A method for preparing water-based polyester with antibacterial function
By introducing quaternary ammonium salt polymer into water-based polyester, the problem of lack of antibacterial properties of traditional water-based polyester is solved, efficient antibacterial effect and excellent coating performance are achieved, and the environmental and health hazards of using toxic solvents are avoided.
Patent Information
- Application Number
- CN202410980207.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Traditional water-based polyester coatings lack antibacterial properties and require the addition of additional antibacterial agents, which limits their application scope. The synthesis of oil-based polyester resins uses toxic solvents, which harms the environment and human health.
A water-based polyester preparation method including a multi-step reaction is adopted, through the polycondensation of glycolic acid and diethanolamine, and then enamine addition with hydroxyethyl methacrylate to generate tertiary aminated modified polyglycolic acid, and through the polycondensation with water-based The polyester molecular chain is copolymerized, and finally undergoes a quaternization reaction with 2-bromoethyl ether to introduce the quaternary ammonium salt polymer into the polyester molecular chain to achieve antibacterial function.
It achieves the high-efficiency antibacterial effect of water-based polyester materials. The paint film has a smooth appearance, strong adhesion, excellent pencil hardness, and an antibacterial rate of up to 99.99%. No additional antibacterial agents are needed.
Smart Images

Figure SMS_4
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterborne polyester, and in particular to a method for preparing waterborne polyester with antibacterial function. Background Art
[0002] The synthesis of oily polyester resins generally uses highly toxic volatile organic compounds such as xylene as solvents, which poses a hazard to the environment and workers.
[0003] Waterborne polyester coating is an important type of environmentally friendly waterborne coating with the characteristics of high gloss, strong adhesion, high fullness and excellent impact resistance. It can be formulated with water-soluble amino resin into waterborne baking paint. However, traditional waterborne polyester either does not have antibacterial properties or requires the addition of additional antibacterial agents, which limits the application scope of polyester materials. Summary of the invention
[0004] In order to solve the problems mentioned in the above background technology, the present invention provides a method for preparing water-based polyester with antibacterial function.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for preparing water-based polyester with antibacterial function comprises the following steps:
[0007] S1. Add diethylene glycol and 1,6-hexanediol to the reactor under nitrogen conditions, stir and heat to 60-80°C, then add terephthalic acid and catalyst di-n-butyltin oxide, and gradually heat to react until the solid acid value is less than 2;
[0008] S2. Hexahydrophthalic anhydride is then added to the reactor, and the temperature is gradually increased to a solid acid value of 99-102;
[0009] S3. Then trimethylolpropane was added to the reactor, tertiary amine-modified polyglycolic acid, and the temperature was gradually increased to a solid acid value of 18-21;
[0010] S4. Then trimellitic anhydride and dipropylene glycol methyl ether were added to the reactor, and the temperature was gradually increased to a solid acid value of 25.5-27.5;
[0011] S5. Then add 2-bromoethyl ether to the reactor, gradually increase the temperature to 70°C, and keep the reaction for 3h;
[0012] S6. Pass nitrogen through the dilution kettle, add ethylene glycol butyl ether and propylene glycol methyl ether, preheat to 60-80℃, stir at 55-60r / min, transfer the materials in the reactor to the dilution kettle, maintain the dilution temperature at 80-100℃ during the dilution process, after the dilution is completed and the solid content and viscosity tests are qualified, cool to 50-55℃ and discharge the materials to obtain a water-based polyester with antibacterial function.
[0013] Preferably, the conditions for gradually heating up in step S1 are: heating rate of 0.6-0.9°C / min, heating to 144-149°C and keeping warm for 30 minutes, heating rate of 0.4-0.6°C / min after the insulation, heating to 173-178°C and keeping warm for 40 minutes, then heating rate of 0.2-0.3°C / min, heating to the top temperature of 203-205°C, reacting until the solid acid value is less than 2, and cooling to 155-159°C.
[0014] Preferably, the gradual heating conditions in S2 are: heating rate 0.2-0.3°C / min, heating to 187-195°C and keeping warm for 20 minutes, and then continuing to heat to a top temperature of 208-210°C after the insulation is completed, reacting to a solid acid value of 99-102, and cooling to 135-140°C.
[0015] Preferably, the conditions for gradually heating in S3 are: heating rate 0.6-0.9°C / min, heating rate 0.35-0.45°C / min after heating to 150°C, heating rate 0.2-0.3°C / min after heating to 170°C, then heating to 210-212°C, reacting to the solid acid value of 18-21, and cooling to 100-105°C.
[0016] Preferably, the gradual heating conditions in S4 are: heating rate 0.6-0.8°C / min, heating rate 0.2-0.3°C / min after heating to 120°C, heating top temperature 125-135°C, reacting to solid acid value 25.5-27.5, and cooling to 50-55°C.
[0017] Preferably, the stepwise heating condition in S5 is: 0.6-0.8°C / min, heating to 70°C, and keeping the temperature for reaction for 3h.
[0018] Preferably, the molar ratio of diethylene glycol, 1,6-hexanediol, terephthalic acid, hexahydrophthalic anhydride, trimethylolpropane, tertiary amine modified polyglycolic acid, trimellitic anhydride, dipropylene glycol methyl ether, and 2-bromoethyl ether is: (1-5): (2-6): (1-5): (5-10): (1-3): (0.05-0.2): (0.1-0.5): (1-3): (0.05-0.2).
[0019] Preferably, the preparation method of the tertiary amine modified polyglycolic acid is:
[0020] After glycolic acid and diethanolamine are mixed, a catalyst, stannous oxide, is added to carry out a polymerization reaction, and after the reaction is completed, the reaction is cooled to obtain an intermediate.
[0021] Hydroxyethyl methacrylate and the intermediate are dispersed in a proper amount of DMSO for reaction to obtain tertiary amine modified polyglycolic acid.
[0022] Preferably, the molar ratio of glycolic acid to diethanolamine is (15-25):1;
[0023] The molar ratio of hydroxyethyl acrylate and the intermediate is (0.5-2):1.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention firstly performs polycondensation by polymerization of glycolic acid and diethanolamine, and then performs enamine addition with hydroxyethyl methacrylate to obtain tertiary amine-modified polyglycolic acid. Since the tertiary amine-modified polyglycolic acid contains unreacted hydroxyl groups, the tertiary amine-modified polyglycolic acid is introduced into the polyester molecular chain by copolymerization with the carboxyl groups in the water-based polyester molecular chain. Finally, a quaternization reaction is performed with 2-bromoethyl ether to obtain a water-based polyester with antibacterial function.
[0026] 2. Compared with the additional addition of antibacterial agents, the present invention introduces quaternary ammonium salt polymers into the polyester molecular chain, so that the paint film prepared using the water-based polyester of the present invention has a smooth and high-gloss appearance, excellent adhesion and pencil hardness, and an antibacterial rate of up to 99.99%. DETAILED DESCRIPTION
[0027] Unless otherwise specified, the raw materials and reagents used in the present invention are commercially available or can be prepared by known methods.
[0028] Preparation Example 1
[0029] Preparation method of tertiary amine modified polyglycolic acid:
[0030] 760 g of glycolic acid and 52.5 g of diethanolamine were mixed and heated to 85°C, and 7.6 g of stannous oxide catalyst was added to carry out polymerization reaction. After the reaction was completed, the intermediate was cooled to obtain a structure of
[0031] ;
[0032] Disperse 52g of hydroxyethyl methacrylate and 650g of the intermediate in an appropriate amount of DMSO (dimethyl sulfoxide) and react at 70°C for 3h to obtain tertiary amine-modified polyglycolic acid, the structure of which is
[0033] .
[0034] Preparation Example 2
[0035] Disperse 175.5g of tertiary amine modified polyglycolic acid and 15.3g of 2-bromoethyl ether in an appropriate amount of ethanol, gradually increase the temperature at a rate of 0.6-0.8℃ / min to 70℃, and keep the temperature for 3h to obtain a quaternary ammonium salt antibacterial agent, whose structural formula is
[0036] . Example 1
[0037] S1. Under nitrogen conditions, 318g of diethylene glycol and 525g of 1,6-hexanediol were added to the reactor, stirred and heated to 60-80°C, and then 564g of terephthalic acid and 3.76g of di-n-butyltin oxide were added, and the temperature was gradually increased at a heating rate of 0.6-0.9°C / min. When the temperature was increased to 144-149°C, it was kept warm for 30min. After the insulation was completed, the heating rate was 0.4-0.6°C / min, and when the temperature was increased to 173-178°C, it was kept warm for 40min, and then the heating rate was 0.2-0.3°C / min, and the temperature was increased to a top temperature of 203-205°C, and the reaction was carried out until the solid acid value was less than 2, and the temperature was lowered to 155-159°C;
[0038] S2. Then 1206g of hexahydrophthalic anhydride was added to the reactor, and the temperature was gradually increased at a heating rate of 0.2-0.3 ° C / min, and the temperature was increased to 187-195 ° C for 20 min. After the end of the insulation, the temperature was continued to rise to the top temperature of 208-210 ° C, and the reaction was continued until the solid acid value was 99-102, and the temperature was cooled to 135-140 ° C;
[0039] S3. Then 200g of trimethylolpropane and 162.5g of tertiary amine-modified polyglycolic acid were added to the reactor, and the temperature was gradually increased at a rate of 0.6-0.9°C / min. After the temperature was increased to 150°C, the temperature was increased at a rate of 0.35-0.45°C / min. After the temperature was increased to 170°C, the temperature was increased at a rate of 0.2-0.3°C / min, and then the temperature was increased to 210-212°C, and the reaction was continued until the solid acid value reached 18-21, and the temperature was lowered to 100-105°C.
[0040] S4. Then 44g of trimellitic anhydride and 240g of dipropylene glycol methyl ether were added to the reactor, and the temperature was gradually increased at a heating rate of 0.6-0.8 ° C / min. After the temperature was increased to 120 ° C, the heating rate was 0.2-0.3 ° C / min, and the top temperature was increased to 125-135 ° C. The reaction was continued until the solid acid value was 25.5-27.5, and the temperature was cooled to 50-55 ° C.;
[0041] S5. Then 15.3 g of 2-bromoethyl ether was added to the reactor, and the temperature was gradually increased at a rate of 0.6-0.8 ° C / min to 70 ° C, and the reaction was kept warm for 3 h;
[0042] S6. Pass nitrogen through the dilution kettle, add 545g of ethylene glycol butyl ether and 236g of propylene glycol methyl ether, preheat to 60-80℃, stir at 55-60r / min, transfer the materials in the reactor to the dilution kettle, maintain the dilution temperature at 80-100℃ during the dilution process, purge the transfer pipeline with nitrogen after the transfer is completed to ensure that there is no residual resin in the pipeline, take samples for testing after the transfer is completed, and after the solid content and viscosity are qualified, cool to 50-55℃ and discharge the materials to obtain a water-based polyester with antibacterial function. Example 2
[0043] The difference between this embodiment and embodiment 1 is that:
[0044] Add 212 g of diethylene glycol and 643.1 g of 1,6-hexanediol;
[0045] The rest is exactly the same as in Example 1. Example 3
[0046] The difference between this embodiment and embodiment 1 is that:
[0047] Add 730.4 g terephthalic acid and 1051 g hexahydrophthalic anhydride;
[0048] The rest is exactly the same as in Example 1.
[0049] Comparative Example 1 (without adding tertiary amine-modified polyglycolic acid and 2-bromoethyl ether)
[0050] S1. Under nitrogen conditions, 318g of diethylene glycol and 525g of 1,6-hexanediol were added to the reactor, stirred and heated to 60-80°C, and then 564g of terephthalic acid and 3.76g of di-n-butyltin oxide were added, and the temperature was gradually increased at a heating rate of 0.6-0.9°C / min. When the temperature reached 144-149°C, it was kept warm for 30min. After the insulation was completed, the heating rate was 0.4-0.6°C / min, and when the temperature reached 173-178°C, it was kept warm for 40min, and then the heating rate was 0.2-0.3°C / min, and the temperature was raised to a top temperature of 203-205°C, and the reaction was carried out until the solid acid value was less than 2, and the temperature was quickly cooled to 155-159°C;
[0051] S2. Then 1206g of hexahydrophthalic anhydride was added to the reactor, and the temperature was gradually increased at a heating rate of 0.2-0.3 ° C / min, and the temperature was increased to 187-195 ° C for 20 min. After the end of the insulation, the temperature was continued to rise to the top temperature of 208-210 ° C, and the reaction was continued to the solid acid value of 99-102, and the temperature was rapidly cooled to 135-140 ° C;
[0052] S3. Then 200g of trimethylolpropane was added to the reactor, and the temperature was gradually increased at a heating rate of 0.6-0.9 ° C / min. After the temperature was increased to 150 ° C, the heating rate was 0.35-0.45 ° C / min, and the temperature was increased to 170 ° C. After the heating rate was 0.2-0.3 ° C / min, the temperature was increased to 210-212 ° C, the reaction was continued until the solid acid value was 18-21, and the temperature was rapidly cooled to 100-105 ° C;
[0053] S4. Then 44 g of trimellitic anhydride and 240 g of dipropylene glycol methyl ether were added to the reactor, and the temperature was gradually increased at a heating rate of 0.6-0.8 ° C / min. After the temperature was increased to 120 ° C, the heating rate was 0.2-0.3 ° C / min, and the top temperature was increased to 125-135 ° C. The reaction was continued until the solid acid value was 25.5-27.5, and the temperature was rapidly cooled to 50-55 ° C.;
[0054] S5. The dilution kettle is purged with nitrogen, 545 g of ethylene glycol butyl ether and 236 g of propylene glycol methyl ether are added, preheated to 60-80 ° C, stirred at 55-60 r / min, and the materials in the reactor are transferred to the dilution kettle. The dilution temperature is maintained at 80-100 ° C during the dilution process. After the transfer is completed, the transfer pipeline is purged with nitrogen to ensure that there is no residual resin in the pipeline. After the transfer is completed, samples are taken for testing. After the solid content and viscosity are qualified, the temperature is lowered to 50-55 ° C and the material is discharged to obtain water-based polyester.
[0055] Comparative Example 2
[0056] The difference between this comparative example and comparative example 1 is that:
[0057] S5. After the transfer is completed, the transfer pipeline is purged with nitrogen to ensure that there is no residual resin in the pipeline. After the transfer is completed, sampling and testing are performed. After the solid content and viscosity are qualified, the temperature is lowered to 50-55 ° C, 170.5g of the quaternary ammonium antibacterial agent obtained in Preparation Example 2 is added, and the material is stirred and discharged to obtain a water-based antibacterial polyester;
[0058] The rest is exactly the same as Comparative Example 1.
[0059] Results and Testing
[0060] After testing, the water-based polyesters obtained in Examples 1-3 and Comparative Examples 1 and 2 all appeared as light yellow transparent viscous liquids, with solid contents ranging from 68 to 72 and acid values ranging from 16 to 25 mgKOH / g.
[0061] According to the mass parts, 45 parts of water and 5 parts of dimethylaminoethanol were mixed, and 50 parts of water-based polyester prepared in Examples 1-3 and Comparative Examples 1 and 2 were added respectively, and 15 parts of amino resin 325 were added after stirring and mixing, and the mixture was stirred again, and the mixture was allowed to stand for degassing, and the mixture was pre-cured at 60-80°C for 5-10 minutes, and finally cured at 120-140°C for 20-30 minutes. According to the mass parts, 45 parts of water and 5 parts of dimethylaminoethanol were mixed, and 50 parts of water-based polyester prepared in Examples 1-3 and Comparative Examples 1 and 2 were added respectively, and 15 parts of amino resin 325 were added after stirring and mixing, and the mixture was stirred again, and the mixture was allowed to stand for degassing, and the mixture was pre-cured at 60-80°C for 5-10 minutes, and finally cured at 120-140°C for 20-30 minutes;
[0062] Among them, the appearance of the paint film was visually inspected;
[0063] Adhesion was tested according to the hundred-grid method;
[0064] Pencil hardness is tested according to GB / T 6739-2022;
[0065] The antibacterial test method is as follows: the paint films obtained in Examples 1-3 and Comparative Examples 1 and 2 are cut into samples with a radius of 0.5 cm, and then a concentration of 10 8 CFU / mL of Escherichia coli suspension was added with the sample as the experimental group and the blank group without the sample. The suspension was shaken at room temperature for 2 h, and 2 ml was inoculated into beef extract peptone basal medium respectively. The suspension was cultured at 37°C for 24 h. The experiment was repeated 5 times, and the viable bacteria were counted and the average value was taken to calculate the inhibition rate. The inhibition rate = (the number of colonies in the blank group - the number of colonies in the experimental group) / the number of colonies in the blank group × 100%. The results are shown in Table 1.
[0066] Table 1
[0067]
[0068] From the data in Table 1, it can be seen that the paint film prepared using the water-based polyester of the present invention has a smooth and high-gloss appearance and has excellent adhesion, pencil hardness and antibacterial rate;
[0069] By comparing Example 1, Comparative Examples 1 and 2, it can be seen that when the quaternary ammonium salt antibacterial agent is added to the water-based polyester alone, the antibacterial rate is only 68.75%. However, when the quaternary ammonium salt is introduced into the water-based polyester molecular chain through a chemical reaction, the antibacterial rate is increased to 99.99%.
[0070] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing water-based polyester with antibacterial function, characterized in that: The steps include: S1. Add diethylene glycol and 1,6-hexanediol to the reactor under nitrogen conditions, stir and heat to 60-80°C, then add terephthalic acid and catalyst di-n-butyltin oxide, and gradually heat to react until the solid acid value is less than 2; S2. Hexahydrophthalic anhydride is then added to the reactor, and the temperature is gradually increased to a solid acid value of 99-102; S3. Then trimethylolpropane was added to the reactor, tertiary amine-modified polyglycolic acid, and the temperature was gradually increased to a solid acid value of 18-21; S4. Then trimellitic anhydride and dipropylene glycol methyl ether were added to the reactor, and the temperature was gradually increased to a solid acid value of 25.5-27.5; S5. Then add 2-bromoethyl ether to the reactor, gradually increase the temperature to 70°C, and keep the reaction for 2-4h; S6. The dilution kettle was purged with nitrogen, ethylene glycol butyl ether and propylene glycol methyl ether were added, preheated to 60-80 ° C, stirred at 55-60 r / min, and the reactor material was transferred to the dilution kettle. The dilution temperature was maintained at 80-100 ° C during the dilution process. After the dilution was completed, the solid content and viscosity were tested to be qualified, and the temperature was lowered to 50-55 ° C to discharge the material to obtain a water-based polyester having an antibacterial function; The preparation method of the tertiary amine modified polyglycolic acid: After glycolic acid and diethanolamine are mixed, a catalyst, stannous oxide, is added to carry out a polymerization reaction, and after the reaction is completed, the reaction is cooled to obtain an intermediate. Dispersing hydroxyethyl methacrylate and the intermediate in an appropriate amount of DMSO for reaction to obtain tertiary amine-modified polyglycolic acid; The molar ratio of glycolic acid to diethanolamine is (15-25):1; The molar ratio of hydroxyethyl acrylate and the intermediate is (0.5-2):
1.
2. The method for preparing a water-based polyester with antibacterial function according to claim 1, characterized in that: The conditions for gradually increasing the temperature in step S1 are: a heating rate of 0.6-0.9°C / min, heating to 144-149°C and keeping the temperature for 30 minutes, a heating rate of 0.4-0.6°C / min after the insulation is completed, heating to 173-178°C and keeping the temperature for 40 minutes, then a heating rate of 0.2-0.3°C / min, heating to a top temperature of 203-205°C, reacting until the solid acid value is less than 2, and then cooling to 155-159°C.
3. The method for preparing a water-based polyester with antibacterial function according to claim 1, characterized in that: The conditions for gradually increasing the temperature in S2 are: a heating rate of 0.2-0.3°C / min, heating to 187-195°C and keeping the temperature for 20 minutes, and then continuing to heat to a top temperature of 208-210°C after the insulation is completed, reacting until the solid acid value reaches 99-102, and then cooling to 135-140°C.
4. The method for preparing a water-based polyester with antibacterial function according to claim 1, characterized in that: The conditions for gradually increasing the temperature in S3 are: a heating rate of 0.6-0.9°C / min, a heating rate of 0.35-0.45°C / min after the temperature reaches 150°C, a heating rate of 0.2-0.3°C / min after the temperature reaches 170°C, then a heating rate of 0.2-0.3°C / min, then a heating rate of 210-212°C, reaction until the solid acid value reaches 18-21, and then a cooling rate of 100-105°C.
5. The method for preparing water-based polyester with antibacterial function according to claim 1, characterized in that: The conditions for gradually increasing the temperature in S4 are: a heating rate of 0.6-0.8°C / min, a heating rate of 0.2-0.3°C / min after the temperature reaches 120°C, a top temperature of 125-135°C, reaction until the solid acid value reaches 25.5-27.5, and then cooling to 50-55°C.
6. The method for preparing water-based polyester with antibacterial function according to claim 1, characterized in that: The stepwise heating condition in S5 is: 0.6-0.8°C / min, heating to 70°C, and keeping the temperature for reaction for 3 hours.
7. The method for preparing water-based polyester with antibacterial function according to claim 1, characterized in that: The molar ratio of diethylene glycol, 1,6-hexanediol, terephthalic acid, hexahydrophthalic anhydride, trimethylolpropane, tertiary amine modified polyglycolic acid, trimellitic anhydride, dipropylene glycol methyl ether, and 2-bromoethyl ether is: (1-5): (2-6): (1-5): (5-10): (1-3): (0.05-0.2): (0.1-0.5): (1-3): (0.05-0.2).