Biodegradable polymer foam particles and preparation method thereof

Through the combination of materials such as polylactic acid, thermoplastic starch and high pressure foaming process, polymer foamed particles with high foaming ratio, low bulk density and good biodegradability were prepared, which solved the problem of insufficient material performance in the prior art. , achieving improvements in strength and degradability.

CN118496644BActive Publication Date: 2024-11-19SHANGHAI ZHENFENG APARTMENT MANAGEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410766239.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-11-19
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

Existing polymer foaming materials are difficult to achieve high foaming ratio, low bulk density and good biodegradability. The mechanical properties of thermoplastic starch are poor and water resistance, resulting in thin and easy rupture of the bubble wall, which cannot meet market demand.

Method used

Biodegradable polymers are prepared by mixing, extruding and high-pressure foaming processes using a combination of polylactic acid, thermoplastic starch, EBP oxidation-biobiodegradation additive, TMC nucleating agent, plasticizer, anti-hydrolyzing agent and light stabilizer. Foaming particles, the foamability and sheet compression modulus are improved by combining EBP and TMC nucleating agents.

Benefits of technology

It achieves high foaming ratio, low bulk density and good biodegradability, and improves the compression strength and rapid degradation performance of the plate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a biodegradable polymer foam particle and a preparation method thereof, comprising the following components: polylactic acid, thermoplastic starch, a compatibilizer, an EBP oxidation-biological dual degradation additive, a TMC nucleating agent, a plasticizer, an anti-hydrolysis agent, and a light stabilizer. The invention solves the problem of poor dispersion effect of polylactic acid and EBP by adding a compatibilizer and thermoplastic starch. Meanwhile, EBP acts as a heterogeneous nucleating agent in the foaming process, and is compounded with the TMC nucleating agent, thereby greatly improving the foamability of the polylactic acid and the compression strength of the foamed plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to the field of degradable plastics, and more particularly to biodegradable polymer foam particles and a preparation method thereof. Background technology:

[0002] Polymer foam materials are generally based on resins and are formed by physical or chemical foaming methods to form a foam with uniform open or closed cell structure. Polymer foam materials have the advantages of light weight, good cushioning performance, good heat insulation and sound insulation, etc. They can be widely used in industrial products such as electronics and precision equipment, as well as shockproof linings for daily necessities such as ceramics and home appliances, becoming an indispensable cushioning packaging material for the modern packaging industry.

[0003] At present, most polymer foam materials are polystyrene, polyurethane, etc. While they bring great convenience to our lives and production, they also inevitably bring some troubles, such as difficulty in degradation and resulting in serious white pollution.

[0004] Starch is rich in source and cheap. It is decomposed into glucose under the action of microorganisms, and finally metabolized into water and carbon dioxide. It will not cause harm to the environment and is an inexhaustible renewable resource. However, the thermoplastic starch prepared by plasticizing starch with plasticizers only has poor mechanical properties, is brittle, and has poor water resistance. On this basis, the thermoplastic starch foamed material prepared by adding a foaming agent has poor melt strength, which can cause the bubble wall to be thin, prone to rupture and collapse, and has uneven cell size and distribution, low expansion rate and rebound rate, which is difficult to adapt to the demand of the market. Therefore, modified starch (physical or chemical modification) is used to compound with reinforcements such as inorganic fillers and fibers, with resin as toughening body, assisted by other auxiliary agents, and the preparation of reinforcement / starch biodegradable composite foaming material has become the focus of current research.

[0005] Patent CN1041406569B discloses a polylactic acid foamed particle and a preparation method thereof, which is composed of polylactic acid, a modified resin, a nucleating agent, a flame retardant, and an antioxidant, wherein the modified resin is an amorphous α-olefin copolymer or a petroleum resin; in this method, the addition of petroleum resin will lead to a decrease in the degradability of the polylactic acid foamed particles.

[0006] Patent CN109825046B discloses a biodegradable polylactic acid foam particle and a preparation method thereof. Using dextrorotatory polylactic acid as a matrix material can improve the biodegradability of polylactic acid foam products. However, the common polylactic acid brands on the market are mainly l-lactic acid, and using dextrorotatory polylactic acid as a matrix material does not meet the needs of large-scale production. Summary of the invention:

[0007] The present invention provides a biodegradable polymer foamed particle and a preparation method thereof, and obtains foamed particles with high foaming ratio and low bulk density; at the same time, the molded body prepared from the foamed particles has good biodegradability and plate compression strength.

[0008] To achieve the technical purpose of the present invention, the present invention provides a biodegradable polymer foam particle, which is made of the following raw materials in parts by weight: 50-60 parts of polylactic acid, 15-20 parts of thermoplastic starch, 1-2 parts of a compatibilizer, 1-2 parts of an EBP oxidation-biodegradable dual-degradation additive, 0.5-2 parts of a TMC nucleating agent, 0.5-2 parts of a plasticizer, 0.5-1 parts of an anti-hydrolysis agent, and 0.5-1 parts of a light stabilizer.

[0009] Furthermore, the polylactic acid model is selected as PLA3052 or PLA3251D.

[0010] Furthermore, the TMC nucleating agent is one or more of TMC-200, TMC-300, and TMC-306.

[0011] Furthermore, the compatibilizer is maleic anhydride grafted polyolefin elastomer (POE-g-MAH).

[0012] Furthermore, the plasticizer is one or more of glycerol, sorbitol, and ethylene glycol.

[0013] Furthermore, the anti-hydrolysis agent is a carbodiimide anti-hydrolysis agent.

[0014] Furthermore, the light stabilizer is a hindered amine light stabilizer.

[0015] The method for preparing the biodegradable polymer foam particles comprises the following steps:

[0016] (1) mixing, extruding and pelletizing polylactic acid, thermoplastic starch, a compatibilizer, an EBP oxidation-biodegradable additive, a TMC nucleating agent, a plasticizer, an anti-hydrolysis agent and a light stabilizer to prepare a foaming masterbatch;

[0017] (2) placing the foaming masterbatch into a high-pressure reactor, maintaining the reaction mixture under a pressure of 13-18 MPa, a temperature of 140-160° C. and the presence of a foaming gas for 0.5-4 h, then cooling the reaction mixture to a foaming temperature of 80-130° C. for foaming for 0.5-1 h, and finally rapidly releasing the pressure to atmospheric pressure within 0.5-20 s, introducing cooling water for shaping, and obtaining polymer foam particles.

[0018] Furthermore, in step (1), a high-speed mixer is used for mixing, the mixing temperature is 90-110° C., the stirring rate is 800-1200 r / min, and the mixing time is 40-60 min.

[0019] Furthermore, the extrusion in step (1) adopts a twin-screw extruder, and the temperature of each section of the extruder is 130-150°C, 140-160°C, 160-170°C, 170-180°C, 160-170°C, 150-160°C; the feeding speed is 20-30r / min, and the main engine speed is 80-100r / min.

[0020] Furthermore, the foaming gas used in step (2) is supercritical carbon dioxide or nitrogen, or a mixture of the two.

[0021] The oxidation-biodegradation additive EBP is a degradable masterbatch produced by Shandong Tianzhuang Environmental Protection Technology Co., Ltd., which is formed by adding an additive that can accelerate the oxidation-biodegradation process to a polyolefin resin. This masterbatch is suitable for polyolefin systems such as polyethylene. When it is applied to a polyester system, there will be problems such as poor dispersion effect and inability to effectively promote polyester hydrolysis and degradation. The present invention effectively solves the problems of poor dispersion effect and inability to effectively promote degradation by adding a compatibilizer and thermoplastic starch to EBP.

[0022] At the same time, the EBP in the present invention is used in combination with the TMC nucleating agent in the present invention. During foaming, EBP acts as a heterogeneous nucleating agent, which can effectively promote the heterogeneous foaming nucleation of polylactic acid, and cooperates with the induced crystallization of the TMC nucleating agent to greatly improve the foamability of polylactic acid and the compression modulus of the sheet after foaming.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention makes full use of the dual properties of the compatibilizer and the ability of thermoplastic starch to be blended with polylactic acid and polyolefins at the same time, so as to well connect polylactic acid and EBP. At the same time, the different degradation principles and characteristics of thermoplastic starch and EBP are utilized, thereby ensuring that the final product has good degradability.

[0025] (2) The EBP in the present invention can act as a heterogeneous nucleating agent during the foaming process and interact with the TMC nucleating agent in the present invention to significantly improve the foamability of polylactic acid and the compressive strength of the foamed sheet. Specific implementation method:

[0026] In order to make the purpose, technical scheme and advantages of the present invention more clear, the technical scheme of the present invention is further described below through specific implementation methods. Those skilled in the art should know that the embodiments are only to help understand the technical content and technical effects of the present invention and should not be regarded as limiting the present invention.

[0027] The polylactic acid in the embodiments and comparative examples of the present invention is selected from PLA3052 or PLA3251D of NatureWorks; the anti-hydrolysis agent is selected from Bio-SW100 or Bio-SW500; the EBP is selected from EBP-pp-1502 or EBP-pp-1501 produced by Shandong Tianzhuang Environmental Protection Co., Ltd.; the compatibilizer POE-g-MAH is selected from Fusabond N495 of DuPont; the light stabilizer is selected from UV-3853 or UV944 of Hefei Tianjian Chemical Co., Ltd. TMC nucleating agent and anti-hydrolysis agent are purchased from Shanxi Chemical Research Institute (Co., Ltd.); plasticizers are purchased from Shanghai McLean Biochemical Technology Co., Ltd. The thermoplastic starch in the embodiment is purchased from Suzhou Minghua Sugar Alcohol Co., Ltd., and the cassava starch in the comparative example is purchased from Shandong Gushuo Biotechnology Co., Ltd.

[0028] The present invention includes 3 embodiments and 3 comparative examples.

[0029] Embodiment 1:

[0030] (1) 50 parts of polylactic acid PLA3052, 15 parts of thermoplastic starch, 1.5 parts of compatibilizer Fusabond N495, 1.5 parts of EBP-pp-1501, 1 part of nucleating agent TMC-200, 1 part of glycerol, 0.5 parts of anti-hydrolysis agent Bio-SW500, and 0.5 parts of light stabilizer UV-3853 were added to a mixer, and stirred and mixed at 100° C. and 1000 r / min for 50 min to obtain a mixed material; the mixed material was put into a twin-screw extruder for extrusion granulation, and foaming masterbatch was obtained after cooling and pelletizing; the setting conditions of the extruder were as follows: the temperature of each section of the extruder was 145° C., 155° C., 165° C., 170° C., 165° C., 155° C., the feed speed was 30 r / min, and the main engine speed was 100 r / min;

[0031] (2) placing the foaming masterbatch obtained in step (1) into a high-pressure reactor, maintaining it at a pressure of 16 MPa, a temperature of 150° C. and the presence of carbon dioxide for 2 h, then cooling it to a foaming temperature of 130° C. for foaming for 0.5 h, and finally rapidly releasing the pressure to atmospheric pressure within 5 s, introducing cooling water to shape it, and obtaining polymer foam particles.

[0032] Embodiment 2:

[0033] (1) 50 parts of polylactic acid PLA3052, 20 parts of thermoplastic starch, 1 part of compatibilizer Fusabond N495, 2 parts of EBP-pp-1501, 1 part of nucleating agent TMC-200, 1 part of glycerol, 0.5 parts of anti-hydrolysis agent Bio-SW100, and 1 part of light stabilizer UV-3853 were added to a mixer, and stirred and mixed at 100° C. and 1200 r / min for 40 minutes to obtain a mixed material; the mixed material was put into a twin-screw extruder for extrusion granulation, and foaming masterbatch was obtained after cooling and pelletizing; the setting conditions of the extruder were as follows: the temperature of each section of the extruder was 145° C., 155° C., 165° C., 170° C., 165° C., 155° C., the feed speed was 30 r / min, and the main engine speed was 100 r / min;

[0034] (2) placing the foaming masterbatch obtained in step (1) into a high-pressure reactor, maintaining it for 3 hours at a pressure of 14 MPa, a temperature of 140° C. and the presence of carbon dioxide, then cooling it to a foaming temperature of 100° C. for foaming for 1 hour, and finally rapidly releasing the pressure to atmospheric pressure within 2 seconds, introducing cooling water to shape it, and obtaining polymer foam particles.

[0035] Embodiment 3:

[0036] (1) adding 60 parts of polylactic acid PLA3251D, 15 parts of thermoplastic starch, 1 part of compatibilizer Fusabond N495, 1.5 parts of EBP-pp-1502, 1 part of nucleating agent TMC-300, 1 part of sorbitol, 0.5 parts of anti-hydrolysis agent Bio-SW500, and 0.5 parts of UV-944 into a mixer, stirring and mixing at 100° C. and 1200 r / min for 30 min to obtain a mixed material; putting the mixed material into a twin-screw extruder for extrusion granulation, cooling and pelletizing to obtain a foaming masterbatch; the temperature of each section of the extruder is 145° C., 155° C., 165° C., 170° C., 165° C., 155° C., the feed speed is 20 r / min, and the main engine speed is 80 r / min;

[0037] (2) placing the foaming masterbatch obtained in step (1) into a high-pressure reactor, maintaining it for 1 hour at a pressure of 16 MPa, a temperature of 160° C. and the presence of carbon dioxide, then cooling it to a foaming temperature of 80° C. for foaming for 1 hour, and finally rapidly releasing the pressure to atmospheric pressure within 5 seconds, introducing cooling water to shape it, and obtaining polymer foam particles.

[0038] Comparative Example 1:

[0039] The difference from Example 1 is that the thermoplastic starch is replaced by cassava starch.

[0040] Comparative Example 2:

[0041] The difference from Example 1 is that the compatibilizer Fusabond N495 is not added.

[0042] Comparative Example 3:

[0043] The difference from Example 1 is that no EBP is added, and the amount of nucleating agent TMC-200 is increased to 3 parts.

[0044] The bulk density, compression strength and weight loss rate of Examples 1-3 and Comparative Examples 1-3 were tested.

[0045] (1) Bulk density ρr: The test was conducted by the water displacement method. A certain amount of expanded particles (greater than 50 particles) in the embodiments and comparative examples were taken and weighed, which was recorded as m1. A certain amount of water was added to a measuring cylinder, and the volume at this time was recorded as V0. The expanded particles were placed until they were completely immersed, and the volume at this time was recorded as V1. The bulk density was calculated using the following formula: ρ r =m1 / (V1-V0).

[0046] (2) Compression strength: The foamed particles prepared in Examples 1-3 and Comparative Examples 1-3 were molded using a steam box molding machine to obtain foamed molded bodies. Samples of 50×50×25 mm were cut out and subjected to compression strength tests based on the U.S. ASTM standard D3575-08. The compression test was performed at a compression speed of 10 mm / min to obtain the compression strength of the molded body when it was compressed by 50%.

[0047] (3) Weight loss rate (%): The weight loss rate after burying in soil for 60 days is used as the weight loss rate of the prepared foamed particles: a foamed molded body sample of 50×50×25 mm is cut out and weighed and the weight of each standard sample is recorded; then the standard sample is wrapped in gauze and buried in the soil 20 cm above the ground surface; after 60 days, it is taken out, washed, dried, weighed and the weight is recorded. The weight loss rate of the standard sample is calculated by the following method: weight loss rate (%) = (weight before test - weight after 60 days) / weight before test × 100%.

[0048] In order to better verify the effect of the present invention, the above tests all use 5 groups of samples, and the final results are averaged, as shown in Table 1.

[0049] Test items <![CDATA[Bulk density (g / cm 3 )]]> Compression strength(MPa) Weight loss rate (%) Example 1 0.09 1.67 76.4 Example 2 0.08 1.59 78.9 Example 3 0.11 1.62 74.8 Comparative Example 1 0.21 0.94 72.7 Comparative Example 2 0.17 1.15 64.3 Comparative Example 3 0.14 1.28 58.1

[0050] From the results of Examples 1-3 and Comparative Examples 1-3, it can be seen that the compounding of EBP, thermoplastic starch, compatibilizer, and nucleating agent can make the expanded particles have low bulk density, high compression strength, and good degradability. Since the expanded particles prepared by the present invention are a porous structure material, the active components in EBP have more opportunities to contact oxygen and water in the soil; at the same time, the thermoplastic starch produces a large amount of acidic substances under the erosion of soil microorganisms, which promotes the rapid degradation of the expanded particles of the present invention.

[0051] From the comparison between Example 1 and Comparative Example 1, when cassava starch is added instead of thermoplastic starch, the overall dispersion effect of the composite material formed is not good, so the foaming effect is obviously not as good as the composite of thermoplastic starch, resulting in insufficient bulk density and compression strength of the foam.

[0052] From the comparison between Example 1 and Comparative Example 2, it can be seen that the presence of the compatibilizer can more fully exert the degradation effect and heterogeneous nucleation effect of EBP, thereby improving the foaming property, compression strength and degradability of the foamed particles as a whole.

[0053] From the comparison between Example 1 and Comparative Example 3, the compounding of EBP and TMC as nucleating agents can make the foamed particles have better foamability and compressive strength than adding only TMC nucleating agent; even if the amount of TMC nucleating agent is increased, the effect after compounding cannot be achieved.

[0054] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A biodegradable polymer foam particle, characterized in that: The invention is prepared from the following raw materials in parts by weight: 50-60 parts of polylactic acid, 15-20 parts of thermoplastic starch, 1-2 parts of compatibilizer, 1-2 parts of EBP oxidation-biological dual degradation additive, 0.5-2 parts of TMC nucleating agent, 0.5-2 parts of plasticizer, 0.5-1 parts of anti-hydrolysis agent and 0.5-1 parts of light stabilizer; the compatibilizer is maleic anhydride grafted polyolefin elastomer.

2. The biodegradable polymer foam particles according to claim 1, characterized in that: The polylactic acid model is PLA3052 or PLA3251D.

3. The biodegradable polymer foam particles according to claim 1, characterized in that: The TMC nucleating agent is one or more of TMC-200, TMC-300 and TMC-306; the plasticizer is one or more of glycerol, sorbitol and ethylene glycol; the anti-hydrolysis agent is a carbodiimide anti-hydrolysis agent; and the light stabilizer is a hindered amine light stabilizer.

4. A method for preparing the biodegradable polymer foam particles according to any one of claims 1 to 3, characterized in that: The steps include: (1) mixing, extruding and pelletizing polylactic acid, thermoplastic starch, a compatibilizer, an EBP oxidation-biodegradable additive, a TMC nucleating agent, a plasticizer, an anti-hydrolysis agent and a light stabilizer to prepare a foaming masterbatch; (2) The foaming masterbatch is placed in a high-pressure reactor, maintained at a pressure of 13-18 MPa, a temperature of 140-160°C and the presence of a foaming gas for 0.5-4 h, then cooled to a foaming temperature of 80-130°C for foaming for 0.5-1 h, and finally the pressure is quickly released to atmospheric pressure within 0.5-20 s, and cooling water is introduced to shape the polymer foamed particles.

5. The method for preparing biodegradable polymer foam particles according to claim 4, characterized in that: In step (1), a high-speed mixer is used for mixing, the mixing temperature is 90-110° C., the stirring rate is 800-1200 r / min, and the mixing time is 40-60 min.

6. The method for preparing biodegradable polymer foam particles according to claim 4, characterized in that: The extrusion in step (1) adopts a twin-screw extruder, and the temperature of each section of the extruder is 130-150°C, 140-160°C, 160-170°C, 170-180°C, 160-170°C, 150-160°C; the feeding speed is 20-30r / min, and the main engine speed is 80-100r / min.

7. The method for preparing biodegradable polymer foam particles according to claim 4, characterized in that: The foaming gas used in step (2) is supercritical carbon dioxide or nitrogen, or a mixture of the two.

Citation Information

Patent Citations

  • A biodegradable polylactic acid foaming particle and its preparation method

    CN109825046B

  • Bi-axially stretched article

    CN104470986A

  • Bio-based fully-degradable plastic masterbatch as well as preparation method and application thereof