Ceramic tile, preparation method and application thereof
By evenly distributing irregular metal particles and boron fibers in ceramic tiles, the problem of poor thermal conductivity of ceramic tiles is solved, and the application efficiency and stability of the floor heating system are improved.
Patent Information
- Application Number
- CN202410956504.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The thermal conductivity and insulation performance of existing ceramic tiles cannot meet the application environment of the floor heating system, resulting in low efficiency when used in the floor heating system.
The wet ball milling method is used to mix the ceramic powder with water, boron fibers and foam metal particles. After ultrasonic dispersion and firing, irregular metal particles and boron fibers are formed evenly distributed in the ceramic matrix to improve the thermal conductivity and strength.
It significantly improves the thermal conductivity and strength of ceramic tiles, accelerates the temperature rise in the room, reduces the bulging phenomenon caused by changes in metal volume after firing, and improves the application efficiency and stability of ceramic tiles.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the field of ceramic technology, and in particular to a ceramic tile, a preparation method and application thereof. Background Art
[0002] Floor heating system is an efficient independent heating method for families. It uses the heat source under the floor to evenly heat the floor and transfers the heat to the indoor space through floor radiation. The main phases of existing ceramic tiles are mostly quartz SiO2, mullite Al (Al 0.69 Si 1.22 O 4.85 ), corundum α-Al2O3 and other inorganic components, their thermal conductivity and thermal insulation performance cannot meet the application environment of the floor heating system. Summary of the invention
[0003] The main purpose of the present invention is to provide a ceramic tile, a preparation method and an application thereof, aiming to solve the problem of poor thermal conductivity and heat preservation performance of existing ceramic tiles.
[0004] In one aspect, the present application provides a method for preparing a ceramic tile, comprising the following steps:
[0005] Wet ball milling the ceramic powder;
[0006] adding water, boron fiber and foamed metal particles to the ball-milled ceramic powder to obtain a slurry;
[0007] The foamed metal particles are converted into irregular metal particles by firing to obtain ceramic tiles.
[0008] In any embodiment, the chemical composition of the ceramic powder is: SiO2: 57~67wt.%, Al2O3: 17~26wt.%, Fe2O3: 0.4~1.1wt.%, TiO2: 0.2~0.5wt.%, CaO: 0.1~0.4wt.%, MgO: 0.2~0.8wt.%, K2O: 1.5~3.5wt.%, Na2O: 1.5~4.5wt.%, P2O3: 0.01~0.07wt.%, SO3: 0.1~0.8wt.%, and loss on ignition: 3~9wt.%.
[0009] In any embodiment, the step of adding water, boron fibers and foamed metal particles to the ball-milled ceramic powder to obtain a slurry comprises:
[0010] The ball-milled ceramic powder is magnetically stirred in deionized water;
[0011] Boron fibers and foamed metal particles ultrasonically dispersed in deionized water are added to ceramic powder respectively, and then polyvinyl alcohol solution is added; slurry is obtained after secondary ultrasonication.
[0012] In any embodiment, the ultrasonic dispersion time is 30-60 minutes, the secondary ultrasonic time is 2-6 hours, and the mass concentration of the polyvinyl alcohol solution is 5-10%.
[0013] On the other hand, the present application provides a ceramic tile, comprising a ceramic matrix and boron fibers and irregular metal particles uniformly distributed in the ceramic matrix.
[0014] In any embodiment, the boron fiber has a diameter of 20-100 μm and a length of more than 400 μm.
[0015] In any embodiment, the length of the boron fiber is 400-700 μm.
[0016] In any embodiment, the mass percentage of the boron fiber in the ceramic matrix is 5% to 10%.
[0017] In any embodiment, the irregular metal particles account for 0.1% to 10% by mass in the ceramic matrix.
[0018] In any embodiment, the irregular metal particles include at least one of aluminum particles, copper particles, and nickel particles.
[0019] On the other hand, the present application provides an application of ceramic tiles for use in a venue with a floor heating system.
[0020] In the technical solution of the present application, the heat transfer performance of the irregular metal particles uniformly distributed in the ceramic matrix is better than that of the inorganic components of the conventional ceramic matrix. When applied to an environment with a floor heating system, for example, when the ceramic bricks in the present application are set on the heating device of the floor heating system, the metal particles uniformly distributed in the ceramic matrix can enhance heat conduction and accelerate the temperature rise in the room. In addition, during the preparation process, foam metal particles are added as metal raw materials. Due to the large compressibility of the foam metal particles, although some of them are pressed into powder during the pressing process, there are still certain pores in the foam metal particles. During the high-temperature firing stage, the foam metal particles melt into a liquid state, and some of them become oxidized and then change in volume. Since there are still certain pores in the foam metal particles after pressing, the foam metal particles are transformed into irregular metal particles after firing, which can reduce the bulging caused by the volume change of the metal after firing. In addition, the boron fibers uniformly distributed in the ceramic matrix can be used as a guide rail for the discharge of bubbles, which is conducive to the discharge of bubbles in the ceramic matrix. The boron fibers can provide a skeleton effect, which is conducive to the uniform distribution of irregular metal particles and improves the strength of the ceramic brick. DETAILED DESCRIPTION
[0021] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.
[0022] On the one hand, the present invention provides a method for preparing a ceramic tile, comprising the following steps:
[0023] Wet ball milling the ceramic powder;
[0024] adding water, boron fiber and foamed metal particles to the ball-milled ceramic powder to obtain a slurry;
[0025] The foamed metal particles are converted into irregular metal particles by firing to obtain ceramic tiles.
[0026] The preparation method is simple and easy to industrialize.
[0027] Among them, boron fiber refers to an inorganic fiber formed by depositing boron on a metal wire. It is usually obtained by reacting hydrogen and boron trichloride on a hot tungsten wire to displace amorphous boron and deposit it on the surface of the tungsten wire. Boron fiber is generally produced by chemical vapor deposition (CVD). Usually a very thin tungsten wire with a diameter of 12.5 um is used, which is heated by a resistor through a reaction tube. A chemical mixture of boron trichloride (BCl3) and hydrogen flows in from the upper inlet of the reaction tube and is heated to about 1300°C. After a chemical reaction, a boron layer is deposited on the clean surface of the tungsten wire, and the produced boron fiber is led out and wound on a wire tube.
[0028] Foam metal refers to a special metal material containing foam pores. Through its unique structural characteristics, foam metal has a series of good advantages such as low density, good thermal insulation, good sound insulation and the ability to absorb electromagnetic waves. Foam metal can be prepared by powder metallurgy and electroplating. The former is prepared by adding a foaming agent to the molten metal to prepare foam metal; the latter is replicated into foam metal on the polyurethane foam plastic skeleton through an electrodeposition process. The powder metallurgy method is to add a foaming agent (such as NH4Cl) to the powder. The foaming agent evaporates during sintering, leaving pores. Foam metal with regular pores and a porosity of up to 95% can be prepared by electrochemical deposition, including foam materials with metals and alloys such as Cu, Ni, NiCrFe, ZnCu, NiCu, NiCrW, NiFe as the skeleton. The metal deposited on the porous body by electrochemical deposition is sintered to connect the deposited components into a whole, and the strength reaches the required high-porosity foam metal with high porosity. More substances such as catalysts and electrolytes can be filled in use.
[0029] The boron fiber and foam metal in the examples of the present application are both purchased conventionally. The foam metal particles in the examples of the present application are obtained by cutting the purchased foam metal to obtain particles with a volume of, for example, 5×5×5mm, 4×4×4mm, and 3×3×3mm. Usually, the thickness of the ceramic brick blank is 10mm, and any size of the foam metal particles should be smaller than the thickness of the ceramic brick blank. The method of cutting the foam metal can be achieved by a high-precision cutting tool such as a water jet or a laser cutter.
[0030] In the preparation process of the embodiment of the present application, foam metal particles are added as metal raw materials. Due to the high compressibility of the foam metal particles, although some of them are pressed into powder during the pressing process, there are still certain pores in the foam metal particles. During the high-temperature firing stage, the foam metal particles melt into a liquid state, and some of them become oxidized and then change in volume. Since there are still certain pores in the foam metal particles after pressing, the foam metal particles are transformed into irregular metal particles after firing, which can reduce the bulging caused by the volume change of the metal after firing. In addition, the boron fibers evenly distributed in the ceramic matrix can serve as a guide rail for the discharge of bubbles, which is conducive to the discharge of bubbles in the ceramic matrix. The boron fibers can provide a skeleton effect, which is conducive to the uniform distribution of irregular metal particles and improves the strength of ceramic tiles.
[0031] In some embodiments, the chemical composition of the ceramic powder is: SiO2: 57~67wt.%, Al2O3: 17~26wt.%, Fe2O3: 0.4~1.1wt.%, TiO2: 0.2~0.5wt.%, CaO: 0.1~0.4wt.%, MgO: 0.2~0.8wt.%, K2O: 1.5~3.5wt.%, Na2O: 1.5~4.5wt.%, P2O3: 0.01~0.07wt.%, SO3: 0.1~0.8wt.%, loss on ignition: 3~9wt.%.
[0032] The chemical composition of the ceramic powder in the embodiments of the present application can be conventional components, and changes in its chemical composition do not affect the performance improvement of the ceramic tile by the boron fiber and the foam metal.
[0033] In some embodiments, the step of adding water, boron fibers and foamed metal particles to the ball-milled ceramic powder to obtain a slurry comprises:
[0034] The ball-milled ceramic powder is magnetically stirred in deionized water;
[0035] Boron fibers and foamed metal particles ultrasonically dispersed in deionized water are added to ceramic powder respectively, and then polyvinyl alcohol solution is added; slurry is obtained after secondary ultrasonication.
[0036] Under the action of ultrasound, the boron fibers and foam metal particles can be evenly dispersed in the slurry.
[0037] In some embodiments, the mass proportion of boron fiber in the ceramic powder is 5% to 10%. In the embodiment of the present application, the obtained slurry is dried, granulated and then pressed to obtain a green body. In the present application, it is considered that the volume of the green body is approximately the same as the volume of the final ceramic tile, and the mass proportion of the foam metal particles in the green body is 0.1% to 10%.
[0038] In some embodiments, the ultrasonic dispersion time is 30-60 minutes, the secondary ultrasonic time is 2-6 hours, and the mass concentration of the polyvinyl alcohol solution is 5-10%.
[0039] An embodiment of the present application provides a ceramic tile, comprising a ceramic matrix and boron fibers and irregular metal particles uniformly distributed in the ceramic matrix.
[0040] In the technical solution of the present application, the heat transfer performance of the irregular metal particles uniformly distributed in the ceramic matrix is better than that of the inorganic components of the conventional ceramic matrix. When applied to an environment with a floor heating system, for example, when the ceramic bricks in the present application are set on the heating device of the floor heating system, the foam metal particles uniformly distributed in the ceramic matrix can enhance heat conduction and accelerate the temperature rise in the room. The boron fibers uniformly distributed in the ceramic matrix can serve as a guide rail for the discharge of bubbles, which is conducive to the discharge of bubbles in the ceramic matrix. The boron fibers can provide a skeleton effect, which is conducive to the uniform distribution of irregular metal particles and improves the strength of ceramic tiles.
[0041] In some embodiments, the boron fiber has a diameter of 20-100 μm and a length greater than 400 μm. Boron fibers greater than 400 μm are beneficial for discharging bubbles in the brick and supporting irregular metal particles. If the length of the boron fiber is too small, bubbles in the brick cannot be effectively discharged.
[0042] In some embodiments, the length of the boron fiber is 400-700 μm. If the length of the boron fiber is too short, the bubbles in the brick cannot be effectively discharged.
[0043] In some embodiments, the mass proportion of the boron fiber in the ceramic matrix is 5% to 10%. If the mass proportion of the boron fiber in the ceramic matrix is too small, bubbles in the brick cannot be effectively discharged.
[0044] In some embodiments, the mass proportion of the foamed metal particles in the ceramic matrix is 0.1% to 10%. Due to the difference in physical properties between irregular metal particles and the ceramic matrix, if there are too many irregular metal particles, the ceramic brick will be easily bulged due to different stresses during temperature changes. If the volume proportion of irregular metal particles is too small, it will not be able to conduct heat effectively.
[0045] In some embodiments, the irregular metal particles include at least one of aluminum particles, copper particles, and nickel particles.
[0046] On the other hand, the present application provides an application of ceramic tiles for use in a venue with a floor heating system.
[0047] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0048] Example 1
[0049] This embodiment provides a method for preparing a ceramic tile, and a ceramic tile prepared by the method, wherein the method comprises the following steps:
[0050] The foam copper was cut into particles of about 5×5×5 mm using a laser cutting machine, and the cut foam metal particles were immersed in anhydrous ethanol for 1 hour, and then the foam metal particles were taken out and dried;
[0051] The ceramic powder is wet ball milled, wherein the chemical composition of the ceramic powder is: SiO2: 61.85wt.%, Al2O3: 24.62wt.%, Fe2O3: 0.75wt.%, TiO2: 0.38wt.%, CaO: 0.31wt.%, MgO: 0.48wt.%, K2O: 2.56wt.%, Na2O: 3.02wt.%, P2O3: 0.04wt.%, SO3: 0.40wt.%, and loss on ignition: 5.59wt.%.
[0052] The ball-milled ceramic powder was magnetically stirred in deionized water; at the same time, the boron fibers and foamed metal particles, which were ultrasonically dispersed in deionized water for 30 minutes, were gradually added to the ceramic slurry, and then a polyvinyl alcohol solution with a concentration of 8.0wt.% was added dropwise, and then a uniform slurry was obtained after ultrasonic treatment for 3 hours. The slurry was dried at 100°C, and the semi-dry powder obtained was granulated and pressed to obtain a green body. After drying at 110°C, it was sintered at 1200°C for 1 hour to obtain a ceramic tile. Among them, the diameter of the boron fiber is 50μm and the length is 500μm. The mass proportion of the added boron fiber in the ceramic powder is 5%. The mass proportion of the added foamed metal particles in the green body is 2%.
[0053] Example 2
[0054] This embodiment provides a method for preparing a ceramic tile, and a ceramic tile prepared by the method, wherein the method comprises the following steps:
[0055] The foam copper was cut into particles of about 5×5×5 mm using a laser cutting machine, and the cut foam metal particles were immersed in anhydrous ethanol for 1 hour, and then the foam metal particles were taken out and dried;
[0056] The ceramic powder is wet ball milled, wherein the chemical composition of the ceramic powder is: SiO2: 61.85wt.%, Al2O3: 24.62wt.%, Fe2O3: 0.75wt.%, TiO2: 0.38wt.%, CaO: 0.31wt.%, MgO: 0.48wt.%, K2O: 2.56wt.%, Na2O: 3.02wt.%, P2O3: 0.04wt.%, SO3: 0.40wt.%, and loss on ignition: 5.59wt.%.
[0057] The ball-milled ceramic powder was magnetically stirred in deionized water; at the same time, the boron fibers and foamed metal particles, which were ultrasonically dispersed in deionized water for 30 minutes, were gradually added to the ceramic slurry, and then a polyvinyl alcohol solution with a concentration of 8.0wt.% was added dropwise, and then a uniform slurry was obtained after ultrasonic treatment for 3 hours. The slurry was dried at 100°C, and the semi-dry powder obtained was granulated and pressed to obtain a green body. After drying at 110°C, it was sintered at 1200°C for 1 hour to obtain a ceramic tile. Among them, the diameter of the boron fiber is 50μm and the length is 500μm. The mass proportion of the added boron fiber in the ceramic powder is 5%. The mass proportion of the added foamed metal particles in the green body is 0.5%.
[0058] Example 3
[0059] This embodiment provides a method for preparing a ceramic tile, and a ceramic tile prepared by the method, wherein the method comprises the following steps:
[0060] The foam copper was cut into particles of about 4×4×4 mm using a laser cutting machine, and the cut foam metal particles were immersed in anhydrous ethanol for 1 hour, and then the foam metal particles were taken out and dried;
[0061] The ceramic powder is wet ball milled, wherein the chemical composition of the ceramic powder is: SiO2: 61.85wt.%, Al2O3: 24.62wt.%, Fe2O3: 0.75wt.%, TiO2: 0.38wt.%, CaO: 0.31wt.%, MgO: 0.48wt.%, K2O: 2.56wt.%, Na2O: 3.02wt.%, P2O3: 0.04wt.%, SO3: 0.40wt.%, and loss on ignition: 5.59wt.%.
[0062] The ball-milled ceramic powder was magnetically stirred in deionized water; at the same time, the boron fibers and foamed metal particles, which were ultrasonically dispersed in deionized water for 30 minutes, were gradually added to the ceramic slurry, and then a polyvinyl alcohol solution with a concentration of 8.0wt.% was added dropwise, and then a uniform slurry was obtained after ultrasonic treatment for 3 hours. The slurry was dried at 100°C, and the semi-dry powder obtained was granulated and pressed to obtain a green body. After drying at 110°C, it was sintered at 1200°C for 1 hour to obtain a ceramic tile. Among them, the diameter of the boron fiber is 50μm and the length is 500μm. The mass proportion of the added boron fiber in the ceramic powder is 10%. The mass proportion of the added foamed metal particles in the green body is 8%.
[0063] Comparative Example 1
[0064] This comparative example provides a method for preparing a ceramic tile, and a ceramic tile prepared by the preparation method, wherein the preparation method comprises the following steps:
[0065] The ceramic powder is wet ball milled, wherein the chemical composition of the ceramic powder is: SiO2: 61.85wt.%, Al2O3: 24.62wt.%, Fe2O3: 0.75wt.%, TiO2: 0.38wt.%, CaO: 0.31wt.%, MgO: 0.48wt.%, K2O: 2.56wt.%, Na2O: 3.02wt.%, P2O3: 0.04wt.%, SO3: 0.40wt.%, and loss on ignition: 5.59wt.%.
[0066] The ball-milled ceramic powder was magnetically stirred in deionized water; at the same time, the boron fiber after ultrasonic dispersion in deionized water for 30 minutes was gradually added to the ceramic slurry, and then a polyvinyl alcohol solution with a concentration of 8.0wt.% was added dropwise with a total weight of 5.0wt.% of the powder; after ultrasonic treatment for 3 hours, a uniform slurry was obtained. The slurry was dried at 100°C, and the semi-dry powder obtained was granulated and pressed to obtain a green body. After drying at 110°C, it was sintered at 1200°C for 1 hour to obtain a ceramic tile. Among them, the diameter of the boron fiber is 50μm and the length is 200μm. The mass proportion of the added boron fiber in the ceramic powder is 5%.
[0067] Comparative Example 2
[0068] The ceramic powder is wet ball milled, wherein the chemical composition of the ceramic powder is: SiO2: 61.85wt.%, Al2O3: 24.62wt.%, Fe2O3: 0.75wt.%, TiO2: 0.38wt.%, CaO: 0.31wt.%, MgO: 0.48wt.%, K2O: 2.56wt.%, Na2O: 3.02wt.%, P2O3: 0.04wt.%, SO3: 0.40wt.%, and loss on ignition: 5.59wt.%.
[0069] The ball-milled ceramic powder is magnetically stirred in deionized water to obtain a uniform slurry. The slurry is dried at 100°C, and the semi-dry powder obtained is granulated and pressed to obtain a green body. After drying at 110°C, it is sintered at 1200°C for 1 hour to obtain a ceramic tile.
[0070] Comparative Example 3
[0071] This comparative example provides a method for preparing a ceramic tile, and a ceramic tile prepared by the preparation method, wherein the preparation method comprises the following steps:
[0072] The foam copper was cut into particles of about 5×5×5 mm using a laser cutting machine, and the cut foam metal particles were immersed in anhydrous ethanol for 1 hour, and then the foam metal particles were taken out and dried;
[0073] The ceramic powder is wet ball milled, wherein the chemical composition of the ceramic powder is: SiO2: 61.85wt.%, Al2O3: 24.62wt.%, Fe2O3: 0.75wt.%, TiO2: 0.38wt.%, CaO: 0.31wt.%, MgO: 0.48wt.%, K2O: 2.56wt.%, Na2O: 3.02wt.%, P2O3: 0.04wt.%, SO3: 0.40wt.%, and loss on ignition: 5.59wt.%.
[0074] The ball-milled ceramic powder was magnetically stirred in deionized water; at the same time, the boron fibers and foamed metal particles, which were ultrasonically dispersed in deionized water for 30 minutes, were gradually added to the ceramic slurry, and then a polyvinyl alcohol solution with a concentration of 8.0wt.% was added dropwise, and then a uniform slurry was obtained after ultrasonic treatment for 3 hours. The slurry was dried at 100°C, and the semi-dry powder obtained was granulated and pressed to obtain a green body. After drying at 110°C, it was sintered at 1200°C for 1 hour to obtain a ceramic tile. Among them, the diameter of the boron fiber is 50μm and the length is 500μm. The mass proportion of the added boron fiber in the ceramic powder is 5%. The mass proportion of the added foamed metal particles in the green body is 12%.
[0075] Performance Testing:
[0076] Check whether the ceramic tiles prepared in Examples 1-5 have bulging.
[0077] Table 1 Performance parameters of Examples 1-5
[0078]
[0079] From the hot and cold alternating experimental data in Table 1, it can be seen that the mass proportion of the foamed metal particles added in Examples 1, 2, and 3 in the green body is within an appropriate range, and no bulging phenomenon occurs. However, in Comparative Example 3, the mass proportion of the foamed metal particles in the green body is too large, and bulging phenomenon occurs. Since no metal substance is added in Comparative Examples 1 and 2, no bulging phenomenon occurs. However, since no metal particles are added in Comparative Examples 1 and 2, their thermal conductivity is worse than that of Examples 1-3.
[0080] In the technical solution of the present application, the heat transfer performance of the irregular metal particles uniformly distributed in the ceramic matrix is better than that of the inorganic components of the conventional ceramic matrix. When applied to an environment with a floor heating system, for example, when the ceramic bricks in the present application are set on the heating device of the floor heating system, the metal particles uniformly distributed in the ceramic matrix can enhance heat conduction and accelerate the temperature rise in the room. In addition, during the preparation process, foam metal particles are added as metal raw materials. Due to the large compressibility of the foam metal particles, although part of them are pressed into powder during the pressing process, there are still certain pores in the foam metal particles. During the high-temperature firing stage, the foam metal particles melt into a liquid state, and part of them become oxidized and then change in volume. Since there are still certain pores in the foam metal particles after pressing, the bulging caused by the volume change of the metal after firing can be reduced. In addition, the boron fibers uniformly distributed in the ceramic matrix can serve as a guide rail for the discharge of bubbles, which is conducive to the discharge of bubbles in the ceramic matrix. The boron fibers can provide a skeleton effect, which is conducive to the uniform distribution of irregular metal particles and improves the strength of ceramic tiles.
[0081] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A method for preparing a ceramic tile, characterized in that: The following steps are involved: Wet ball milling the ceramic powder; The ball-milled ceramic powder is magnetically stirred in deionized water; The boron fibers and foamed metal particles ultrasonically dispersed in deionized water are added to the ceramic powder, and then the polyvinyl alcohol solution is added; and a slurry is obtained after a second ultrasonic treatment; Firing to transform the foamed metal particles into irregular metal particles to obtain ceramic bricks; Wherein, the ceramic brick comprises a ceramic matrix and boron fibers and irregular metal particles uniformly distributed in the ceramic matrix; The length of the boron fiber is greater than 400 μm; The mass proportion of the boron fiber in the ceramic matrix is 5% to 10%; The irregular metal particles account for 0.1% to 10% by mass in the ceramic matrix.
2. The preparation method according to claim 1, characterized in that The chemical composition of the ceramic powder is: SiO2: 57-67wt.%, Al2O3: 17-26wt.%, Fe2O3: 0.4-1.1wt.%, TiO2: 0.2-0.5wt.%, CaO: 0.1-0.4wt.%, MgO: 0.2-0.8wt.%, K2O: 1.5-3.5wt.%, Na2O: 1.5-4.5wt.%, P2O3: 0.01-0.07wt.%, SO3: 0.1-0.8wt.%, and loss on ignition: 3-9wt.%.
3. The preparation method according to claim 2, characterized in that: The ultrasonic dispersion time is 30-60 minutes, the secondary ultrasonic time is 2-6 hours, and the mass concentration of the polyvinyl alcohol solution is 5-10%.
4. A ceramic tile prepared according to the preparation method according to any one of claims 1 to 3.
5. The ceramic tile according to claim 4, characterized in that: The diameter of the boron fiber is 20-100 μm.
6. The ceramic tile according to claim 5, characterized in that The length of the boron fiber is 400-700 μm.
7. The ceramic tile according to claim 4, characterized in that: The irregular metal particles include at least one of aluminum particles, copper particles, and nickel particles.
8. Use of the ceramic tile according to any one of claims 4 to 7, characterized in that: Used in venues with floor heating systems.
Citation Information
Patent Citations
Heat-conducting wear-resistant ceramic sleeve and preparation method thereof
CN109503127A
Ceramic green body, ceramic plate and preparation method of ceramic green body
CN113443893A