0014] Preferably, in step (1), when the substrate 2 is an oxidized silicon wafer spin-coated with PVA, the graphene sample is peeled off from the surface of the PVA; the substrate 2 in the present invention does not limit the spin-coating amount of PVA on the oxidized silicon wafer.

[0015] Preferably, the parameters for Raman scanning to identify the edge of graphene are: 532nm laser, power of 22.5mW, scanning range of 1000-2000cm -1 , the laser step length is no more than 1.5um. The present invention greatly shortens the scanning time by controlling the optimal parameters. For a graphene sample of 50um×50um in size, the scanning time only takes ten minutes.

[0016] Preferably, the graphene sample identified by Raman scanning edge contains a sharp edge of 30°(2n+1), wherein n is an integer, i.e., the graphene sample identified by Raman scanning edge contains sharp edges of 30°, 90°, and 150°; one of the two edges of the angle is armchair-shaped and the other is sawtooth-shaped. The present invention combines graphene samples at specific angles to facilitate edge identification in Raman experiments.

[0017] Preferably, in step (1), the concentration of the PVA solution is 2-4wt%, and the concentration of the PMMA solution is 7-10wt%.

[0018] Preferably, in step (1), the drying temperature is 90-110° C., and the drying time is 5-10 min.

[0019] Preferably, in step (3), the heating temperature is 80-100° C. and the heating time is 8-12 min.

[0020] Preferably, when the corner graphene prepared in step (3) is transferred to a transmissive support film for transmission electron microscopy observation, when substrate 2 is a silicon oxide wafer spin-coated with PVA, PVA is dissolved in water to obtain a suspended sample, and then the sample is cleaned with acetone to remove PMMA, and the suspended corner graphene is obtained after drying, which can be observed by transmission electron microscopy; when substrate 2 is a silicon oxide wafer, KOH solution is used to soak and react with the silicon oxide substrate to obtain a suspended sample, and then acetone is used to clean the sample to remove PMMA, and the suspended corner graphene is obtained after drying, which can be observed by transmission electron microscopy.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The traditional Raman graphene edge identification technology is improved by selecting and preparing graphene samples and adjusting Raman experimental conditions, making the process more efficient and easier to combine with mechanical exfoliation and transfer technology, thereby achieving simple and efficient preparation of corner graphene with precise control of corners and clean interfaces.

[0023] (1) Efficient identification of graphene sample edges: Graphene samples are screened by mechanical exfoliation and Raman experimental conditions are adjusted to achieve efficient identification of sample edge types, shortening the traditional scanning time of several hours or even dozens of hours to ten minutes. In addition, traditional TEM identification is prone to damage to samples due to electron beam irradiation, and it is difficult to remove them from the support film for other characterizations.

[0024] (2) Accuracy of angle control: It is difficult to accurately control the angle with traditional methods, especially when preparing graphene with angles close to the magic angle. With the assistance of Raman spectroscopy, the edge features of the graphene sheets can be more accurately determined before superposition, which helps to accurately adjust the angle, and the probability of achieving small angle construction can reach 100%.

[0025] (3) Highly compatible with mechanical stripping and transfer technologies: A variety of substrates were screened, and Raman identification was achieved on silicon oxide substrates and silicon oxide or silicon wafer substrates spin-coated with organic layers (polyvinyl alcohol (PVA), polymethyl methacrylate (PMMA)). These substrates are commonly used in mechanical stripping and transfer methods, and the combination of methods is highly compatible.

[0026] (4) Simplified preparation process: Compared with the preparation method that requires precision equipment, this mechanical exfoliation method combined with Raman spectroscopy simplifies the preparation process and reduces the dependence on equipment, making the preparation of twisted graphene more popular and feasible.

[0027] (5) Preparation efficiency and sample quality: The samples prepared by mechanical exfoliation generally have a more perfect crystal structure than graphene prepared by methods such as CVD, and graphene samples with good edge structure and few defects can be selected. In addition, the preparation of corner samples can be combined with mature transfer technology to greatly improve the preparation efficiency and sample quality. The corner graphene sample preparation scheme provided by the present invention can keep the interface clean at all times. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Schematic diagram of the graphene sample screened in Example 1;

[0029] Figure 2 The Raman test spectra of different edges in Example 1;

[0030] Figure 3The sample scanning area and results on the silicon oxide substrate in Example 1, Figure a is the Raman scanning area and the edge type marked according to the scanning results, and Figure b is the Raman surface scanning peak area imaging;

[0031] Figure 4 The sample scanning area and results on the silicon oxide substrate in Example 2, Figure a is the Raman scanning area and the edge type marked according to the scanning results, and Figure b is the Raman surface scanning peak area imaging;

[0032] Figure 5 The sample scanning area and results on the PMMA / PVA / silicon oxide substrate in Example 2, Figure a is the Raman scanning area and the edge type marked according to the scanning results, and Figure b is the Raman surface scanning peak area imaging;

[0033] Figure 6 This is the optical microscopy image of the small-angle graphene sample;

[0034] Figure 7 This is the TEM bright field image of the small-angle graphene sample;

[0035] Figure 8 Selected electron diffraction image for small-angle graphene sample. DETAILED DESCRIPTION

[0036] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0037] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.

[0038] The Raman-assisted method for preparing controllable angle graphene of the present invention comprises the following steps:

[0039] (1) Sample preparation:

[0040] 1. Prepare a clean silicon oxide substrate, and prepare PMMA solution and PVA solution; use a coating machine to spin coat PVA and PMMA on a portion of silicon oxide in turn, and dry to obtain a PMMA / PVA / silicon oxide substrate; the spin coating parameters are: 3000 rpm for 1 minute, and after spin coating one layer, it needs to be heated and dried before the next spin coating, the drying temperature is 100°C, and the time is 5 minutes.

[0041] 2. Use mechanical exfoliation to exfoliate graphene samples of appropriate thickness on substrate 2 (silicon oxide substrate or PVA / silicon oxide substrate) and PMMA / PVA / silicon oxide substrate.

[0042] The graphene samples in the embodiments of the present invention need to meet the following requirements:

[0043] The sample contains a sharp corner of 30°(2n+1), (n∈Z), one of the two edges of which is armchair type and the other is serrated type (mechanically exfoliated graphene edges are generally cleaved along armchair or serrated edges, and the angle between the two edges is 30° to facilitate edge identification in subsequent Raman experiments);

[0044] (2) Raman identification of graphene edges:

[0045] When using Raman scanning to identify graphene edges, before testing, the sample position needs to be adjusted so that the laser polarization direction is located on the bisector of the edge angle to avoid errors caused by polarization.

[0046] Use line scanning to scan the two edges and observe the D peak: about 1350cm -1 At the armchair edge, due to its poor symmetry, a small peak will generally appear. If no obvious D peak is found, increase the laser power or scan time to enhance the armchair edge defect signal. After observing the obvious D peak signal difference, you can perform a surface scan according to the current parameters. After the surface scan is completed, the entire spectrum is processed to remove cosmic ray interference. If necessary, the baseline can be removed. The point spectrum containing obvious D peaks is called out and its D peak range is recorded. Peak area imaging is performed in this range to enhance the resolution. If the D peak is more obvious, the peak position, i.e. 1350cm, can be used directly. -1 The intensity imaging at the edge is performed. The edge type of graphene is distinguished according to the edge intensity. The edge with a strong signal is an armchair edge, and the edge with a weak signal is a sawtooth edge.

[0047] After experiments, the optimal parameters of this scheme are: 532nm laser with a power of 22.5mW, number of scans: 1, exposure time: 0.5s. To obtain a higher resolution, the laser step length must be no higher than 1.5um. For a graphene sample of 50um x 50um in size, the scanning time is only ten minutes.

[0048] (3) Controllable angle graphene preparation: The solution provided by the present invention can realize the identification of the edges of graphene samples on various substrates, which is very compatible with various relatively mature transfer technologies at present. The transfer method can be selected according to the preparation purpose and the sample cleanliness requirements. It includes the following steps:

[0049] Prepare graphene samples on two substrates (silicon oxide substrate and PMMA / PVA / silicon oxide substrate) with edge identification completed, dissolve the PVA in the PMMA / PVA / silicon oxide substrate with deionized water, make the PMMA film carrying the graphene sample float on the water surface, and use a gasket with holes to pick up the PMMA, so that the graphene is located in the center of the hole as much as possible, and then invert and dry at 80°C to avoid adverse effects of the liquid on the film. During this process, be careful not to let water touch the graphene surface, which may introduce contamination.

[0050] Place the dried graphene / PMMA sample gasket on the upper sample stage of the two-dimensional transfer platform, and place the silicon oxide substrate containing the graphene sample on the lower sample stage. With the help of an optical microscope, the identified edges are rotated and aligned at a certain angle to achieve controllable angle. Then adjust the transfer stage knob to lower the upper sample stage. During this process, attention should be paid to angle alignment (i.e., the relative angle between the two samples). Then, fit the two samples together and keep them still for a period of time to make the inside of the samples fit tightly. During this period, heating can be performed (80-100°C for ~10 minutes) to accelerate the process to ensure that the bonding force between the samples is strong enough, thereby achieving the preparation of corner graphene with controllable angle.

[0051] If it is to be transferred to a transmissive support film for transmission electron microscopy observation, when substrate 2 is a silicon oxide wafer spin-coated with PVA, use water to dissolve PVA to obtain a suspended sample, then use acetone to clean the sample to remove PMMA, and then dry it for transmission electron microscopy observation; when substrate 2 is a silicon oxide wafer, use KOH solution (mass fraction is about 2%) to soak and react with the silicon oxide substrate, so that the PMMA carrying the corner graphene sample floats, move it to deionized water for cleaning and transfer it to a transmissive support film, use acetone to clean PMMA, and then dry it for transmission electron microscopy observation.

[0052] Example 1 Raman Efficient Identification of Graphene Sample Edge Type

[0053] (1) Prepare a clean silicon oxide substrate and prepare a PVA solution with a concentration of 3% by mass. Spin coat the PVA solution on the substrate. The spin coating parameters are: 3000 rpm for 1 minute. After one layer is spin-coated, it needs to be heated and dried before the next spin coating. The drying temperature is 100°C and the time is 5 minutes. Then, the graphene is prepared by mechanical exfoliation on the substrate. The samples screened are as follows: Figure 1 As shown, the angle of its thick edge is 90°.

[0054] (2) Graphene edge Raman identification test: first perform a single spectrum scan on the edge of the graphene sample to make a preliminary judgment on the sample. The conditions are: laser wavelength: 532nm, power: 22.5mW, exposure time: 10s, scanning range: 1200~1500cm -1The results are as follows Figure 2 As shown, two edges can be observed at 1350 cm -1 There is a clear difference in the intensity variation nearby, and the armchair edge contains an obvious defect peak.

[0055] In order to identify the edge of the entire graphene sample, the entire graphene sample was scanned. The experimental conditions were: laser wavelength: 532nm, power: 22.5mW, exposure time: 0.5s, scanning range: 1200~1500cm -1 , step length: 0.5um (can be selected according to experimental requirements, the step length can be reduced to improve resolution), and the results obtained are between 1300 and 1400cm -1 Peak area imaging is performed within the range of Figure 3 As shown, from Figure 3 In b, two edge types are found to be very obvious in Raman spectroscopy imaging, among which the armchair edge is obviously brighter, while the jagged edge has a weaker signal.

[0056] Example 2 Raman small-angle graphene sample preparation

[0057] (1) Substrate preparation: Prepare a clean silicon oxide substrate and prepare a PMMA solution with a concentration of 8% by mass and a PVA solution with a concentration of about 3% by mass; then use a coating machine to spin coat PVA and PMMA on a portion of the silicon wafer in turn, and dry to obtain a PMMA / PVA / silicon oxide substrate; the spin coating parameters are: 3000 rpm for 1 minute, and after spin coating one layer, it needs to be heated and dried before the next spin coating can be performed. The drying temperature is 100°C and the time is 5 minutes.

[0058] (2) Sample preparation and screening: Graphene samples of appropriate thickness were obtained by mechanical exfoliation on silicon oxide substrate and PMMA / PVA / silicon oxide substrate. Figure 4 a, as shown in 5a, where Figure 4 The sample angle on the silicon wafer substrate in a is 30°, and the sample is a thin sample (about 2 to 3 layers); Figure 5 The thick edge angle of the sample on the PMMA / PVA / silicon oxide substrate in a is 150°.

[0059] Graphene edge Raman scanning identification: The experimental conditions are: laser wavelength: 532nm, power: 22.5mW, exposure time: 0.5s, scanning range: 1000~2000cm -1 , step length: 1.4um. The results are as follows Figure 4 a, as shown in 5a, the edge type is marked in the light microscopy image.

[0060] (3) Preparation of small-angle graphene samples: Use deionized water to dissolve the PVA in the PMMA / PVA / silicon oxide substrate, so that the PMMA film carrying the graphene sample floats on the water surface, and use a perforated gasket to pick up the PMMA, dry it, and place it on the upper sample stage of the two-dimensional transfer platform. Place the silicon oxide substrate containing the graphene sample on the lower sample stage. With the help of an optical microscope, in this experiment, the armchair edges of the two samples are aligned, and then the transfer stage knob is adjusted to lower the upper sample to fit. After fitting, it is heated at 80°C to ensure sample bonding. The optical microscope image of the obtained angle graphene sample is shown in the figure. Figure 6 shown.

[0061] (4) The sample is immersed in a KOH solution with a concentration of about 2% by mass. KOH reacts with the oxide layer on the silicon wafer, so that the PMMA carrying the small-angle graphene sample floats, and is transferred to deionized water for washing three times and then transferred to a transmission support film. The PMMA is washed with acetone and dried before being observed by transmission electron microscopy. The obtained TEM bright field image is shown in Figure 7. It can be clearly observed that the moiré fringes formed by the lattice reconstruction of the small-angle sample are selected. The electron diffraction image is shown in Figure 7. Figure 8 As shown, after measurement, it can be confirmed that the angle of the obtained small-angle sample is ∼0.9°.

[0062] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. A Raman-assisted method for preparing controllable angle graphene, It is characterized in that The following steps are involved: (1) Spin coating a PVA solution and a PMMA solution on a silicon oxide wafer in sequence, and drying to obtain PMMA / PVA / silicon oxide; taking another substrate 2, wherein the substrate 2 is a silicon oxide wafer or a silicon oxide wafer spin coated with PVA, and using a mechanical exfoliation method to exfoliate the substrate 2 and PMMA / PVA / silicon oxide to obtain a graphene sample; (2) using Raman scanning combined with peak area imaging to identify the edge of graphene; selecting a suitable substrate 2 and a graphene sample on PMMA / PVA / silicon oxide through identification; using deionized water to dissolve the PVA in PMMA / PVA / silicon oxide, so that the PMMA film carrying the graphene sample floats on the water surface, and using a gasket with holes to pick up the PMMA with graphene, so that the graphene is located in the center of the hole as much as possible, and then inverting and drying, during which it is necessary to pay attention to the graphene surface not contacting with water; (3) Place the dried PMMA sample with graphene on the upper sample stage of the two-dimensional transfer platform, and place the substrate 2 containing the graphene sample on the lower sample stage. With the help of an optical microscope, the identified edge is rotated and aligned at a certain angle, and the angle is set through the sample stage to achieve controllable angle. Then adjust the transfer stage knob to lower the upper sample stage. During this process, attention should be paid to angle alignment. Then, fit the two samples together and keep them still for a period of time so that the sample interface can be tightly bonded. During this period, heating can be performed to accelerate the process, thereby achieving the preparation of angle graphene with controllable angle.

2. The method for preparing controlled angle graphene by Raman-assisted method according to claim 1, It is characterized in that In step (1), when the substrate 2 is a silicon oxide wafer spin-coated with PVA, a graphene sample is obtained by peeling off the surface of the PVA.

3. The method for preparing controlled angle graphene by Raman-assisted method according to claim 1, It is characterized in that The parameters for Raman scanning to identify the graphene edge are: 532nm laser, power of 22.5mW, scanning range of 1000-2000cm -1 , the laser step length is no higher than 1.5um.

4. The method for preparing controlled angle graphene by Raman-assisted method according to claim 2, It is characterized in that The graphene sample identified by Raman scanning edge contains a sharp angle of 30°(2n+1), one of the two edges of the angle is armchair-shaped and the other is sawtooth-shaped.

5. The method for preparing controllable angle graphene by Raman-assisted method according to claim 1, It is characterized in that In step (1), the concentration of the PVA solution is 2-4wt%, and the concentration of the PMMA solution is 7-10wt%.

6. The method for preparing controllable angle graphene by Raman-assisted method according to claim 1, It is characterized in that In step (1), the drying temperature is 90-110° C. and the drying time is 5-10 min.

7. The method for preparing controllable angle graphene by Raman-assisted method according to claim 1 or 2, It is characterized in that In step (3), the heating temperature is 80-100° C. and the heating time is 8-12 min.

8. The method for preparing controllable angle graphene by Raman-assisted method according to claim 1, It is characterized in that When the corner graphene prepared in step (3) is transferred to a transmissive support film for transmission electron microscopy observation, when substrate 2 is an oxidized silicon wafer spin-coated with PVA, PVA is dissolved in water to obtain a suspended sample, and then the sample is cleaned with acetone to remove PMMA, and the suspended corner graphene is obtained after drying, which can be observed by transmission electron microscopy; when substrate 2 is an oxidized silicon wafer, KOH solution is used to soak and react with the oxidized silicon substrate to obtain a suspended sample, and then acetone is used to clean the sample to remove PMMA, and the suspended corner graphene is obtained after drying, which can be observed by transmission electron microscopy.