A kind of high strength mullite insulation brick and preparation method thereof

Through the design of fiber mesh and porous structure, combined with vanadium pentoxide and polystyrene microspheres, the problem of uneven dispersion of mullite fibers and high-aluminum fly ash impurities is solved, and the strength and heat insulation of the insulation bricks are improved. performance, achieving efficient utilization of resources and environmental protection.

CN118495936BActive Publication Date: 2024-10-29洛阳智源再生资源有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410954201.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-29
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The uneven dispersion of mullite fibers in insulating bricks results in a loose structure, and the impurities in high-aluminum fly ash affect the sintering performance, increasing preparation costs and environmental pollution.

Method used

Mullite fibers are used to prepare fiber webs, and the fiber webs are reinforced by silica amine sol spraying, combined with vanadium pentoxide and polystyrene microspheres to form a porous structure and fiber/whisker hierarchical structure to improve the sintering temperature and mechanical properties. .

Benefits of technology

The strength, thermal shock resistance and thermal insulation performance of the insulation bricks are improved, the influence of uneven fiber dispersion and impurities is avoided, the preparation cost is reduced, and the full utilization of resources is promoted.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of thermal insulation bricks, specifically to a high-strength mullite thermal insulation brick and a preparation method thereof, comprising the following process steps: step 1, taking mullite fiber, adding water to disperse, forming a suspension, wet-forming a net, and obtaining a net tire; step 2, spraying silicon boron amine sol on the surface of the net tire, drying, sintering, and obtaining a fiber net; step 3, taking aluminum hydroxide, silicon micropowder, α-alumina, and vanadium pentoxide, pre-burning, and obtaining pre-burned particles; pre-burned particles, polystyrene, dispersant and water are mixed, stirred, and slurry is obtained; superimposed fiber nets, slurry is added again, and repeated multiple times; vibration, static pressure molding, forming a green brick; sintering, and obtaining a thermal insulation brick. The present invention prepares a fiber net through mullite fiber, which can alleviate uneven dispersion in the thermal insulation brick body, avoid the loose brick structure caused by the occurrence of agglomeration, prevent the strength of the thermal insulation brick body from being affected, and promote the uniformity of the thermal insulation brick body structure and performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat-insulating bricks, in particular to a high-strength mullite heat-insulating brick and a preparation method thereof. Background Art

[0002] Mullite is a binary solid solution compound composed of aluminum oxide and calcium oxide. It is the most stable compound in the Al2O3-SiO2 binary phase diagram. Mullite has excellent physical properties, such as high fracture toughness, high temperature resistance, oxidation resistance, thermal shock resistance, creep resistance, low thermal conductivity, strong electrical insulation, and low dielectric constant. As a raw material for thermal insulation bricks, the mullite fiber raw material is flocculent as a whole, entangled together, and not easy to disperse. Direct use will cause uneven dispersion of mullite fibers in the brick body, causing defects in the internal structure of the thermal insulation brick. There are very few natural minerals of mullite. At present, it is mostly synthesized at high temperature using aluminum and silicon raw materials, and the cost of raw materials and preparation process is relatively high. High-aluminum fly ash, as a bulk solid waste, contains a large amount of mullite phase and is a potential mullite resource. However, impurities in high-alumina fly ash will have a negative impact on the sintering of mullite insulation materials. In order to apply high-alumina fly ash to composite materials, dispose of solid waste and make full use of mullite resources, we propose a high-strength mullite insulation brick and a preparation method thereof. Summary of the invention

[0003] The object of the present invention is to provide a high-strength mullite insulation brick and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0004] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing high-strength mullite insulation bricks, comprising the following process steps:

[0005] Step 1: Preparation of mesh:

[0006] The mullite fibers are dispersed in water to form a suspension, and then formed into a web in a wet state to obtain a web matrix;

[0007] Step 2: Deposition of modified substances:

[0008] Spraying borosilicate amine sol on the surface of the web obtained in step 1, drying, and sintering to obtain a fiber web;

[0009] Step 3: Preparation of insulation bricks:

[0010] Aluminum hydroxide, silicon powder, α-alumina, and vanadium pentoxide are mixed, ball-milled, pressed, and pre-calcined to obtain pre-calcined particles;

[0011] The pre-calcined particles, polystyrene, dispersant and water are mixed and stirred to obtain a slurry;

[0012] Put the fiber mesh obtained in step 2 into a mold and add slurry; stack the fiber mesh and add slurry again, repeating the process for multiple times; vibrate and statically press to form a green brick; and sinter to obtain an insulating brick.

[0013] Furthermore, in step 1, the mullite fiber is immersed in the dispersant solution for 10 to 20 minutes before use, and then taken out for use;

[0014] Mullite fiber: average diameter 3.2μm, average length 210mm, sourced from Shandong Luyang Energy Saving Materials Co., Ltd.;

[0015] The ratio of mullite fiber to dispersant solution is (6-9) g:100 mL;

[0016] The concentration of the dispersant solution is 0.6-0.7wt%;

[0017] The dispersant is polyacrylamide, which comes from Tianjin Komiou Chemical Reagent Co., Ltd.

[0018] In the above technical solution, the mullite fiber raw material is flocculent as a whole, entangled together, and difficult to disperse. Direct use will cause uneven dispersion of the mullite fiber in the brick body, causing defects in the internal structure of the manufactured insulation brick. Therefore, before using the mullite fiber, it needs to be treated and immersed in a dispersant solution so that the dispersant is adsorbed on the fiber surface, improving the interaction force between the mullite fibers and enhancing the repulsion between the fibers, thereby preventing the agglomeration of the mullite fibers.

[0019] Further, in step 1, the mass fraction of the mullite fiber in the suspension is 10% to 20%;

[0020] The surface density of the mesh is 100-160g / m 2 ; Thickness is 0.5~1.0mm.

[0021] Furthermore, in step 2, the borosilicate amine sol is prepared by the following process: mix ethyl orthosilicate and anhydrous ethanol, adjust the pH of the system to 6.0-6.5 with dilute nitric acid, and stir for 20-30 minutes; add boric acid / ethylene glycol methyl ether, and stir for 30-60 minutes; heat to 45-50° C., add melamine / anhydrous ethanol, and stir for 40-60 minutes;

[0022] The mass ratio of tetraethyl orthosilicate, boric acid and melamine is 100: (13.7-18.3): (4.7-9.3);

[0023] The volume ratio of ethyl orthosilicate and anhydrous ethanol is 1:1;

[0024] Boric acid / ethylene glycol methyl ether: The mass concentration of boric acid in ethylene glycol methyl ether is 3.5%;

[0025] Melamine / anhydrous ethanol, the mass concentration of melamine in anhydrous ethanol is 3.0%, and the temperature is 45-50°C.

[0026] Furthermore, in step 2, the spraying amount of the borosilicate amine sol is 80 to 100 g / m 2 .

[0027] Furthermore, in step 2, the drying process conditions are: drying at a temperature of 85 to 95° C. for 12 to 18 hours.

[0028] Furthermore, in step 2, the sintering process conditions are: in an argon atmosphere, the gas flow rate is 150 sccm, and the temperature is increased from room temperature to 700-800° C. at a rate of 5-10° C. / h;

[0029] Ammonia gas was introduced at a flow rate of 50 sccm and argon gas at a flow rate of 150 sccm, and the temperature was raised to 1100-1200°C at a rate of 10°C / h, and the temperature was kept at this temperature for 2-4h, and the introduction of ammonia gas was stopped;

[0030] The temperature was lowered to 200°C at a cooling rate of 5°C / min and then naturally cooled to room temperature.

[0031] In the above technical scheme, the formation of the fiber mesh can avoid the uneven dispersion of mullite fibers in the insulating brick body, avoid the loose brick structure caused by the occurrence of agglomeration, prevent the strength of the insulating brick body from being affected, and promote the uniformity of the structure and performance of the insulating brick body. The prepared fiber mesh is treated by spraying and impregnating with wet gel (silicon boron amine sol), and a precursor with a porous structure is formed after drying. Then sintering is carried out, and tetraethyl orthosilicate is hydrolyzed and condensed. After high-temperature sintering, a quartz phase can be formed, but it will undergo multiple phase changes during the sintering process, causing changes in the lattice size and forming defects. The present application uses boric acid as a boron source, and the introduction of boron oxide can improve the stability of the quartz phase, and can reduce the sintering temperature to obtain a sintered product with higher strength. Under the action of surface tension, the liquid phase is more likely to be enriched at the overlapping points of the mullite fibers to reinforce the fiber mesh; under the protection of inert gas, ammonia is used as the active gas and melamine is used as the nitrogen source to sinter and nitride the silicon boron amine sol to obtain silicon boron nitrogen oxide compounds, which improves the mechanical strength of the overlapping points of the mullite fibers and improves its flexibility, which helps to improve the strength and antioxidant properties of the fiber mesh. The resulting insulating bricks have better mechanical properties, thermal shock stability, thermal fatigue performance and other properties.

[0032] Further, in step 3, the pre-calcined particles are prepared from the following components by mass: 55-65 parts of aluminum hydroxide, 30-35 parts of silicon powder, 9-12 parts of alpha alumina, and 3.2-5.6 parts of vanadium pentoxide;

[0033] The process conditions of ball milling are as follows: dry ball milling until all components pass through a 250-mesh sieve;

[0034] The pressing process conditions are: water spray granulation, sealed aging for 24 hours, and pressing at a pressure of 8-10MPa;

[0035] The pre-burning process conditions are: pre-burning temperature 780-820°C, heat preservation 28-35 minutes; after pre-burning, crush until all pass through a 120-mesh sieve.

[0036] Furthermore, aluminum hydroxide is prepared from aluminum ash, and the specific preparation process is as follows:

[0037] Mix aluminum ash and water, introduce carbon dioxide into a reactor at a rate of 40 mL / min, and heat to 20-77°C for 3-5 hours to decompose aluminum nitride in the aluminum ash; the ratio of aluminum ash to water is (10-20) g / 100 mL;

[0038] Then filter, take the precipitate, add hydrochloric acid and hydrogen peroxide, and ball mill for 2 to 5 hours to decompose the metallic aluminum in the precipitate; the ratio of precipitate, dilute hydrochloric acid, and hydrogen peroxide is (20 to 30) g: (20 to 30) mL: (1 to 3) mL; the ball-to-material ratio is (3 to 5): 1;

[0039] Slowly add 25-40wt% sodium hydroxide until the system pH is 10-12, with an addition rate of 7-10mL / min; react at 80-100°C for 1-5h, filter, wash, and dry to obtain aluminum hydroxide with a yield of about 80%.

[0040] Aluminum ash: specification 200μm, sourced from Yichuan Yugang Longquan Aluminum Co., Ltd.; composition as follows: by mass, 50.2% Al2O3, 21.7% Al, 9.7% AlN, 3.2% SiO2, and the remainder is impurities;

[0041] Silica powder: The ingredients are as follows: SiO2 ≥ 99.0%, Al2O3 ≤ 0.3%, Fe2O3 ≤ 0.02%, specification 0.1 ~ 0.3μm, from Luoyang Yumin Micro Silica Powder Co., Ltd.;

[0042] α-alumina: α-Al2O3 powder composition is as follows: Al2O3 ≥ 99.0%, SiO2 ≤ 0.02%, Fe2O3 ≤ 0.03%, Na2O ≤ 0.1%; brand AW-12M, from Henan Hecheng Inorganic New Materials Co., Ltd.;

[0043] Further, in step 3, the slurry includes the following components by mass: 97-117 parts of pre-calcined particles, 10-11 parts of polystyrene, 0.43-0.44 parts of dispersant, and 54-56 parts of water;

[0044] Polystyrene: spherical, particle size 0.5-1.0 mm, from Suzhou Zhiyi Microsphere Technology Co., Ltd.;

[0045] Furthermore, in step 3, the mass ratio of slurry to fiber web is 100:(15-25).

[0046] Furthermore, in step 3, the static pressure molding pressure is 17-22 MPa.

[0047] Furthermore, in step 3, the drying process conditions are: 190-210° C., and drying for 4-6 hours.

[0048] Furthermore, in step 3, the sintering process conditions are: heating to 500-530°C at a rate of 20°C / h, and keeping warm for 4 hours; heating to 950-1000°C within 3 hours, and keeping warm for 10 hours; heating to 1300-1350°C within 4 hours, and keeping warm for 5 hours; heating to 1600-1650°C within 4 hours, and keeping warm for 10 hours; and naturally cooling in the furnace.

[0049] In the above technical scheme, vanadium pentoxide is added to the aluminum silicon matrix. Due to its low melting point, it can form a low-temperature liquid phase, improve the material transfer rate, reduce the reaction activation energy, promote the solid phase reaction between silicon dioxide and aluminum hydroxide, increase the rate of nucleus formation, and promote the increase of the size of mullite whiskers. The introduction of the fiber mesh can serve as a crystal nucleus. With the assistance of the liquid phase of vanadium pentoxide, it promotes the precipitation of vertically grown mullite whiskers on its surface, interweaving to form a mesh structure, and obtaining a fiber / whisker hierarchical structure. Affected by the effects of structural bridging and pinning, the strength of the prepared insulation brick is further improved. The use of aluminum fluoride is avoided, and the aluminum silicon compound in the fiber mesh is prevented from reacting with the gas phase, and the decomposition during the growth of mullite whiskers affects the strength and other properties of the fiber mesh, thereby degrading the performance of the prepared insulation brick. With the increase of the vanadium pentoxide content, the mullite content in the insulation brick body gradually increases. Excessive vanadium pentoxide will lead to the formation of a glass phase, which is not conducive to the strength and high-temperature insulation performance of the insulation brick. Too high a sintering temperature will cause a sharp increase in the material transfer rate, and the local concentration of the reactants will be too high, exceeding the amount required for the rapid directional growth of the whiskers. The growth of the whiskers in other directions will intensify, resulting in a decrease in the difference in the growth rates of the whiskers and an increase in the diameter of the mullite whiskers, which is not conducive to the establishment of the fiber / whisker network structure and the improvement of the performance of the insulation brick.

[0050] Using aluminum ash as the aluminum source in the preparation of insulation bricks can reduce the pollution of industrial solid waste to the environment and increase its economic and social value and resource utilization value. However, aluminum ash contains oxide impurities such as metal titanium, calcium, and iron, which will affect the performance of mullite bricks. Therefore, before preparing insulation bricks, the aluminum ash is treated and used as a raw material to prepare aluminum hydroxide; the obtained aluminum hydroxide is used as a mullite precursor, which can effectively eliminate the negative impact of impurities in the preparation of mullite insulation bricks and make full use of aluminum-rich resources. In the process of preparing aluminum hydroxide using aluminum ash as a raw material, aluminum ash is first mixed with water, and aluminum nitride in the aluminum ash is hydrolyzed to generate Al (OH) 3 and release ammonia. Carbon dioxide is introduced to neutralize the ammonia to achieve denitrification of aluminum ash and elution of soluble salts. Then the precipitate is mixed with leaching medium hydrochloric acid and co-solvent hydrogen peroxide, and the aluminum ash is mechanically activated by ball milling to leach the aluminum element; then alkali solution is added to react and aluminum hydroxide is precipitated, thereby obtaining aluminum hydroxide as a component of insulation bricks. The addition of vanadium pentoxide helps its sintering performance and improves the mechanical properties and structural uniformity of the produced insulation bricks.

[0051] The burn-out method is adopted, and polystyrene microspheres are used as pore-forming agents. Polystyrene undergoes oxidation and decomposition during the sintering process to produce gas and leave pores, forming holes in the insulating brick body, the matrix continuity becomes worse, the heat conduction path becomes longer, and the thermal insulation capacity of the brick body is improved, thereby preparing a brick body with thermal insulation performance; its bulk density is reduced, and the effect of the fiber mesh can alleviate the impact of the holes on the strength of the brick body, and it has more long-lasting and stable thermal fatigue resistance and strength, thermal insulation and other properties. Polystyrene oxidative degradation can form a carbon layer, and the gas produced reduces the supersaturation of the reactants, which is conducive to the formation of whiskers; the pores formed by the oxidative degradation of polystyrene can also provide growth space for whiskers, which is conducive to the development of whiskers.

[0052] However, due to factors such as structure and atmosphere, the polystyrene inside the brick may be incompletely burned to form a carbon layer. The oxygen in the silicon, boron, nitrogen and oxygen on the surface of the fiber mesh is reduced, and the boron element can diffuse into the polystyrene through self-diffusion at high temperature and enter the carbon lattice, catalyzing and promoting the graphitization of the polystyrene carbon layer, accelerating its recrystallization rate, making the crystal growth more perfect, the interlayer spacing of the graphite reduced, and the orientation degree increased, thereby obtaining an insulating brick with partial graphite, which helps to alleviate the negative impact of the carbon layer formed by polystyrene on the brick body and improve the mechanical properties and dimensional stability of the brick body.

[0053] Compared with the prior art, the present invention has the following beneficial effects:

[0054] 1. The high-strength mullite insulation brick and preparation method thereof of the present invention prepares a fiber mesh by using mullite fibers, which can alleviate the uneven dispersion in the insulation brick body, avoid the loose brick structure caused by the occurrence of agglomeration, prevent the strength of the insulation brick body from being affected, and promote the uniformity of the insulation brick body structure and performance.

[0055] 2. The high-strength mullite insulation brick and preparation method thereof of the present invention treat the fiber web by spraying silicon boron amine sol. Under the action of surface tension, the liquid phase is enriched at the overlapping points of the mullite fibers, the fiber web is reinforced, and nitridation is performed to obtain silicon boron nitride compounds, which improves the mechanical strength of the overlapping points, increases its flexibility, and contributes to improving the strength and oxidation resistance of the fiber web. The insulation bricks thus prepared have better mechanical properties, thermal shock stability, thermal fatigue performance and other properties.

[0056] 3. The high-strength mullite thermal insulation brick and its preparation method of the present invention can form a low-temperature liquid phase by adding vanadium pentoxide with a low melting point into the thermal insulation brick matrix, thereby improving the material transfer rate, promoting the solid phase reaction between silicon dioxide and aluminum oxide, increasing the rate of crystal nucleus formation, and promoting the increase in the size of mullite whiskers; the fiber mesh serves as the crystal nucleus, and the vertically grown mullite whiskers precipitated on its surface are interwoven to form a network structure, thereby obtaining a fiber / whisker hierarchical structure, which further improves the strength of the thermal insulation brick; and it is helpful to the sintering performance of the thermal insulation brick matrix, and improves the mechanical properties and structural uniformity of the prepared thermal insulation brick.

[0057] 4. The high-strength mullite insulation brick and its preparation method of the present invention use polystyrene microspheres as pore-forming agents and adopt the burn-out method. During the sintering process, polystyrene undergoes oxidation and decomposition to produce gas and leave pores to form holes, thereby preparing a brick body with heat-insulating properties. The polystyrene is oxidatively degraded, and the gas produced can reduce the supersaturation of the reactants, which is beneficial to the formation of whiskers. The produced pores can also provide growth space for whiskers, which is beneficial to the development of whiskers. During sintering, the oxygen in the silicon, boron, nitrogen and oxygen on the surface of the fiber mesh is reduced, and the boron element diffuses into the polystyrene through self-diffusion and enters the carbon lattice, catalyzing and promoting the graphitization of the polystyrene carbon layer, which helps to alleviate the negative impact of the formation of the carbon layer of polystyrene on the brick body and improve the mechanical properties and dimensional stability of the brick body. DETAILED DESCRIPTION

[0058] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0059] In the following specific implementations,

[0060] Mullite fiber: average diameter 3.2μm, average length 210mm, sourced from Shandong Luyang Energy Saving Materials Co., Ltd.;

[0061] Dispersant polyacrylamide: from Tianjin Komiou Chemical Reagent Co., Ltd.;

[0062] Aluminum ash: specification 200μm, sourced from Yichuan Yugang Longquan Aluminum Co., Ltd.; composition as follows: by mass, 50.2% Al2O3, 21.7% Al, 9.7% AlN, 3.2% SiO2, and the remainder is impurities;

[0063] Aluminum hydroxide is made from aluminum ash, and the specific preparation process is as follows:

[0064] Mix aluminum ash and water, introduce carbon dioxide into the reactor at a rate of 40 mL / min, and heat to 20°C for 5 hours to decompose the aluminum nitride in the aluminum ash; the ratio of aluminum ash to water is 10 g / 100 mL;

[0065] Then filter, take the precipitate, add hydrochloric acid and hydrogen peroxide, and ball mill for 5 hours to decompose the metal aluminum in the precipitate; the ratio of precipitate, dilute hydrochloric acid, and hydrogen peroxide is 20g:25mL:2mL; the ball-to-material ratio is 3:1;

[0066] Slowly add 25-40wt% sodium hydroxide until the pH of the system is 11, and the addition rate is 8mL / min; react at 90°C for 5h, filter, wash, and dry to obtain aluminum hydroxide with a yield of about 80%;

[0067] Silica powder: The ingredients are as follows: SiO2 ≥ 99.0%, Al2O3 ≤ 0.3%, Fe2O3 ≤ 0.02%, specification 0.1 ~ 0.3μm, from Luoyang Yumin Micro Silica Powder Co., Ltd.;

[0068] α-alumina: α-Al2O3 powder composition is as follows: Al2O3 ≥ 99.0%, SiO2 ≤ 0.02%, Fe2O3 ≤ 0.03%, Na2O ≤ 0.1%; brand AW-12M, from Henan Hecheng Inorganic New Materials Co., Ltd.;

[0069] Polystyrene: spherical, KBsphere 0.8PS, from Suzhou Zhiyi Microsphere Technology Co., Ltd.;

[0070] Vanadium pentoxide: analytical grade, sourced from San Chemical Technology (Shanghai) Co., Ltd.

[0071] Embodiment 1: A method for preparing high-strength mullite insulation bricks, comprising the following process steps:

[0072] Step 1: Preparation of mesh:

[0073] Take mullite fiber, immerse it in 0.6wt% dispersant polyacrylamide solution for 20min, take it out for use, the ratio of mullite fiber to dispersant solution is 6g:100mL; add water to disperse to form a suspension with a mass fraction of 10%; wet-form a net to obtain a surface density of 120g / m 2 , mesh tire with a thickness of 0.8mm;

[0074] Step 2: Deposition of modified substances:

[0075] Take tetraethyl orthosilicate and anhydrous ethanol and mix them in a volume ratio of 1:1, use 1M dilute nitric acid to adjust the pH of the system to 6.5, and stir for 20 minutes; add boric acid / ethylene glycol methyl ether with a mass concentration of 3.5%, and stir for 30 minutes; heat to 45°C, add melamine / anhydrous ethanol with a mass concentration of 3.0% and a temperature of 45°C, and stir for 40 minutes to form a silicon boroamine sol; the mass ratio of tetraethyl orthosilicate, boric acid, and melamine is 100:13.7:4.7;

[0076] The surface of the mesh obtained in step 1 is sprayed with borosilicate amine sol, and the spraying amount of borosilicate amine sol is 80g / m 2 ; Drying, the drying process conditions are: drying at 85°C for 18h; sintering, the sintering process conditions are: in an argon atmosphere, the gas flow rate is 150sccm, and the temperature is raised from room temperature to 700°C at a rate of 10°C / h; ammonia is introduced, the ammonia gas flow rate is 50sccm, the argon gas flow rate is 150sccm, the temperature is raised to 1100°C at a rate of 10°C / h, and the temperature is kept for 4h, and the introduction of ammonia is stopped; the temperature is lowered to 200°C at a cooling rate of 5°C / min, and naturally cooled to room temperature to obtain a fiber mesh;

[0077] Step 3: Preparation of insulation bricks:

[0078] Aluminum hydroxide, silicon micropowder, α-alumina, and vanadium pentoxide are mixed, dry-milled until all components pass through a 250-mesh sieve, granulated by water spraying, sealed and aged for 24 hours, and pressed into shape at a pressure of 8MPa; pre-calcined, the process conditions are: pre-calcined temperature 780°C, heat preservation for 35 minutes; after pre-calcined, crushed until all components pass through a 120-mesh sieve to obtain pre-calcined particles; the pre-calcined particles are prepared from the following mass components: 55 parts of aluminum hydroxide, 30 parts of silicon micropowder, 9 parts of α-alumina, and 3.2 parts of vanadium pentoxide;

[0079] The pre-burned particles, polystyrene, dispersant and water are mixed and stirred to obtain a slurry; the slurry includes the following components by weight: 97 parts of pre-burned particles, 10 parts of polystyrene, 0.43 parts of dispersant polyacrylamide and 56 parts of water;

[0080] Put the fiber mesh obtained in step 2 into a mold and add slurry; superimpose the fiber mesh, add slurry again, and repeat 10 times; the mass ratio of slurry to fiber mesh is 100:15; vibrate and statically press to form a green brick at a pressure of 17 MPa; dry, and the drying process conditions are: dry at 190°C for 6 hours; sinter, and the sintering process conditions are: heat to 500°C at a rate of 20°C / h, and keep warm for 4 hours; heat to 950°C within 3 hours, and keep warm for 10 hours; heat to 1300°C within 4 hours, and keep warm for 5 hours; heat to 1600°C within 4 hours, and keep warm for 10 hours; cool naturally in the furnace to obtain insulating bricks.

[0081] Embodiment 2: A method for preparing high-strength mullite insulation bricks, comprising the following process steps:

[0082] Step 1: Preparation of mesh:

[0083] Take mullite fiber, immerse it in 0.65wt% dispersant polyacrylamide solution for 15min, take it out for use, the ratio of mullite fiber to dispersant solution is 8g:100mL; add water to disperse to form a suspension with a mass fraction of 10%; wet-form a net to obtain a surface density of 120g / m 2 , mesh tire with a thickness of 0.8mm;

[0084] Step 2: Deposition of modified substances:

[0085] Take tetraethyl orthosilicate and anhydrous ethanol and mix them in a volume ratio of 1:1, use 1M dilute nitric acid to adjust the pH of the system to 6.2, and stir for 25 minutes; add boric acid / ethylene glycol methyl ether with a mass concentration of 3.5%, and stir for 45 minutes; heat to 48°C, add melamine / anhydrous ethanol with a mass concentration of 3.0% and a temperature of 48°C, and stir for 50 minutes to form a silicon boroamine sol; the mass ratio of tetraethyl orthosilicate, boric acid, and melamine is 100:16.0:7.0;

[0086] The surface of the mesh obtained in step 1 is sprayed with borosilicate amine sol, and the spraying amount of borosilicate amine sol is 90g / m 2 ; Drying, the drying process conditions are: drying at 90°C for 15h; sintering, the sintering process conditions are: in an argon atmosphere, the gas flow rate is 150sccm, and the temperature is raised from room temperature to 750°C at a rate of 8°C / h; ammonia is introduced, the ammonia gas flow rate is 50sccm, the argon gas flow rate is 150sccm, the temperature is raised to 1150°C at a rate of 10°C / h, and the temperature is kept for 3h, and the introduction of ammonia is stopped; the temperature is lowered to 200°C at a cooling rate of 5°C / min, and naturally cooled to room temperature to obtain a fiber mesh;

[0087] Step 3: Preparation of insulation bricks:

[0088] Aluminum hydroxide, silicon micropowder, α-alumina, and vanadium pentoxide are mixed, dry-milled until all components pass through a 250-mesh sieve, granulated by water spraying, sealed and aged for 24 hours, and pressed into shape at a pressure of 9 MPa; pre-calcined, the process conditions are: pre-calcined temperature 800°C, heat preservation for 30 minutes; after pre-calcined, crushed until all pass through a 120-mesh sieve to obtain pre-calcined particles; the pre-calcined particles are prepared from the following mass components: 60 parts of aluminum hydroxide, 32 parts of silicon micropowder, 10 parts of α-alumina, and 4.4 parts of vanadium pentoxide;

[0089] The pre-burned particles, polystyrene, dispersant and water are mixed and stirred to obtain a slurry; the slurry includes the following components by weight: 107 parts of pre-burned particles, 10.5 parts of polystyrene, 0.44 parts of dispersant polyacrylamide and 55 parts of water;

[0090] Put the fiber mesh obtained in step 2 into a mold and add slurry; superimpose the fiber mesh, add slurry again, and repeat 10 times; the mass ratio of slurry to fiber mesh is 100:20; vibrate and statically press to form a green brick at a pressure of 20 MPa; dry at 200°C for 5 hours; sinter, and the sintering process conditions are as follows: heat to 5150°C at a rate of 20°C / h, and keep warm for 4 hours; heat to 976°C within 3 hours, and keep warm for 10 hours; heat to 1325°C within 4 hours, and keep warm for 5 hours; heat to 1625°C within 4 hours, and keep warm for 10 hours; cool naturally in the furnace to obtain insulating bricks.

[0091] Embodiment 3: A method for preparing high-strength mullite insulation bricks, comprising the following process steps:

[0092] Step 1: Preparation of mesh:

[0093] Take mullite fiber, immerse it in 0.7wt% dispersant polyacrylamide solution for 10 minutes, take it out for use, the ratio of mullite fiber to dispersant solution is 9g:100mL; add water to disperse to form a suspension with a mass fraction of 10%; wet-form a net to obtain a surface density of 120g / m 2 , mesh tire with a thickness of 0.8mm;

[0094] Step 2: Deposition of modified substances:

[0095] Take tetraethyl orthosilicate and anhydrous ethanol and mix them in a volume ratio of 1:1, use 1M dilute nitric acid to adjust the pH of the system to 6.0, and stir for 30 minutes; add boric acid / ethylene glycol methyl ether with a mass concentration of 3.5%, and stir for 60 minutes; heat to 50°C, add melamine / anhydrous ethanol with a mass concentration of 3.0% and a temperature of 50°C, and stir for 60 minutes to form a borosilicate amine sol; the mass ratio of tetraethyl orthosilicate, boric acid, and melamine is 100:18.3:9.3;

[0096] The surface of the mesh obtained in step 1 is sprayed with borosilicate amine sol, and the spraying amount of borosilicate amine sol is 100g / m 2 ; Drying, the drying process conditions are: drying at a temperature of 95°C for 18 hours; sintering, the sintering process conditions are: in an argon atmosphere, the gas flow rate is 150sccm, and the temperature is raised from room temperature to 800°C at a rate of 10°C / h; ammonia is introduced, the ammonia gas flow rate is 50sccm, the argon gas flow rate is 150sccm, the temperature is raised to 1200°C at a rate of 10°C / h, and the temperature is kept for 4 hours, and the introduction of ammonia is stopped; the temperature is lowered to 200°C at a cooling rate of 5°C / min, and naturally cooled to room temperature to obtain a fiber mesh;

[0097] Step 3: Preparation of insulation bricks:

[0098] Aluminum hydroxide, silicon micropowder, α-alumina, and vanadium pentoxide are mixed, dry-milled until all components pass through a 250-mesh sieve, granulated by water spraying, sealed and aged for 24 hours, and pressed into shape at a pressure of 10 MPa; pre-calcined, the process conditions are: pre-calcined temperature 820°C, heat preservation for 28 minutes; after pre-calcined, crushed until all components pass through a 120-mesh sieve to obtain pre-calcined particles; the pre-calcined particles are prepared from the following mass components: 65 parts of aluminum hydroxide, 35 parts of silicon micropowder, 12 parts of α-alumina, and 5.6 parts of vanadium pentoxide;

[0099] The pre-burned particles, polystyrene, dispersant and water are mixed and stirred to obtain a slurry; the slurry includes the following components by weight: 117 parts of pre-burned particles, 11 parts of polystyrene, 0.44 parts of dispersant polyacrylamide and 54 parts of water;

[0100] Put the fiber mesh obtained in step 2 into a mold and add slurry; superimpose the fiber mesh, add slurry again, and repeat 10 times; the mass ratio of slurry to fiber mesh is 100:25; vibrate and statically press to form a green brick at a pressure of 22 MPa; dry, and the drying process conditions are: dry at 210°C for 4 hours; sinter, and the sintering process conditions are: heat to 530°C at a rate of 20°C / h, and keep warm for 4 hours; heat to 1000°C within 3 hours, and keep warm for 10 hours; heat to 1350°C within 4 hours, and keep warm for 5 hours; heat to 1650°C within 4 hours, and keep warm for 10 hours; cool naturally in the furnace to obtain insulating bricks.

[0101] Comparative Example 1: A method for preparing a high-strength mullite insulation brick, comprising the following process steps:

[0102] Step 1: Preparation of mesh:

[0103] Take mullite fiber, immerse it in 0.6wt% dispersant polyacrylamide solution for 20min, take it out for use, the ratio of mullite fiber to dispersant solution is 6g:100mL; add water to disperse to form a suspension with a mass fraction of 10%; wet-form a net to obtain a surface density of 120g / m2 , mesh tire with a thickness of 0.8mm;

[0104] Step 2: Deposition of modified substances:

[0105] Take tetraethyl orthosilicate and anhydrous ethanol and mix them in a volume ratio of 1:1, use 1M dilute nitric acid to adjust the pH of the system to 6.5, and stir for 20 minutes; add 3.5% boric acid / ethylene glycol methyl ether and 5% metallic sodium / anhydrous ethanol, and stir for 30 minutes to form a sol; the mass ratio of tetraethyl orthosilicate, boric acid, and metallic sodium is 100:13.7:1.85;

[0106] The surface of the mesh obtained in step 1 is sprayed with sol, and the spraying amount of sol is 80g / m 2 ; Drying, the drying process conditions are: drying at 85°C for 18h; sintering, the sintering process conditions are: in an argon atmosphere, the gas flow rate is 150sccm, the temperature is increased from room temperature to 700°C at a rate of 10°C / h; the temperature is reduced to 200°C at a cooling rate of 5°C / min, and naturally cooled to room temperature to obtain a fiber mesh;

[0107] The other process steps are the same as those in Example 1 to obtain thermal insulation bricks.

[0108] Comparative Example 2: A method for preparing high-strength mullite insulation bricks, comprising the following process steps:

[0109] Step 3: Preparation of insulation bricks:

[0110] Aluminum hydroxide, silicon micropowder, α-alumina, polystyrene, a dispersant and water are mixed and stirred to obtain a slurry; the slurry includes the following components by weight: 55 parts of aluminum hydroxide, 30 parts of silicon micropowder, 9 parts of α-alumina, 10 parts of polystyrene, 0.43 parts of a dispersant polyacrylamide and 56 parts of water;

[0111] The other process steps are the same as those in Comparative Example 1 to obtain thermal insulation bricks.

[0112] Comparative Example 3: A method for preparing high-strength mullite insulation bricks, comprising the following process steps:

[0113] Take mullite fiber, immerse it in 0.6wt% dispersant polyacrylamide solution for 20 minutes, and then take it out for use. The ratio of mullite fiber to dispersant solution is 6g:100mL;

[0114] Aluminum hydroxide, silicon micropowder, α-alumina, mullite fiber, polystyrene, a dispersant and water are mixed and stirred to obtain a slurry; the slurry includes the following components by weight: 55 parts of aluminum hydroxide, 30 parts of silicon micropowder, 9 parts of α-alumina, 36 parts of mullite fiber, 10 parts of polystyrene, 0.43 parts of dispersant polyacrylamide and 108 parts of water;

[0115] Vibration and static pressing with a pressure of 17MPa to form a green brick; drying, the drying process conditions are: drying at 190℃ for 6h; sintering, the sintering process conditions are: heating to 500℃ at a rate of 20℃ / h, keeping warm for 4h; heating to 950℃ within 3h, keeping warm for 10h; heating to 1300℃ within 4h, keeping warm for 5h; heating to 1600℃ within 4h, keeping warm for 10h; natural cooling in the furnace to obtain insulating bricks.

[0116] Take the insulating bricks obtained in Examples 1-3 and Comparative Examples 1-3, prepare samples, test their properties respectively and record the test results:

[0117] Apparent porosity and bulk density test: Use an apparent porosity tester and GB 2997 as the reference standard to test the apparent porosity and bulk density of the sample;

[0118] Mechanical properties test: Based on GB 5072 as the reference standard, the insulation brick samples were tested for compressive strength at room temperature with a pressure rate of 1MPa / s; based on GB 3001 as the reference standard, the insulation brick samples were tested for flexural strength;

[0119] Thermal insulation performance test: Taking YB / T 4130 as the reference standard, the water flow plate method is used to test the thermal conductivity of the insulation brick sample as the performance index, the heating rate is 10℃ / min, and the thermal conductivity of the 800℃ sample is tested;

[0120] Thermal shock resistance test: With YB / T 4118 as the reference standard, the insulation brick sample was heated to 1200℃ at a heating rate of 5℃ / min, kept warm for 20 minutes, and then placed on a non-ventilated shelf and naturally cooled to room temperature. The flexural strength was tested again, and the residual strength obtained was compared with the initial flexural strength to calculate the residual strength retention rate of the sample;

[0121]

[0122] According to the data in the above table, we can clearly draw the following conclusions:

[0123] The insulation bricks obtained in Examples 1-3 are compared with the insulation bricks obtained in Comparative Examples 1-3. The test results show that:

[0124] Compared with the comparative example, the insulating bricks obtained in Examples 1-3 have better compressive strength, flexural strength, thermal conductivity and residual strength retention rate data, which fully demonstrates that the present invention achieves improvement in the strength, thermal insulation and thermal shock resistance of the insulating bricks.

[0125] Compared with Example 1, there are obvious technical differences in the preparation process of the insulating bricks obtained in Examples 1-3, and the compressive strength, flexural strength, thermal conductivity and residual strength retention data are deteriorated. It can be seen that the setting of the fiber mesh and insulating brick process and the components used in the present invention can promote the comprehensive improvement of the strength, thermal insulation and thermal shock resistance of the prepared insulating bricks.

[0126] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0127] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing high-strength mullite insulation bricks, characterized in that: The process steps include: Step 1: Preparation of mesh: The mullite fibers are dispersed in water to form a suspension, and then formed into a web in a wet state to obtain a web matrix; Step 2: Deposition of modified substances: Spraying borosilicate amine sol on the surface of the web obtained in step 1, drying, and sintering to obtain a fiber web; Step 3: Preparation of insulation bricks: Aluminum hydroxide, silicon powder, α-alumina, and vanadium pentoxide are mixed, ball-milled, pressed, and pre-calcined to obtain pre-calcined particles; The pre-calcined particles, polystyrene, dispersant and water are mixed and stirred to obtain a slurry; Put the fiber mesh obtained in step 2 into the mold and add slurry; stack the fiber mesh and add slurry again, repeating several times; vibrate and statically press to form a green brick; Sintering to obtain insulation bricks; In step 1, the mullite fiber is immersed in the dispersant solution for 10 to 20 minutes before use, and then taken out for use.

2. The method for preparing a high-strength mullite insulation brick according to claim 1, characterized in that: In step 2, the borosilicate amine sol is prepared by the following process: mix ethyl orthosilicate and anhydrous ethanol, adjust the pH of the system to 6.0-6.5 with dilute nitric acid, and stir for 20-30 minutes; add ethylene glycol methyl ether solution of boric acid, and stir for 30-60 minutes; heat to 45-50° C., add anhydrous ethanol solution of melamine, and stir for 40-60 minutes.

3. The method for preparing a high-strength mullite insulation brick according to claim 2, characterized in that: The mass ratio of the tetraethyl orthosilicate, boric acid and melamine is 100:(13.7-18.3):(4.7-9.3).

4. The method for preparing a high-strength mullite insulation brick according to claim 3, characterized in that: In step 2, the spraying amount of the borosilicate amine sol is 80 to 100 g / m 2 .

5. The method for preparing a high-strength mullite insulation brick according to claim 4, characterized in that: In step 2, the sintering process conditions are: in an argon atmosphere, the gas flow rate is 150 sccm, and the temperature is increased from room temperature to 700-800° C. at a rate of 5-10° C. / h; Ammonia gas was introduced at a flow rate of 50 sccm and argon gas at a flow rate of 150 sccm, and the temperature was raised to 1100-1200°C at a rate of 10°C / h, and the temperature was kept at this temperature for 2-4h, and the introduction of ammonia gas was stopped; The temperature was lowered to 200°C at a cooling rate of 5°C / min and then naturally cooled to room temperature.

6. The method for preparing a high-strength mullite insulation brick according to claim 1, characterized in that: In step 3, the pre-calcined particles are prepared from the following components by mass: 55-65 parts of aluminum hydroxide, 30-35 parts of silicon powder, 9-12 parts of alpha alumina, and 3.2-5.6 parts of vanadium pentoxide; The slurry includes the following components by mass: 97-117 parts of pre-burned particles, 10-11 parts of polystyrene, 0.43-0.44 parts of dispersant and 54-56 parts of water.

7. The method for preparing a high-strength mullite insulation brick according to claim 6, characterized in that: In step 3, the mass ratio of slurry to fiber web is 100:(15-25).

8. The method for preparing a high-strength mullite insulation brick according to claim 7, characterized in that: In step 3, the sintering process conditions are: heating to 500-530°C at a rate of 20°C / h, keeping warm for 4 hours; heating to 950-1000°C within 3 hours, keeping warm for 10 hours; heating to 1300-1350°C within 4 hours, keeping warm for 5 hours; heating to 1600-1650°C within 4 hours, keeping warm for 10 hours; and naturally cooling in the furnace.

9. The method for preparing a high-strength mullite insulation brick according to claim 1, characterized in that: In the step 1, the mass fraction of the mullite fiber in the suspension is 10% to 20%; The surface density of the mesh is 100-160g / m 2 ; Thickness is 0.5~1.0mm.

10. A high-strength mullite insulation brick prepared according to the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for preparing mullite fiber or mullilte whisker high-temperature structural material

    CN104446578A

  • Mullite fiber provided with SiBCN coating deposited on surface and preparation method of mullite fiber

    CN104609892A