A carbon fiber reinforced multiphase ceramic matrix composite material and its preparation method and application
By introducing Ti powder and resin slurry into C/C-SiC composite materials for in-situ reaction to form fine-grained TiC and island-like resin carbon, the problem of residual Si and uneven ceramic phases in existing materials is solved, and the mechanical properties are improved. and friction properties, and improves high-temperature stability and lubricity through uniformly distributed TiC and ZrC.
Patent Information
- Application Number
- CN202410563708.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-08
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-05-08
AI Technical Summary
The existing C/C-SiC composite materials have high content of residual Si and uneven ceramic phase distribution during the preparation process, resulting in poor friction and high-temperature mechanical properties, and lack of lubricating components, resulting in large wear and tear during friction braking. The noise and vibration are strong, and the friction is unstable.
After pretreatment with a carbon fiber preform, a pyrolytic carbon matrix is introduced, followed by impregnation, cross-linking and solidification, cracking carbonization and heat treatment in a resin slurry containing Ti powder to form a C/C-TiC body and embedded in it. Silicon and zirconium mixed powder Reactive infiltration is carried out in the process to produce carbon fiber reinforced multi-phase ceramic matrix composite materials. The violent in-situ reaction during the resin carbonization process is used to form fine-grained TiC and island-like soft resin carbon, which uniformly distributes the ceramic phase, reduces residual Si and improves lubrication. sex.
The material's mechanical properties, thermal shock resistance and friction properties are significantly improved, the wear rate is reduced, friction stability and wear resistance are improved, and high-temperature mechanical properties and oxidation resistance are improved through uniformly distributed TiC and ZrC.
Smart Images

Figure CN118495976B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ceramic matrix composite materials, and in particular relates to a carbon fiber reinforced multiphase ceramic matrix composite material and a preparation method and application thereof. Background Art
[0002] As a new generation of high-performance friction materials, C / C-SiC composite materials have the advantages of low density, wear resistance, smooth braking, oxidation resistance, high temperature resistance, corrosion resistance, strong environmental applicability and long life. They have good application prospects in aircraft braking systems, high-speed train braking systems, maglev train braking systems, automobile braking systems, engineering machinery braking systems and other fields.
[0003] At present, the preparation methods of C / C-SiC composite materials mainly include chemical vapor deposition, precursor impregnation and cracking, and reactive infiltration. Among them, reactive infiltration has become the mainstream method for large-scale production of low-cost C / C-SiC composites due to its advantages such as short preparation cycle, low cost, near net shape, and residual porosity of materials. The basic principle of this method is to use the capillary force generated by the interconnected pores inside the porous C / C composite material to introduce Si melt and react with C to form a SiC matrix, and finally obtain a C / C-SiC composite material. However, the C / C-SiC composite material prepared by reactive infiltration usually has a high content of residual Si inside, which may cause greater wear and obvious thermal decay during braking, thereby affecting the friction performance and high-temperature mechanical properties of the material. In addition, the C / C-SiC composite material prepared by reactive infiltration often has an uneven ceramic phase segregation distribution, which is very likely to cause the friction brake material to produce problems such as loud noise, strong vibration, and unstable friction during use. In addition, C / C-SiC composite materials only contain a single SiC ceramic component and usually lack sufficient lubricating components and have poor adjustability, which will lead to excessively high friction coefficients and poor braking stability during braking.
[0004] In summary, it is very necessary to provide a carbon fiber reinforced multiphase ceramic matrix composite material and its preparation method and application. Summary of the invention
[0005] In order to solve one or more technical problems existing in the prior art, the present invention provides a carbon fiber reinforced multiphase ceramic matrix composite material and a preparation method and application thereof.
[0006] In a first aspect, the present invention provides a method for preparing a carbon fiber reinforced multiphase ceramic matrix composite material, the method comprising the following steps:
[0007] (1) pretreating a carbon fiber preform, and then introducing a pyrolytic carbon matrix into the pretreated carbon fiber preform to obtain a C / C blank;
[0008] (2) placing the C / C body in a resin slurry containing Ti powder for impregnation, and then cross-linking, solidifying, cracking, carbonizing and heat treating to obtain a C / C-TiC body; the resin slurry containing Ti powder is prepared from furan resin, phosphoric acid aqueous solution, cellulose acetate butyrate, polyvinyl pyrrolidone and Ti powder;
[0009] (3) The C / C-TiC blank is embedded in a silicon-zirconium mixed powder for reactive infiltration to obtain a carbon fiber reinforced multiphase ceramic matrix composite material.
[0010] Preferably, when preparing the resin slurry containing Ti powder, the mass ratio of the furan resin, the phosphoric acid aqueous solution, the cellulose acetate butyrate, the polyvinyl pyrrolidone and the Ti powder is (40-88): (5-10): (1-10): (1-10): (5-30).
[0011] Preferably, the resin slurry containing Ti powder is prepared by adding furan resin, phosphoric acid aqueous solution, cellulose acetate butyrate, polyvinyl pyrrolidone and Ti powder into a planetary mixer and mixing for 1 to 10 hours; the rotation speed of the planetary mixer is 100 to 500 r / min.
[0012] Preferably, the phosphoric acid in the phosphoric acid aqueous solution contains 60-90% by mass of phosphoric acid; and / or the particle size of the Ti powder is not greater than 5 μm.
[0013] Preferably, the silicon-zirconium mixed powder consists of 40-95% Si powder and 5-60% Zr powder in mass percentage; the particle size of the Si powder is not greater than 500 μm, and the particle size of the Zr powder is not greater than 500 μm.
[0014] Preferably, in step (1): the pretreatment is carried out under an argon atmosphere, the pretreatment temperature is 1800-2000°C, and the pretreatment time is 2-4h; and / or the pyrolytic carbon matrix is introduced into the interior of the pretreated carbon fiber preform by chemical vapor infiltration, when chemical vapor infiltration is performed, propylene is used as the carbon source and nitrogen is used as the dilution gas, the flow ratio of propylene to the nitrogen is (1-4):1, the deposition pressure is 0.4-1.2kPa, the deposition temperature is 900-1000°C, and the deposition time is 30-150h.
[0015] Preferably, in step (2): the impregnation is vacuum impregnation and pressure impregnation; the temperature of the cross-linking and curing is 50-200°C, the time of the cross-linking and curing is 10-20 hours, and the pressure of the cross-linking and curing is 2-5 MPa; the temperature of the cracking and carbonization is 750-1000°C, and the time of the cracking and carbonization is 1-3 hours; the temperature is increased to the cracking and carbonization temperature at a heating rate of 0.2-0.6°C / min; and / or the temperature of the heat treatment is 2000-2200°C, and the time of the heat treatment is 2-4 hours.
[0016] Preferably, the resin carbon in the carbon fiber reinforced multiphase ceramic matrix composite material is uniformly distributed in the carbon fiber reinforced multiphase ceramic matrix composite material in the form of islands; and / or the carbon fiber reinforced multiphase ceramic matrix composite material has a residual Si content of 0.2-1.2wt%, a bending strength of 221-246MPa, a compressive strength of 357-409MPa, a dynamic friction coefficient of 0.40-0.46, and a wear rate of 0.402-1.074×10 -9 m 3 N -1 m -1 .
[0017] In a second aspect, the present invention provides a carbon fiber reinforced multiphase ceramic matrix composite material prepared by the preparation method described in the first aspect of the present invention.
[0018] The present invention provides, in a third aspect, the use of the carbon fiber reinforced multiphase ceramic matrix composite material prepared by the preparation method described in the first aspect of the present invention as a friction brake material.
[0019] Compared with the prior art, the present invention has at least the following beneficial effects:
[0020] (1) The present invention introduces high-activity Ti powder and furan resin into a C / C blank, and utilizes the violent in-situ reaction between Ti powder and resin carbon during the resin carbonization process to intensify the cracking of the resin, thereby forming a fine-grained TiC hard phase and an island-shaped soft resin carbon; wherein the uniformly distributed fine-grained TiC hard phase can promote the non-uniform nucleation of the ceramic phase during the subsequent reaction infiltration process, reduce the ceramic grain size, and improve the mechanical properties and thermal shock resistance of the composite material; the island-shaped soft resin carbon can refine the pore structure of the blank, increase the specific surface area of the pores, provide a high-activity carbon source for the metal melt introduced in the subsequent reaction infiltration, reduce the content of the residual Si phase in the final product, and promote the uniform distribution of the ceramic phase, thereby improving the friction performance and thermal stability of the material.
[0021] (2) The present invention uses a resin slurry containing furan resin, phosphoric acid aqueous solution, cellulose acetate butyrate, polyvinyl pyrrolidone and Ti powder as an impregnation liquid to introduce high-activity Ti powder and furan resin into the C / C body. The present invention finds that the furan resin used in the resin slurry has a high residual carbon rate and is used as a carbon source. After cracking and carbonization, soft resin carbon is formed. The soft resin carbon not only provides a sufficient carbon source for the reaction of the metal melt, but also can serve as a lubricating component of the friction brake composite material after reaction infiltration; the phosphoric acid in the resin slurry is used as a catalytic curing agent for the resin to accelerate the curing process of the furan resin; in addition, the present invention finds that the cellulose acetate butyrate added to the resin slurry can be used as a leveling agent to improve the leveling property of the slurry and help the Ti powder in the slurry. The polyvinyl pyrrolidone in the resin slurry can be used as a dispersant to prevent the Ti powder from agglomerating in the slurry. The Ti powder added to the resin slurry is highly active and can react violently with the resin carbon in situ. The addition of cellulose acetate butyrate and polyvinyl pyrrolidone helps to effectively disperse the Ti powder in the slurry to form a uniformly distributed fine-grained TiC hard phase, while intensifying the cracking of the resin carbon to form island-shaped resin carbon, refine the pore structure of the blank, increase the pore specific surface area, and promote the reaction between the metal melt and carbon in the subsequent reaction infiltration process, thereby reducing the content of the residual Si phase in the final product and promoting the uniform distribution of the ceramic phase, thereby improving the friction performance and thermal stability of the material.
[0022] (3) The island-shaped soft resin carbon introduced into the carbon fiber reinforced multiphase ceramic matrix composite material of the present invention can still remain uniformly in the form of islands after reactive infiltration. It can act as a lubricating component to form a friction film on the friction surface during friction braking, which can effectively reduce the wear rate of the material and improve the wear resistance and friction stability of the material.
[0023] (4) The TiC and ZrC introduced into the carbon fiber reinforced multiphase ceramic matrix composite material of the present invention not only have high hardness, but also have excellent high temperature mechanical properties and oxidation resistance, which can further improve the high temperature thermal stability of the C / C-SiC composite material.
[0024] (5) The carbon fiber reinforced multiphase ceramic matrix composite material (also referred to as C / C-TiC-SiC-ZrC friction brake composite material) prepared by the present invention is mainly composed of four matrices: C, TiC, SiC and ZrC. The overall hardness of the material can be adjusted by regulating the proportion of each matrix, and can be more widely applicable to the performance requirements of brake materials for different vehicles. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a flow chart for preparing carbon fiber reinforced multiphase ceramic matrix composite materials in some specific embodiments of the present invention;
[0026] Figure 2 is a scanning electron microscope image of the C / C-TiC body in Example 1 of the present invention;
[0027] Figure 3 is a scanning electron microscope image of the C / C body in Comparative Example 1 of the present invention;
[0028] Figure 4 This is a real picture of a brake pad made of the carbon fiber reinforced multiphase ceramic matrix composite material prepared by the present invention. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] In a first aspect, the present invention provides a method for preparing a carbon fiber reinforced multiphase ceramic matrix composite material, the method comprising the following steps:
[0031] (1) pretreating a carbon fiber preform, and then introducing a pyrolytic carbon matrix into the pretreated carbon fiber preform to obtain a C / C blank;
[0032] (2) The C / C body is immersed in a resin slurry containing Ti powder, and then cross-linked, solidified, cracked, carbonized and heat-treated to obtain a C / C-TiC body; the resin slurry containing Ti powder is prepared from furan resin (liquid furan resin), phosphoric acid aqueous solution, cellulose acetate butyrate, polyvinyl pyrrolidone and Ti powder; in the present invention, the impregnation is, for example, vacuum-pressure impregnation; the present invention has no special requirements for the furan resin, cellulose acetate butyrate, polyvinyl pyrrolidone, Ti powder, etc., and the products that can be directly purchased on the market can be used; in the present invention, the cracking, carbonization and heat treatment are carried out in an inert atmosphere; in the present invention, after the impregnation is completed, the impregnated C / C body is first taken out from the resin slurry containing Ti powder, and then cross-linked, solidified, cracked, carbonized and heat-treated are carried out in sequence;
[0033] (3) The C / C-TiC blank is embedded in a silicon-zirconium mixed powder for reaction infiltration to obtain a carbon fiber reinforced multiphase ceramic matrix composite material (also referred to as a C / C-TiC-SiC-ZrC friction brake composite material); in the present invention, the reaction infiltration temperature is, for example, 1550 to 2000°C, preferably 1600 to 2000°C, the reaction infiltration time is, for example, 0.5 to 4 hours, and the reaction infiltration is carried out under an inert atmosphere (for example, an argon atmosphere).
[0034] The invention utilizes the violent in-situ reaction of high-activity Ti powder and resin carbon to introduce and form fine-grained TiC hard phase and island-shaped soft resin carbon, thereby refining the pore structure of the blank to reduce the final residual Si phase, homogenizing the distribution of the ceramic phase, and using the residual resin carbon as a lubricating component after reactive infiltration to improve the friction braking performance of the material; the carbon fiber reinforced multiphase ceramic matrix composite material prepared by the invention has low residual silicon content, fine ceramic grains, uniform distribution of each phase, excellent mechanical / friction properties, thermal stability and thermal shock resistance, and its residual Si content is 0.2-1.2%, the bending strength is 221-246 MPa, the compressive strength is 357-409 MPa, the dynamic friction coefficient is 0.40-0.46, and the wear rate is 0.402-1.074×10 -9 m 3 N -1 m -1 , can be used to prepare friction brake products such as brake discs / pads.
[0035] The present invention uses a resin slurry containing furan resin, phosphoric acid aqueous solution, cellulose acetate butyrate, polyvinyl pyrrolidone and Ti powder as an impregnation liquid to introduce high-activity Ti powder and furan resin into a C / C blank. The present invention finds that the furan resin used in the resin slurry has a high residual carbon rate and is used as a carbon source. After cracking and carbonization, soft resin carbon is formed. The soft resin carbon not only provides a sufficient carbon source for the reaction of the metal melt, but also can serve as a lubricating component of the friction brake composite material after reaction infiltration; the phosphoric acid in the resin slurry is used as a catalytic curing agent for the resin to accelerate the curing process of the furan resin; in addition, the present invention finds that the cellulose acetate butyrate added in the resin slurry can be used as a leveling agent to improve the leveling property of the slurry and help the uniformity of the Ti powder in the slurry. The polyvinyl pyrrolidone in the resin slurry can be used as a dispersant to prevent the Ti powder from agglomerating in the slurry. The Ti powder added to the resin slurry is highly active and can react violently with the resin carbon in situ. The addition of cellulose acetate butyrate and polyvinyl pyrrolidone helps the effective dispersion of the Ti powder in the slurry to form a uniformly distributed fine-grained TiC hard phase, while aggravating the cracking of the resin carbon to form island-shaped resin carbon, refine the pore structure of the blank, increase the pore specific surface area, and promote the reaction between the metal melt and carbon in the subsequent reaction infiltration process, thereby reducing the content of the residual Si phase in the final product and promoting the uniform distribution of the ceramic phase, thereby improving the friction performance and thermal stability of the material. The island-shaped soft resin carbon introduced into the carbon fiber reinforced composite ceramic matrix composite material by the present invention can still remain uniformly in the form of islands after the reaction infiltration. It can act as a lubricating component to form a friction film on the friction surface during the friction braking process, which can effectively reduce the wear rate of the material and improve the wear resistance and friction stability of the material.
[0036] According to some preferred embodiments, when preparing the resin slurry containing Ti powder, the mass ratio of the furan resin, the phosphoric acid aqueous solution, the cellulose acetate butyrate, the polyvinyl pyrrolidone and the Ti powder is (40-88): (5-10): (1-10): (1-10): (5-30), preferably (64-76): (5-7): (1-3): (1-3): (10-25). In the present invention, when preparing the resin slurry containing Ti powder, it is preferred to control the mass ratio of the furan resin, the phosphoric acid aqueous solution, the cellulose acetate butyrate, the polyvinyl pyrrolidone and the Ti powder to be (40-88): (5-10): (1-10): (1-10): (5-30), and more preferably to be (64-76): (5-7): (1-3): (1-3): (10-25). This is more conducive to reducing the content of residual Si phase in the final product and promoting the uniform distribution of the ceramic phase, further improving the friction performance and thermal stability of the material, and is more conducive to reducing the wear rate of the material. Strictly controlling the ratio of each component is the key to ensuring that the carbon fiber reinforced multiphase ceramic matrix composite material has excellent friction braking performance, and an inappropriate ratio may lead to poor compactness, mechanical properties, friction performance and thermal stability of the final product. The present invention finds that cellulose acetate butyrate used as a leveling agent can effectively improve the leveling property of the resin slurry and help to evenly distribute the Ti powder in the slurry, while insufficient cellulose acetate butyrate may lead to poor flow uniformity of the resin slurry and uneven distribution of the Ti powder, while excessive cellulose acetate butyrate may affect the process operability; polyvinyl pyrrolidone used as a dispersant can make the Ti powder dispersed evenly in the resin slurry, while too little polyvinyl pyrrolidone may cause the Ti powder to agglomerate, affecting the uniformity and performance of the product, while too much may increase the cost and affect the viscosity of the resin slurry; Ti powder has high activity and can react violently with the resin carbon in situ, while too little Ti powder will lead to insufficient hard phase formation, affecting the friction performance of the product, while too much Ti powder will also lead to increased viscosity of the resin slurry and poor fluidity.
[0037] According to some preferred embodiments, the resin slurry containing Ti powder is prepared as follows: furan resin, phosphoric acid aqueous solution, cellulose acetate butyrate, polyvinyl pyrrolidone and Ti powder are added to a planetary mixer and mixed for 1 to 10 hours (for example, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 hours); the rotation speed of the planetary mixer is 100 to 500 r / min (for example, 100, 200, 300, 400 or 500 r / min).
[0038] According to some preferred embodiments, the mass fraction of phosphoric acid contained in the phosphoric acid aqueous solution is 60-90% (for example, 60%, 65%, 70%, 75%, 80%, 85% or 90%); and / or the particle size of the Ti powder (titanium powder) is not more than 5 μm; in the present invention, the purity of the Ti powder is ≥99%.
[0039] According to some preferred embodiments, the silicon-zirconium mixed powder (Si-Zr mixed powder) is composed of 40-95% Si powder (silicon powder) and 5-60% Zr powder (zirconium powder) in mass percentage; the particle size of the Si powder is not greater than 500 μm, and the particle size of the Zr powder is not greater than 500 μm; it is particularly noted that the "particle size" involved in the specific embodiments of the present invention refers to the average particle size.
[0040] According to some specific embodiments, the silicon-zirconium mixed powder is prepared as follows: Si powder and Zr powder are placed in a ball mill, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is (2-10):1, the ball milling speed is 30-100 r / min, preferably 40-80 r / min, the ball milling time is 12-24 h, and after the ball milling is completed, it is placed in a 40-100°C oven for drying for 12-48 h to obtain the silicon-zirconium mixed powder.
[0041] According to some preferred embodiments, in step (1): the pretreatment is carried out under an argon atmosphere, the pretreatment temperature is 1800-2000°C, and the pretreatment time is 2-4h; in the present invention, the carbon fiber preform can be degummed and the internal stress can be reduced by high-temperature pretreatment; and / or the pyrolytic carbon matrix is introduced into the interior of the pretreated carbon fiber preform by chemical vapor infiltration, when the chemical vapor infiltration is carried out, propylene is used as the carbon source and nitrogen is used as the diluent gas, the flow ratio of the propylene to the nitrogen is (1-4):1, the deposition pressure is 0.4-1.2kPa, the deposition temperature is 900-1000°C, and the deposition time is 30-150h; in the present invention, the pyrolytic carbon matrix is introduced into the interior of the pretreated carbon fiber preform by chemical vapor infiltration, and the pyrolytic carbon can reduce the corrosion of the metal melt to the fiber in the subsequent reaction infiltration process and provide a carbon source for it to form carbides.
[0042] According to some preferred embodiments, in step (2): the impregnation is vacuum impregnation and pressure impregnation; in the present invention, when the impregnation is vacuum impregnation and pressure impregnation, the impregnation is also recorded as vacuum-pressure impregnation. The vacuum-pressure impregnation of the present invention can ensure that the resin slurry can fully fill the pores of the C / C body; in the present invention, for example, the number of vacuum-pressure impregnation is 1 to 2 times, the vacuum degree of the vacuum impregnation is, for example, -0.08MPa to -0.1MPa, the temperature of the vacuum impregnation is, for example, 50 to 80°C, the time of the vacuum impregnation is, for example, 1 to 3h, the pressure of the pressure impregnation is, for example, 2 to 5MPa, the pressurized gas is, for example, nitrogen, the time of the pressure impregnation is ≥1h, preferably 1 to 3h, and the temperature of the pressure impregnation is, for example, 50 to 80°C; The cross-linking and curing temperature is 50-200°C, the cross-linking and curing time is 10-20h, and the cross-linking and curing pressure is 2-5MPa; the cracking and carbonization temperature is 750-1000°C, and the cracking and carbonization time is 1-3h; the temperature is raised to the cracking and carbonization temperature at a heating rate of 0.2-0.6°C / min, for example, the heating rate to the cracking and carbonization temperature is controlled to be 0.2-0.6°C / min, so that the time to rise to the cracking and carbonization temperature is 20-30h; and / or the heat treatment temperature is 2000-2200°C, and the heat treatment time is 2-4h; unless otherwise specified in the present invention, the heating rate to the pretreatment temperature, the heat treatment temperature or the reverse osmosis infiltration temperature, etc., can be, for example, 3-10°C / min.
[0043] According to some preferred embodiments, before performing step (3), the process further includes subjecting the C / C-TiC body obtained in step (2) to surface machining to further improve pore connectivity.
[0044] According to some preferred embodiments, the resin carbon in the carbon fiber reinforced multiphase ceramic matrix composite material is uniformly distributed in the carbon fiber reinforced multiphase ceramic matrix composite material in the form of islands; and / or the carbon fiber reinforced multiphase ceramic matrix composite material has a residual Si content of 0.2 to 1.2 wt%, a bending strength of 221 to 246 MPa, a compressive strength of 357 to 409 MPa, a dynamic friction coefficient of 0.40 to 0.46, and a wear rate of 0.402 to 1.074×10 -9 m 3 N -1 m -1 .
[0045] In a second aspect, the present invention provides a carbon fiber reinforced multiphase ceramic matrix composite material prepared by the preparation method described in the first aspect of the present invention. The carbon fiber reinforced multiphase ceramic matrix composite material prepared by the present invention has a low residual Si content, fine ceramic grains, uniform distribution of each phase, excellent mechanical / friction properties, thermal stability and thermal shock resistance, and a residual Si content of 0.2-1.2%, a bending strength of 221-246 MPa, a compressive strength of 357-409 MPa, a dynamic friction coefficient of 0.40-0.46, and a wear rate of 0.402-1.074×10 -9 m 3 N -1 m -1 , can be used to prepare friction brake products such as automobile brake discs / pads.
[0046] The present invention provides, in a third aspect, the use of the carbon fiber reinforced multiphase ceramic matrix composite material prepared by the preparation method described in the first aspect of the present invention as a friction brake material.
[0047] The present invention will be further described below by way of examples, but the protection scope of the present invention is not limited to these examples. Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available products or can be prepared by known methods.
[0048] Example 1
[0049] ①T700 12K PANCF carbon fiber was used as raw material, and alternately intermittent non-woven fabric / mesh tire was used as structural unit for continuous layering. Carbon fiber needle-punched integral felt was obtained by continuous needle-punching, and the volume density was 0.55g / cm 3 The carbon fiber preform was subjected to high temperature pretreatment at 2000℃ for 2h under argon protective atmosphere; propylene was used as carbon source gas and nitrogen was used as diluent gas, and pyrolytic carbon matrix was introduced into the carbon fiber preform by chemical vapor infiltration. The deposition temperature was 900℃, the deposition pressure was 1.2kPa, the flow ratio of propylene to nitrogen was 2:1, and the deposition time was 100h. The obtained volume density and porosity were 1.10g / cm 3 and 40% C / C billet.
[0050] ② Place furan resin, phosphoric acid aqueous solution (the phosphoric acid aqueous solution contains 85% phosphoric acid by mass), cellulose acetate butyrate, polyvinyl pyrrolidone and Ti powder in a planetary mixer in a mass ratio of 76:7:2:2:13 to obtain a resin slurry containing Ti powder; wherein the Ti particle size is 1 μm, the planetary mixer speed is 300 r / min, and the stirring and mixing time is 5 h; using the obtained resin slurry containing Ti powder as the impregnation liquid, the C / C blank obtained in step ① is subjected to one round of vacuum-pressure impregnation, and after being taken out, cross-linking curing, cracking carbonization and high-temperature heat treatment are sequentially performed to prepare a bulk density and porosity of 1.47 g / cm 3 and 22% C / C-TiC blank; wherein, vacuum-pressure impregnation includes vacuum impregnation and pressure impregnation, which is carried out in an impregnation furnace containing the resin slurry containing Ti powder, when vacuum impregnation is carried out, the vacuum degree is -0.10MPa, the vacuum impregnation temperature is 60°C, and the vacuum impregnation time is 1h, when pressure impregnation is carried out, the pressure of pressure impregnation is 2.0MPa, the pressure impregnation time is 1h, and the pressure impregnation temperature is 60°C; the cross-linking and curing process is: 120°C cross-linking and curing for 4h, 190°C cross-linking and curing for 7h; cracking and carbonization are carried out in an argon atmosphere, the cracking and carbonization temperature is 900°C, the heating rate to 900°C is 0.5°C / min, the cracking and carbonization time is 2h, and the high-temperature heat treatment is carried out in an argon protective atmosphere, the high-temperature heat treatment temperature is 2200°C, and the high-temperature heat treatment time is 2h.
[0051] ③ Place Si powder and Zr powder in a ball mill equipped with zirconium oxide grinding balls, mix them by ball milling, then filter them with a sieve and dry them at 50°C for 12 hours to obtain a silicon-zirconium mixed powder; wherein the mass percentage of Si powder in the silicon-zirconium mixed powder is 85%, the mass percentage of Zr powder is 15%, the particle size of Si powder and Zr powder is 45μm, the ball milling medium is ethanol, the ball-to-material ratio is 2:1, the ball milling speed is 50r / min, and the ball milling mixing time is 24h; the C / C-TiC blank obtained in step ② is embedded in the silicon-zirconium mixed powder and placed in a vacuum carbon tube furnace for reaction infiltration, the reaction infiltration temperature is 1800°C, the reaction infiltration time is 2h, and the volume density is 2.30g / cm 3 C / C-TiC-SiC-ZrC friction brake composite material (carbon fiber reinforced multiphase ceramic matrix composite material).
[0052] The scanning electron microscope image of the C / C-TiC body obtained in this embodiment is as follows: Figure 2 As shown, from Figure 2 It can be seen that the resin carbon in the C / C-TiC body is evenly distributed in the form of islands.
[0053] The bending strength of the C / C-TiC-SiC-ZrC friction brake composite material obtained in this embodiment was measured to be 246MPa, the compressive strength was 357MPa, and the residual Si content was 0.2%. After the SAE J2522 AK Master bench test, the dynamic friction coefficient of the C / C-TiC-SiC-ZrC friction brake composite material was measured to be 0.40, and the wear rate was 0.402×10 -9 m 3 N -1 m -1 .
[0054] Example 2
[0055] ①T700 12K PANCF carbon fiber was used as raw material, and alternately intermittent non-woven fabric / mesh tire was used as structural unit for continuous layering. Carbon fiber needle-punched integral felt was obtained by continuous needle-punching, and the volume density was 0.55g / cm 3 The carbon fiber preform was subjected to high temperature pretreatment at 2000℃ for 3h under argon protective atmosphere; propylene was used as carbon source gas and nitrogen was used as diluent gas, and pyrolytic carbon matrix was introduced into the carbon fiber preform by chemical vapor infiltration. The deposition temperature was 950℃, the deposition pressure was 1.0kPa, the flow ratio of propylene to nitrogen was 3:1, and the deposition time was 60h. The obtained volume density and porosity were 1.00g / cm 3 and 46% C / C green body.
[0056] ② Place furan resin, phosphoric acid aqueous solution (the phosphoric acid aqueous solution contains 85% phosphoric acid by mass), cellulose acetate butyrate, polyvinyl pyrrolidone and Ti powder in a planetary mixer in a mass ratio of 69:7:2:2:20 to obtain a resin slurry containing Ti powder; wherein the Ti particle size is 5 μm, the planetary mixer speed is 500 r / min, and the stirring and mixing time is 8 h; using the obtained resin slurry containing Ti powder as the impregnation liquid, the C / C blank obtained in step ① is subjected to one round of vacuum-pressure impregnation, and after being taken out, cross-linking curing, cracking carbonization and high-temperature heat treatment are sequentially performed to prepare a bulk density and porosity of 1.45 g / cm 3and 26% C / C-TiC blank; wherein, vacuum-pressure impregnation includes vacuum impregnation and pressure impregnation, which is carried out in an impregnation furnace containing the resin slurry containing Ti powder, when vacuum impregnation is carried out, the vacuum degree is -0.10MPa, the vacuum impregnation temperature is 65°C, and the vacuum impregnation time is 1h, when pressure impregnation is carried out, the pressure of pressure impregnation is 2.5MPa, the pressure impregnation time is 2h, and the pressure impregnation temperature is 65°C; the cross-linking and curing process is: 130°C cross-linking and curing for 5h, 200°C cross-linking and curing for 8h; cracking and carbonization are carried out in an argon atmosphere, the cracking and carbonization temperature is 950°C, the heating rate to 950°C is 0.5°C / min, the cracking and carbonization time is 2h, and the high-temperature heat treatment is carried out in an argon protective atmosphere, the high-temperature heat treatment temperature is 2000°C, and the high-temperature heat treatment time is 4h.
[0057] ③ Place Si powder and Zr powder in a ball mill equipped with zirconium oxide grinding balls for ball milling and mixing, then filter with a sieve and dry at 45°C for 12 hours to obtain a silicon-zirconium mixed powder; wherein the mass percentage of Si powder in the silicon-zirconium mixed powder is 80%, the mass percentage of Zr powder is 20%, the particle size of Si powder and Zr powder is 75μm, the ball milling medium is ethanol, the ball-to-material ratio is 5:1, the ball milling speed is 60r / min, and the ball milling mixing time is 24h; the C / C-TiC blank obtained in step ② is embedded in the silicon-zirconium mixed powder and placed in a vacuum carbon tube furnace for reaction infiltration, the reaction infiltration temperature is 1700°C, the reaction infiltration time is 4h, and the volume density is 2.34g / cm 3 C / C-TiC-SiC-ZrC friction brake composite material (carbon fiber reinforced multiphase ceramic matrix composite material).
[0058] The bending strength of the C / C-TiC-SiC-ZrC friction brake composite material obtained in this embodiment is measured to be 233 MPa, the compressive strength is 397 MPa, and the residual Si content is 0.5%. After the SAE J2522 AK Master bench test, the dynamic friction coefficient of the C / C-TiC-SiC-ZrC friction brake composite material is measured to be 0.42, and the wear rate is 0.488×10 -9 m 3 N -1 m -1 .
[0059] Example 3
[0060] ①T700 12K PANCF carbon fiber was used as raw material, and alternately intermittent non-woven fabric / mesh tire was used as structural unit for continuous layering. Carbon fiber needle-punched integral felt was obtained by continuous needle-punching, and the volume density was 0.55g / cm 3The carbon fiber preform was subjected to high temperature pretreatment at 2000℃ for 4h under argon protective atmosphere; propylene was used as carbon source gas and nitrogen was used as diluent gas, and pyrolytic carbon matrix was introduced into the carbon fiber preform by chemical vapor infiltration. The deposition temperature was 1000℃, the deposition pressure was 0.6kPa, the flow ratio of propylene to nitrogen was 2:1, and the deposition time was 30h. The obtained volume density and porosity were 0.90g / cm 3 and 50% C / C billet.
[0061] ② Place furan resin, phosphoric acid aqueous solution (the phosphoric acid aqueous solution contains 85% phosphoric acid by mass), cellulose acetate butyrate, polyvinyl pyrrolidone and Ti powder in a planetary mixer in a mass ratio of 64:5:3:3:25 to obtain a resin slurry containing Ti powder; wherein the Ti particle size is 5 μm, the planetary mixer speed is 450 r / min, and the stirring and mixing time is 10 h; using the obtained resin slurry containing Ti powder as the impregnation liquid, the C / C blank obtained in step ① is subjected to one round of vacuum-pressure impregnation, and after being taken out, cross-linking curing, cracking carbonization and high-temperature heat treatment are sequentially performed to prepare a bulk density and porosity of 1.39 g / cm 3 and 29% C / C-TiC blank; wherein, vacuum-pressure impregnation includes vacuum impregnation and pressure impregnation, which is carried out in an impregnation furnace containing the resin slurry containing Ti powder, when vacuum impregnation is carried out, the vacuum degree is -0.10MPa, the vacuum impregnation temperature is 80°C, and the vacuum impregnation time is 1h, when pressure impregnation is carried out, the pressure of pressure impregnation is 3.0MPa, the pressure impregnation time is 1h, and the pressure impregnation temperature is 80°C; the cross-linking and curing process is: 120°C cross-linking and curing for 4h, 180°C cross-linking and curing for 7h; cracking and carbonization are carried out in an argon atmosphere, the cracking and carbonization temperature is 1000°C, the heating rate to 1000°C is 0.5°C / min, the cracking and carbonization time is 3h, and the high-temperature heat treatment is carried out in an argon protective atmosphere, the high-temperature heat treatment temperature is 2200°C, and the high-temperature heat treatment time is 4h.
[0062] ③ The Si powder and Zr powder are placed in a ball mill equipped with zirconium oxide grinding balls for ball milling and mixing, and then filtered with a sieve and dried at 40°C for 20 hours to obtain a silicon-zirconium mixed powder; wherein the mass percentage of Si powder in the silicon-zirconium mixed powder is 70%, the mass percentage of Zr powder is 30%, the particle size of Si powder and Zr powder is 75μm, the ball milling medium is ethanol, the ball-to-material ratio is 10:1, the ball milling speed is 55r / min, and the ball milling mixing time is 24h; the C / C-TiC blank obtained in step ② is embedded in the silicon-zirconium mixed powder and placed in a vacuum carbon tube furnace for reaction infiltration, the reaction infiltration temperature is 1900°C, the reaction infiltration time is 3h, and the volume density is 2.49g / cm 3C / C-TiC-SiC-ZrC friction brake composite material (carbon fiber reinforced multiphase ceramic matrix composite material).
[0063] The bending strength of the C / C-TiC-SiC-ZrC friction brake composite material obtained in this embodiment was measured to be 221 MPa, the compressive strength was 409 MPa, and the residual Si content was 0.7%. After the SAE J2522 AK Master bench test, the dynamic friction coefficient of the C / C-TiC-SiC-ZrC friction brake composite material was measured to be 0.43, and the wear rate was 0.522×10 -9 m 3 N -1 m -1 .
[0064] Example 4
[0065] Embodiment 4 is substantially the same as Embodiment 1, except that:
[0066] ② Place furan resin, phosphoric acid aqueous solution (the phosphoric acid aqueous solution contains 85% phosphoric acid by mass), cellulose acetate butyrate, polyvinyl pyrrolidone and Ti powder in a planetary mixer in a mass ratio of 40:10:10:10:30 to obtain a resin slurry containing Ti powder; wherein the Ti particle size is 1 μm, the planetary mixer speed is 300 r / min, and the stirring and mixing time is 5 h; using the obtained resin slurry containing Ti powder as the impregnation liquid, the C / C blank obtained in step ① is subjected to one round of vacuum-pressure impregnation, taken out and then cross-linked, cured, cracked and carbonized, and subjected to high-temperature heat treatment to obtain a C / C-TiC blank; wherein the vacuum-pressure impregnation includes vacuum impregnation and pressure impregnation, which is carried out in a liquid containing The resin slurry containing Ti powder is impregnated in an impregnation furnace. When vacuum impregnation is performed, the vacuum degree is -0.10MPa, the temperature of vacuum impregnation is 60°C, and the time of vacuum impregnation is 1h. When pressure impregnation is performed, the pressure of pressure impregnation is 2.0MPa, the time of pressure impregnation is 1h, and the temperature of pressure impregnation is 60°C. The cross-linking and curing process is: cross-linking and curing at 120°C for 4h and cross-linking and curing at 190°C for 7h. Cracking and carbonization are performed in an argon atmosphere at a temperature of 900°C, a heating rate of 0.5°C / min to 900°C, and a time of 2h. High-temperature heat treatment is performed in an argon protective atmosphere at a temperature of 2200°C and a time of 2h.
[0067] Example 5
[0068] Example 5 is substantially the same as Example 1, except that:
[0069] ② Place furan resin, phosphoric acid aqueous solution (the phosphoric acid aqueous solution contains 85% by mass of phosphoric acid), cellulose acetate butyrate, polyvinyl pyrrolidone and Ti powder in a planetary mixer in a mass ratio of 88:5:1:1:5 to obtain a resin slurry containing Ti powder; wherein the Ti particle size is 1 μm, the planetary mixer speed is 300 r / min, and the stirring and mixing time is 5 h; using the obtained resin slurry containing Ti powder as the impregnation liquid, the C / C blank obtained in step ① is subjected to one round of vacuum-pressure impregnation, and after being taken out, cross-linking curing, cracking carbonization and high-temperature heat treatment are sequentially performed to prepare a C / C-TiC blank; wherein the vacuum-pressure impregnation includes vacuum impregnation and pressure impregnation, which is performed in a liquid containing the The process is carried out in an impregnation furnace of a resin slurry containing Ti powder. When vacuum impregnation is performed, the vacuum degree is -0.10MPa, the temperature of vacuum impregnation is 60°C, and the time of vacuum impregnation is 1h. When pressure impregnation is performed, the pressure of pressure impregnation is 2.0MPa, the time of pressure impregnation is 1h, and the temperature of pressure impregnation is 60°C. The cross-linking and curing process is: cross-linking and curing at 120°C for 4h and cross-linking and curing at 190°C for 7h. Cracking and carbonization are carried out in an argon atmosphere at a temperature of 900°C, a heating rate of 0.5°C / min to 900°C, and a time of 2h for cracking and carbonization. High-temperature heat treatment is carried out in an argon protective atmosphere at a temperature of 2200°C and a time of 2h.
[0070] Comparative Example 1
[0071] Comparative Example 1 is substantially the same as Example 1, except that:
[0072] ② Place furan resin and phosphoric acid aqueous solution (the phosphoric acid aqueous solution contains 85% by mass of phosphoric acid) in a planetary mixer in a mass ratio of 76:7 to obtain resin slurry; wherein the planetary mixer speed is 300r / min, and the stirring and mixing time is 5h; using the obtained resin slurry as the impregnation liquid, the C / C blank obtained in step ① is subjected to one round of vacuum-pressure impregnation, and after being taken out, cross-linking curing, cracking carbonization and high-temperature heat treatment are sequentially performed to prepare a C / C blank; wherein the vacuum-pressure impregnation includes vacuum impregnation and pressure impregnation, which is performed in an impregnation furnace containing the resin slurry. During the vacuum impregnation, the vacuum The vacuum is -0.10MPa, the temperature of vacuum impregnation is 60℃, the time of vacuum impregnation is 1h, when pressure impregnation is performed, the pressure of pressure impregnation is 2.0MPa, the time of pressure impregnation is 1h, and the temperature of pressure impregnation is 60℃; the cross-linking and curing process is: cross-linking and curing at 120℃ for 4h, and cross-linking and curing at 190℃ for 7h; the cracking and carbonization is carried out in an argon atmosphere, the temperature of cracking and carbonization is 900℃, the heating rate to 900℃ is 0.5℃ / min, and the time of cracking and carbonization is 2h. The high-temperature heat treatment is carried out in an argon protective atmosphere, the temperature of the high-temperature heat treatment is 2200℃, and the time of high-temperature heat treatment is 2h.
[0073] The scanning electron microscope image of the C / C body obtained in this comparative example is as follows: Figure 3 shown; from Figure 3 It can be seen that the resin carbon in this comparative example is distributed all over the original pores after cracking, and some large cracks caused by the cracking of the resin remain; compared with the C / C-TiC body obtained by using the resin slurry containing Ti powder, the resin carbon of the C / C body in this comparative example is unevenly distributed, and the scale of the resin carbon is too large; Figure 2 and Figure 3 Compared with the results of the present invention, it can be seen that the violent in-situ reaction of Ti powder and resin carbon during the resin carbonization process is used to intensify the cracking of the resin, so that the cracks formed in the cracking process are smaller and more numerous, and the resin carbon is divided into more small portions, ensuring the formation of fine-grained TiC hard phase and island-shaped soft resin carbon, thereby refining the pore structure of the green body to reduce the final residual Si phase and homogenize the distribution of the ceramic phase.
[0074] Comparative Example 2
[0075] Comparative Example 2 is substantially the same as Example 1, except that:
[0076] ② Place furan resin, phosphoric acid aqueous solution (the phosphoric acid aqueous solution contains 85% phosphoric acid by mass) in a planetary mixer to mix, and obtain a resin slurry containing Ti powder; wherein the Ti particle size is 1 μm, the planetary mixer speed is 300 r / min, and the stirring and mixing time is 5 h; using the obtained resin slurry containing Ti powder as the impregnation liquid, the C / C blank obtained in step ① is subjected to one round of vacuum-pressure impregnation, and after being taken out, cross-linking curing, cracking carbonization and high-temperature heat treatment are sequentially performed to prepare a C / C-TiC blank; wherein vacuum-pressure impregnation includes vacuum impregnation and pressure impregnation, which is performed in a liquid containing the Ti The process is carried out in an impregnation furnace of a resin slurry of powder. When vacuum impregnation is carried out, the vacuum degree is -0.10MPa, the temperature of vacuum impregnation is 60°C, and the time of vacuum impregnation is 1h. When pressure impregnation is carried out, the pressure of pressure impregnation is 2.0MPa, the time of pressure impregnation is 1h, and the temperature of pressure impregnation is 60°C. The cross-linking and curing process is: cross-linking and curing at 120°C for 4h and cross-linking and curing at 190°C for 7h. Cracking and carbonization are carried out in an argon atmosphere at a temperature of 900°C, a heating rate of 0.5°C / min to 900°C, and a time of 2h for cracking and carbonization. High-temperature heat treatment is carried out in an argon protective atmosphere at a temperature of 2200°C and a time of 2h.
[0077] Comparative Example 3
[0078] Comparative Example 3 is substantially the same as Example 1, except that:
[0079] ② Place furan resin, phosphoric acid aqueous solution (the mass fraction of phosphoric acid in the phosphoric acid aqueous solution is 85%), cellulose acetate butyrate and Ti powder in a planetary mixer in a mass ratio of 76:7:2:13 to obtain a resin slurry containing Ti powder; wherein the Ti particle size is 1 μm, the planetary mixer speed is 300 r / min, and the stirring and mixing time is 5 h; using the obtained resin slurry containing Ti powder as the impregnation liquid, the C / C blank obtained in step ① is subjected to one round of vacuum-pressure impregnation, and after being taken out, cross-linking curing, cracking carbonization and high-temperature heat treatment are sequentially performed to prepare a C / C-TiC blank; wherein the vacuum-pressure impregnation includes vacuum impregnation and pressure impregnation, which is performed in a liquid containing the Ti The process is carried out in an impregnation furnace of a resin slurry of powder. When vacuum impregnation is carried out, the vacuum degree is -0.10MPa, the temperature of vacuum impregnation is 60°C, and the time of vacuum impregnation is 1h. When pressure impregnation is carried out, the pressure of pressure impregnation is 2.0MPa, the time of pressure impregnation is 1h, and the temperature of pressure impregnation is 60°C. The cross-linking and curing process is: cross-linking and curing at 120°C for 4h and cross-linking and curing at 190°C for 7h. Cracking and carbonization are carried out in an argon atmosphere at a temperature of 900°C, a heating rate of 0.5°C / min to 900°C, and a time of 2h for cracking and carbonization. High-temperature heat treatment is carried out in an argon protective atmosphere at a temperature of 2200°C and a time of 2h.
[0080] Comparative Example 4
[0081] ①T700 12K PANCF carbon fiber was used as raw material, and alternately intermittent non-woven fabric / mesh tire was used as structural unit for continuous layering. Carbon fiber needle-punched integral felt was obtained by continuous needle-punching, and the volume density was 0.49g / cm 3 A carbon fiber preform is prepared; the carbon fiber preform is subjected to a high temperature pretreatment at 1800°C for 2 hours under an argon protective atmosphere; natural gas is used as a carbon source gas and nitrogen is used as a diluent gas, and a pyrolytic carbon matrix is introduced into the carbon fiber preform by a chemical vapor infiltration method. The deposition temperature is 1000°C, the deposition pressure is 1.4 kPa, the flow ratio of natural gas to nitrogen is 2:1, and the deposition time is 50 hours to obtain a C / C blank.
[0082] ② Add silicon powder with a particle size of 5 μm as an impregnant to the phenolic resin, and the carbon / silicon molar ratio in the impregnant is 1.5:1, and perform the first impregnation / cracking cycle; add silicon powder with a particle size of 20 μm as an impregnant to the phenolic resin, and the carbon / silicon molar ratio in the impregnant is 5:1, and perform the second impregnation / cracking cycle; the above impregnation temperature is 60°C, the impregnation pressure is 7 MPa, and the impregnation time is 3 hours; the above cracking temperature is 900°C, the inert protective gas is nitrogen, and the cracking time is 2 hours. C is obtained by three impregnation and cracking cycles f / C m -Sim Porous intermediates.
[0083] ③Use silicon powder with a particle size of 50μm to completely coat C f / C m -Si m The porous intermediate is compacted with silicon powder, and then the graphite crucible is placed in a vacuum high-temperature furnace under an argon protective atmosphere for reactive infiltration. The reactive infiltration temperature is 1600° C. and the reactive infiltration time is 2 hours to obtain a carbon fiber reinforced ceramic matrix composite material.
[0084] The residual silicon content, dynamic friction coefficient and wear rate of the ceramic matrix composite material finally prepared in each embodiment and each comparative example of the present invention are measured and the results are shown in Table 1.
[0085] Table 1
[0086]
[0087] It is particularly noted that the dynamic friction coefficient of the friction brake material is generally preferably in the range of 0.35 to 0.50. If the friction coefficient is too low, problems such as insensitive braking will occur, and if the friction coefficient is higher than 0.5, the friction pair will easily vibrate and generate loud noise. The parts not described in detail in the present invention are well known to those skilled in the art.
[0088] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a carbon fiber reinforced multiphase ceramic matrix composite material, characterized in that: The method comprises the following steps: (1) pretreating a carbon fiber preform, and then introducing a pyrolytic carbon matrix into the pretreated carbon fiber preform to obtain a C / C blank; (2) placing the C / C body in a resin slurry containing Ti powder for impregnation, and then cross-linking, solidifying, cracking, carbonizing and heat treating to obtain a C / C-TiC body; the resin slurry containing Ti powder is prepared from furan resin, phosphoric acid aqueous solution, cellulose acetate butyrate, polyvinyl pyrrolidone and Ti powder; (3) The C / C-TiC blank is embedded in a silicon-zirconium mixed powder for reactive infiltration to obtain a carbon fiber reinforced multiphase ceramic matrix composite material.
2. The preparation method according to claim 1, characterized in that: When preparing the resin slurry containing Ti powder, the mass ratio of the furan resin, the phosphoric acid aqueous solution, the cellulose acetate butyrate, the polyvinyl pyrrolidone and the Ti powder is (40-88): (5-10): (1-10): (1-10): (5-30).
3. The preparation method according to claim 1, characterized in that: The resin slurry containing Ti powder is prepared by adding furan resin, phosphoric acid aqueous solution, cellulose acetate butyrate, polyvinyl pyrrolidone and Ti powder into a planetary mixer and mixing for 1 to 10 hours; The rotation speed of the planetary mixer is 100-500 r / min.
4. The preparation method according to claim 1, characterized in that: The phosphoric acid aqueous solution contains 60-90% by mass of phosphoric acid; and / or The particle size of the Ti powder is not greater than 5 μm.
5. The preparation method according to claim 1, characterized in that: The silicon-zirconium mixed powder is composed of 40-95% Si powder and 5-60% Zr powder in terms of mass percentage; The particle size of the Si powder is not greater than 500 μm, and the particle size of the Zr powder is not greater than 500 μm.
6. The preparation method according to claim 1, characterized in that: In step (1): The pretreatment is carried out in an argon atmosphere, the pretreatment temperature is 1800-2000° C., and the pretreatment time is 2-4 hours; and / or The pyrolyzed carbon matrix is introduced into the pretreated carbon fiber preform by chemical vapor infiltration. During the chemical vapor infiltration, propylene is used as the carbon source and nitrogen is used as the diluent gas. The flow ratio of the propylene to the nitrogen is (1-4):1, the deposition pressure is 0.4-1.2 kPa, the deposition temperature is 900-1000°C, and the deposition time is 30-150 hours.
7. The preparation method according to claim 1, characterized in that: In step (2): The impregnation is vacuum impregnation and pressure impregnation; The cross-linking curing temperature is 50 to 200° C., the cross-linking curing time is 10 to 20 hours, and the cross-linking curing pressure is 2 to 5 MPa; The temperature of the cracking and carbonization is 750-1000°C, and the time of the cracking and carbonization is 1-3h; The temperature is raised to the cracking and carbonization temperature at a heating rate of 0.2 to 0.6°C / min; and / or The temperature of the heat treatment is 2000-2200° C., and the time of the heat treatment is 2-4 hours.
8. The preparation method according to claim 1, characterized in that: The resin carbon in the carbon fiber reinforced multiphase ceramic matrix composite material is uniformly distributed in the carbon fiber reinforced multiphase ceramic matrix composite material in the form of islands; and / or The carbon fiber reinforced multiphase ceramic matrix composite material has a residual Si content of 0.2-1.2wt%, a bending strength of 221-246MPa, a compression strength of 357-409MPa, a dynamic friction coefficient of 0.40-0.46, and a wear rate of 0.402-1.074×10 -9 m 3 N -1 m -1 .
9. A carbon fiber reinforced multiphase ceramic matrix composite material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the carbon fiber reinforced multiphase ceramic matrix composite material prepared by the preparation method according to any one of claims 1 to 8 as a friction brake material.
Citation Information
Cited By
Preparation method of carbon-based composite material, carbon-based composite material and application of carbon-based composite material
CN122809915A
A method for preparing carbon-based composite materials, carbon-based composite materials and their applications