A method for improving the wear resistance of aluminum alloy resistance spot welding electrode end surface
By depositing a high-entropy alloy wear-resistant layer on the end surface of the aluminum alloy resistance spot welding electrode, the corrosion and adhesion problems caused by the metallurgical reaction between copper alloy and aluminum alloy are solved, the wear resistance and service life of the electrode are improved, and the welding quality is ensured.
Patent Information
- Application Number
- CN202410955951.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-17
AI Technical Summary
During the use of aluminum alloy resistance spot welding electrodes, the metallurgical reaction between copper alloy and aluminum alloy causes end surface corrosion and adhesion, resulting in poor wear resistance and affecting welding quality and electrode life.
An electric spark process is used to deposit a high-entropy alloy wear-resistant layer on the end surface of the copper alloy electrode, and the high-entropy alloy material is melted by high-temperature heating to form a metallurgically bonded wear-resistant layer to avoid alloying and adhesion.
The wear resistance of the resistance spot welding electrode end surface is improved, the service life of the electrode is extended, and the wear resistance of the electrode is enhanced without reducing the electrical conductivity and thermal conductivity.
Smart Images

Figure CN118497751B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material science and engineering technology, and in particular relates to a method for improving the wear resistance of an aluminum alloy resistance spot welding electrode end surface. Background Art
[0002] Aluminum alloy is the most widely used and consumed alloy among light alloys, and is now widely used in the manufacture of automobile bodies. Due to the requirements and limitations of technologies such as battery energy density, new energy vehicles have higher requirements for lightweighting than traditional energy vehicles. The use of aluminum alloy materials can effectively reduce the weight of the body, which is more in line with the development trend of new energy vehicles. At present, the core issue of the application of aluminum alloy in automobile bodies is the connection technology. The connection of aluminum alloys needs to consider three aspects: parent material, connection process and connection technology. In the process of automobile lightweighting, the connection technologies of aluminum alloy bodies include cold connection and welding. Among them, cold connection includes pressure riveting nuts, SPR lock riveting technology, rivetless riveting, friction plug riveting welding and hot melt rotary tapping riveting. Resistance spot welding is a method of using the resistance heat generated by the current passing through the contact surface and adjacent areas of the connection joint under the condition of applying pressure to form a local melting or plastic melting state to form a metal bond. Resistance spot welding is one of the most widely used welding technologies in the manufacture of automobile steel bodies due to its reliable quality, high efficiency, economy and easy use of robots for automated welding.
[0003] However, there are still many problems in the current resistance spot welding of aluminum alloys compared with steel structural materials. First, the quality of aluminum alloy resistance spot welding welds is unstable, which is reflected in serious spattering and splattering, poor surface forming quality of welds, cracks and pores defects inside the molten core, and unstable molten core size. Secondly, the copper alloy electrode used in the resistance spot welding process is prone to metallurgical reaction with aluminum alloy, copper and aluminum form low-melting point eutectic compounds, and the copper alloy electrode end surface is melted and eroded, resulting in very serious adhesion. The electrode end surface is seriously burned, which reduces the service life of the electrode. Studies have found that the metallurgical reaction between copper alloy electrodes and aluminum alloys is the main cause of wear and failure of resistance spot welding electrodes, and the wear and failure position usually occurs at the electrode end surface. The electrode is a key component used to transmit pressure and current to the workpiece during the resistance spot welding production process. The wear of the electrode end surface increases the contact area between the electrode and the workpiece, changes the electrical and thermal conductivity of the contact surface between the electrode and the workpiece, and seriously affects the current density and electrode pressure of the contact surface between the electrode and the workpiece, which will inevitably affect the formation of the molten core of the spot welding joint. In the process of resistance spot welding of aluminum alloys, electrode wear failure caused by corrosion and adhesion of the electrode end surface has become one of the main factors affecting the quality of resistance spot welded aluminum alloy joints.
[0004] Resistance spot welding electrodes are consumables in production, and their consumption is relatively large. Performance and cost are factors that must be considered in the production process of many companies. Traditional resistance spot welding electrode materials are mostly made of copper alloy materials such as chromium zirconium copper, chromium bronze, copper chromium alloy, copper beryllium alloy, tungsten copper alloy and tungsten molybdenum copper. Resistance spot welding electrode materials are required to withstand high temperature and high pressure at the same time, that is, thermal and force coupling. The electrode material requires excellent high temperature strength, electrical conductivity and thermal conductivity. The electrode end surface needs to be reasonably designed. Otherwise, the resistance spot welding electrode will be aggravated during use, thereby increasing the electrode dressing time and wasting too much electrode material. Therefore, the selection of resistance spot welding electrode material type and electrode end surface morphology needs to be determined according to the specific material to be spot welded. The design of aluminum alloy resistance spot welding electrode material should also consider the metallurgical reaction between the electrode end surface and the aluminum alloy weldment at the spot welding contact surface. For aluminum alloy resistance spot welding, traditional resistance spot welding electrodes can no longer meet production requirements. How to improve the service life of aluminum alloy resistance spot welding electrodes has always been the goal pursued by welding and related researchers.
[0005] In the prior art, research work aimed at improving the service life of resistance spot welding electrodes includes resistance spot welding electrode structure design, resistance spot welding electrode process optimization, resistance spot welding electrode end surface treatment, resistance spot welding electrode materials, etc. Among them, as to how to solve the problem of reducing the alloying and adhesion between copper electrodes and aluminum alloys during resistance spot welding, the research mainly focuses on strengthening the matrix material of resistance spot welding electrodes or treating the end surface of copper alloy electrodes, such as copper-tungsten heavy alloy composite electrodes. Matrix strengthening is to add various ceramic particle reinforcement phases and refractory metals to copper alloys, such as Al2O3, TiC, TiB2, Zr2O3, SiC, B4C, WC, Co, Mo, Nb, Ta and W. At the same time, improving the mechanical properties and thermal stability of copper alloys, adding various ceramic particle reinforcement phases and refractory metals will inevitably reduce the electrical conductivity and thermal conductivity of resistance spot welding electrodes. Generally, the technologies used for the surface treatment of the electrode end face include coating various paints and coatings on the end face of the spot welding electrode, such as graphite-engine oil paint, TiB2 / Cu composite materials, self-generated ceramic particles reinforced copper-based gradient spot welding electrodes, and brazing process to connect a layer of high-temperature alloy or cemented carbide to the end face of the copper alloy resistance spot welding electrode to form a composite electrode or a combined electrode. However, there is a lack of reliable data support for the durability, reliability and stability of the coating of various paints and coatings. In summary, the electrode end face corrosion, adhesion, end face wear and unstable spot welding quality encountered in the resistance spot welding production process of aluminum alloy structural parts are technical problems that need to be solved urgently. Summary of the invention
[0006] The purpose of the present invention is to provide a method for improving the wear resistance of the end face of an aluminum alloy resistance spot welding electrode, using an electric spark process to deposit a high entropy alloy wear-resistant layer with metallurgical bonding on the end face of a copper alloy electrode, so as to solve the problem of improving the wear resistance of the end face of a resistance spot welding electrode and avoiding alloying and adhesion between the end face of the electrode and the material to be welded at the contact surface. This method melts the high entropy alloy material at the end face of an aluminum alloy resistance spot welding electrode by high-temperature heating, and the rapidly solidified high entropy alloy forms a wear-resistant layer with metallurgical bonding at the end face with the resistance spot welding copper alloy electrode substrate, which improves the wear resistance of the end face of the resistance spot welding electrode, and can repair the local damaged part of the end face of the aluminum alloy resistance spot welding electrode.
[0007] The objective of the present invention is achieved through the following technical solutions:
[0008] A method for improving the wear resistance of an aluminum alloy resistance spot welding electrode end surface comprises the following steps:
[0009] A. Preparation of high entropy alloy powder:
[0010] The high entropy alloy powder is prepared by mixing any six metal powders of copper powder, tungsten powder, molybdenum powder, zirconium powder, niobium powder, vanadium powder, chromium powder, nickel powder and iron powder and vacuum ball milling, and the six metal elements have the same molar fraction, and the molar ratio is fixed at 1:1:1:1:1:1;
[0011] B. Preparation of high entropy alloy rods:
[0012] The high entropy alloy powder obtained in step A is melted in a vacuum arc melting furnace and evacuated to Pa, filled with argon as a protective gas, and repeatedly melted 9 times by arc heating to obtain a basic alloy ingot with uniform composition;
[0013] C. Mechanically treat the end surface of the copper alloy electrode body to remove surface oxides and various oil stains;
[0014] D. Electrospark deposition: The prepared high entropy alloy rod is evenly coated on the end surface of the pretreated copper alloy electrode body by electrospark deposition process to form a high entropy alloy wear-resistant layer;
[0015] E. End face finishing: The end face of the copper alloy electrode is processed by mechanical processing methods to obtain the geometric structure dimensions that meet the resistance spot welding electrode.
[0016] Furthermore, in step A, the purity of the metal used is greater than 99.9%, and the particle size of the metal powder is 15-40 μm.
[0017] Furthermore, in step A, the element composition of the high entropy alloy is 16.6% by atomic percentage.
[0018] Further, step A, the ball milling process, is specifically as follows: six kinds of metal powders are accurately weighed in molar proportion and put into a ball mill jar, three kinds of zirconium oxide ball milling beads with diameters of 10 mm, 5 mm and 3 mm are used, the weight ratio is 5:2:4, the ball-to-material ratio is 12:1, the ball milling speed is 350 r / min, and the ball milling time is 15-20 h.
[0019] Furthermore, in step B, the current of arc melting the high entropy alloy powder is 300-400A.
[0020] Furthermore, in step C, the thickness of the high entropy alloy coating is 150-520 μm.
[0021] Furthermore, in step D, the process parameters of the electrospark deposition are: voltage 65-83V, frequency 210-252Hz, and the interface forms a dense metallurgical bond.
[0022] A resistance spot welding electrode made by a method for improving the wear resistance of the end face of an aluminum alloy resistance spot welding electrode, characterized in that it includes a copper alloy electrode body, the end face of the copper alloy electrode body is coated and a layer of high entropy alloy wear-resistant layer with metallurgical bonding is deposited by an electric spark process, and the thickness of the high entropy alloy wear-resistant layer is 150~520μm.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention deposits a layer of high entropy alloy on the end face of a copper alloy electrode for resistance spot welding by an electric spark process, obtains a high entropy alloy wear-resistant layer with metallurgical bonding on the end face of the copper alloy electrode, improves the wear resistance of the end face without reducing the electrical conductivity, thermal conductivity and high-temperature mechanical properties of the copper alloy electrode material, and avoids alloying and adhesion between the end face of the electrode and the material to be welded at the contact surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0026] Figure 1 It is a schematic diagram of the principle and process of resistance spot welding;
[0027] Figure 2 It is a schematic diagram of the structure of the resistance spot welding electrode prepared by the electrospark deposition process of the present invention;
[0028] Figure 3 It is the metallurgical bonding interface between the copper alloy body and the high entropy alloy wear-resistant layer.
[0029] In the figure, 1. High entropy alloy wear-resistant layer 2. Copper alloy electrode body. DETAILED DESCRIPTION
[0030] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only parts related to the present invention, rather than all structures, are shown in the accompanying drawings.
[0031] It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further defined and explained in the subsequent drawings. At the same time, in the description of the present invention, the terms "first", "second", etc. are only used to distinguish the description and cannot be understood as indicating or implying relative importance.
[0032] Research has found that the main reason for the wear and failure of resistance spot welding electrodes is that copper alloy electrodes are prone to metallurgical reactions with aluminum alloys, and the wear and failure location usually occurs at the electrode end face. This is because the resistivity of aluminum alloy is only 1 / 3 of that of steel, and the thermal conductivity is nearly 4 times that of steel, which makes the contact surface between the resistance spot welding electrode and the aluminum weldment generate less heat and dissipate heat quickly, so it is necessary to use the hard specification of resistance spot welding for welding. At the same time, the melting temperature of aluminum alloy is relatively low. Under the action of hard specification, the spot welding contact surface heats up rapidly, which is very easy to produce splashes, causing corrosion of the copper alloy electrode end face and damage to the aluminum alloy weld, seriously affecting product quality. In addition, during the resistance spot welding process, the end face of the electrode is in direct contact with the high-temperature workpiece surface, and is repeatedly subjected to high temperature and high pressure. The heat and force during spot welding are mainly concentrated between the upper and lower electrode end faces and the welded workpiece. To this end, the present invention provides a method for improving the wear resistance of the end face of an aluminum alloy resistance spot welding electrode, which effectively solves the following three technical problems: 1. Electrode corrosion and adhesion caused by alloying of the end face of a copper alloy electrode during the production process of a resistance spot welding aluminum alloy material structural part; 2. The metallurgically bonded wear-resistant layer formed at the end face of the copper alloy electrode cannot affect the function of the electrode, that is, electrical and thermal conductivity; 3. The metallurgically bonded wear-resistant layer formed at the end face of the copper alloy electrode is superior to the copper alloy electrode body material.
[0033] The core technology of this method is to deposit a layer of high entropy alloy on the end surface of the copper alloy electrode by using an electric spark process to obtain a high-entropy alloy wear-resistant layer with high electrical conductivity and thermal conductivity and metallurgical bonding, so as to avoid the electrode and the aluminum alloy to be welded from forming alloys at the contact point during the resistance spot welding process and causing the electrode and the welded material to adhere together, thereby improving the wear resistance of the end surface of the resistance spot welding electrode. In the present invention, the body material of the resistance spot welding electrode is a copper alloy material, specifically a copper-chromium alloy, a tungsten-copper alloy or a tungsten-molybdenum-copper alloy, and the high entropy alloy material is deposited by electric spark to obtain a high entropy alloy wear-resistant layer with metallurgical bonding on the end surface of the copper alloy electrode. The high entropy alloy is composed of at least five elements, with an atomic ratio of 1:1 or approximately 1:1, and the composition of each element is between 5% and 35%. The high entropy alloy is not easy to form a brittle intermetallic compound, but instead forms a body-centered cubic phase, a face-centered cubic phase, a nanostructure or even an amorphous structure with a simple crystal structure. There are 37 main elements of high entropy alloys, which are composed of at least five elements mixed in equal or approximately equal proportions. Studies have shown that more than 480 high entropy alloy systems can be formed. There are many types of high entropy alloys. The high entropy effect is the main factor in regulating its microstructure and structure. The number of alloying elements and processing conditions have a significant impact on its microstructure. The difference in high entropy alloy structure presents different structural properties and functional characteristics. The preparation technology of high entropy alloy coatings includes thermal spraying, sputtering and laser cladding. The high entropy alloy composition used in the present invention needs to consider the conductivity, thermal conductivity and affinity of the elements to aluminum. As a structural and functional part, the resistance spot welding electrode is required to withstand high temperature and high pressure, that is, the dual effects of heat and force coupling. The high entropy alloy wear-resistant layer obtained on the end surface of the copper alloy electrode is also required to have a certain bonding strength with the body. The present invention designs the elements and types of the high entropy alloy system, and prepares a high entropy alloy material with performance suitable for resistance spot welding electrodes by selecting reasonable components and production methods.
[0034] Specifically, the method for improving the wear resistance of the end surface of the aluminum alloy resistance spot welding electrode of the present invention comprises the following steps:
[0035] The first step is to prepare high entropy alloy powder. According to the designed high entropy alloy system and composition, the powder is mixed evenly and vacuum ball milled to obtain high entropy alloy powder.
[0036] First, the type of high entropy alloy elements is designed: In the present invention, a hexavalent system is used, specifically, a high entropy alloy is composed of any six elements of copper, tungsten, molybdenum, zirconium, niobium, vanadium, chromium, nickel and iron, and the six elements have the same mole fraction. The purity of the metals used is greater than 99.9%, and the particle size of the metal powder is 15-40μm. The high entropy alloy element composition is 16.6% in terms of atomic percentage (at%). An electronic balance with an accuracy of 0.0001g is used to accurately weigh six metal powders in a molar ratio and put them into a ball mill. Three zirconium oxide ball milling beads with diameters of 10mm, 5mm and 3mm are used, and the weight ratio is 5:2:4. The powders are mixed evenly and vacuum ball milled, with a ball-to-material ratio of 12:1, a ball milling speed of 350r / min, and a ball milling time of 15-20h to obtain a high entropy alloy powder.
[0037] The second step is to prepare high entropy alloy rods and use arc heating to obtain basic alloy ingots with uniform composition.
[0038] The high entropy alloy powder mixed in the first step is melted in a vacuum arc melting furnace and evacuated to Pa, argon is filled as a protective gas, and arc heating is used to repeatedly melt for 9 times to obtain a basic alloy ingot with uniform composition. In the present invention, the current for arc melting the high entropy alloy powder is 300-400A.
[0039] The third step is mechanical processing.
[0040] The end surface of the copper alloy electrode body 2 is mechanically treated to remove surface oxides and various oil stains.
[0041] The fourth step is electrospark deposition.
[0042] The prepared high entropy alloy rod is uniformly coated on the end face of the pretreated copper alloy electrode body 2 by an electrospark deposition process to form a high entropy alloy coating with a thickness of 150-520 μm, that is, a high entropy alloy wear-resistant layer 1. The electrospark deposition process parameters obtained by optimization are: voltage 65-83V, frequency 210-252Hz, and the interface forms a dense metallurgical bond.
[0043] Step 5: End surface finishing.
[0044] The end surface of the copper alloy electrode is processed by a mechanical processing method to obtain a geometric structure size that meets the resistance spot welding electrode.
[0045] like Figure 2As shown, the resistance spot welding electrode prepared by the method for improving the wear resistance of the end face of the aluminum alloy resistance spot welding electrode of the present invention comprises a copper alloy electrode body 2, and the end face of the copper alloy electrode body 2 is coated and deposited with a layer of high entropy alloy wear-resistant layer 1 with metallurgical bonding by an electric spark process to avoid alloying and adhesion between the end face of the electrode and the material to be welded at the contact surface. The thickness of the high entropy alloy wear-resistant layer 1 is 150-520 μm.
[0046] All the following embodiments are obtained by using the above-mentioned high entropy alloy coating composition, process steps and parameters.
[0047] Embodiment 1: A method for improving the wear resistance of an aluminum alloy resistance spot welding electrode end surface, comprising the following steps:
[0048] The first step is to prepare high entropy alloy powder. The high entropy alloy is composed of copper, tungsten, molybdenum, zirconium, niobium and vanadium elements in a molar ratio of 1:1:1:1:1:1, and the chemical formula is CuWMoZrNbV. The composition is calculated by atomic percentage (at%): copper (Cu) 16.6%, tungsten (W) 16.6%, molybdenum (Mo) 16.6%, zirconium (Zr), niobium (Nb) 16.6%, and vanadium (V) 16.6%. The purity of the above six metals is greater than 99.9%, and the particle size of the metal powder is 15-40μm. An electronic balance with an accuracy of 0.0001g is used to accurately weigh the six metal powders in molar proportions and put them into a ball mill. Three zirconium oxide ball mills with diameters of 10mm, 5mm and 3mm are used, and the weight ratio is 5:2:4. The powders were mixed evenly and vacuum ball-milled with a ball-to-material ratio of 12:1, a ball-milling speed of 350 r / min, and a ball-milling time of 15-20 h to obtain high entropy alloy powder.
[0049] The second step is to prepare a high entropy alloy rod. The high entropy alloy powder mixed in the first step is melted in a vacuum arc melting furnace and evacuated to Pa, argon gas is filled as a protective gas, and arc heating is used to repeatedly melt for 9 times to obtain a basic alloy ingot with uniform composition. In this embodiment, the current for arc melting the high entropy alloy powder is 300-400A.
[0050] The third step is mechanical treatment: the end surface of the copper alloy electrode body 2 is mechanically treated to remove surface oxides and various oil stains.
[0051] The fourth step is electrospark deposition. The prepared high entropy alloy rod is uniformly coated on the end surface of the pretreated copper alloy electrode body 2 by electrospark deposition process to form a high entropy alloy coating with a thickness of 150-520 μm, that is, a high entropy alloy wear-resistant layer 1. In this embodiment, the electrospark deposition process parameters are: voltage 65-83V, frequency 210-252Hz, and the interface forms a dense metallurgical bond.
[0052] The fifth step is end surface finishing. The end surface of the copper alloy electrode is processed by mechanical processing to obtain the geometric structure size that meets the resistance spot welding electrode.
[0053] Embodiment 2: A method for improving the wear resistance of an aluminum alloy resistance spot welding electrode end surface, comprising the following steps:
[0054] The first step is to prepare high entropy alloy powder. The high entropy alloy is composed of copper, tungsten, zirconium, niobium, vanadium and chromium elements with a molar ratio of 1:1:1:1:1:1, and the chemical formula is CuWZrNbVCr. The composition is 16.6% in terms of atomic percentage (at%). The purity of the above six metals is greater than 99.9%, and the particle size of the metal powder is 15-40μm. An electronic balance with an accuracy of 0.0001g is used to accurately weigh the six metal powders in molar proportions and put them into a ball mill. Three zirconium oxide ball milling beads with diameters of 10mm, 5mm and 3mm are used, and the weight ratio is 5:2:4. The powders are mixed evenly and vacuum ball milled, with a ball-to-material ratio of 12:1, a ball milling speed of 350r / min, and a ball milling time of 15-20h to obtain high entropy alloy powder.
[0055] The second step is to prepare a high entropy alloy rod. The high entropy alloy powder mixed in the first step is melted in a vacuum arc melting furnace and evacuated to Pa, argon gas is filled as a protective gas, and arc heating is used to repeatedly melt for 9 times to obtain a basic alloy ingot with uniform composition. In this embodiment, the current for arc melting the high entropy alloy powder is 300-400A.
[0056] The third step is mechanical treatment: the end surface of the copper alloy electrode body 2 is mechanically treated to remove surface oxides and various oil stains.
[0057] The fourth step is electrospark deposition. The prepared high entropy alloy rod is uniformly coated on the end surface of the pretreated copper alloy electrode body 2 by electrospark deposition process to form a high entropy alloy coating with a thickness of 150-520 μm, that is, a high entropy alloy wear-resistant layer 1. In this embodiment, the electrospark deposition process parameters are: voltage 65-83V, frequency 210-252Hz, and the interface forms a dense metallurgical bond.
[0058] The fifth step is end surface finishing. The end surface of the copper alloy electrode is processed by mechanical processing to obtain the geometric structure size that meets the resistance spot welding electrode.
[0059] Embodiment 3: A method for improving the wear resistance of an aluminum alloy resistance spot welding electrode end surface, comprising the following steps:
[0060] The first step is to prepare high entropy alloy powder. The high entropy alloy is composed of copper, tungsten, molybdenum, niobium, vanadium and chromium elements with a molar ratio of 1:1:1:1:1:1, and the chemical formula is CuWMoNbVCr. The composition is 16.6% in terms of atomic percentage (at%). The purity of the above six metals is greater than 99.9%, and the particle size of the metal powder is 15-40μm. An electronic balance with an accuracy of 0.0001g is used to accurately weigh the six metal powders in molar proportion and put them into a ball mill. Three zirconium oxide ball milling beads with diameters of 10mm, 5mm and 3mm are used, and the weight ratio is 5:2:4. The powders are mixed evenly and vacuum ball milled, with a ball-to-material ratio of 12:1, a ball milling speed of 350r / min, and a ball milling time of 15-20h to obtain high entropy alloy powder.
[0061] The second step is to prepare a high entropy alloy rod. The high entropy alloy powder mixed in the first step is melted in a vacuum arc melting furnace and evacuated to Pa, argon gas is filled as a protective gas, and arc heating is used to repeatedly melt for 9 times to obtain a basic alloy ingot with uniform composition. In this embodiment, the current for arc melting the high entropy alloy powder is 300-400A.
[0062] The third step is mechanical treatment: the end surface of the copper alloy electrode body 2 is mechanically treated to remove surface oxides and various oil stains.
[0063] The fourth step is electrospark deposition. The prepared high entropy alloy rod is uniformly coated on the end surface of the pretreated copper alloy electrode body 2 by electrospark deposition process to form a high entropy alloy coating with a thickness of 150-520 μm, that is, a high entropy alloy wear-resistant layer 1. In this embodiment, the electrospark deposition process parameters are: voltage 65-83V, frequency 210-252Hz, and the interface forms a dense metallurgical bond.
[0064] The fifth step is end surface finishing. The end surface of the copper alloy electrode is processed by mechanical processing to obtain the geometric structure size that meets the resistance spot welding electrode.
[0065] Embodiment 4: A method for improving the wear resistance of an aluminum alloy resistance spot welding electrode end surface, comprising the following steps:
[0066] The first step is to prepare high entropy alloy powder. The high entropy alloy is composed of copper, tungsten, molybdenum, zirconium, chromium and nickel elements with a molar ratio of 1:1:1:1:1:1, and the chemical formula is CuWMoZrCrNi. The composition is 16.6% in terms of atomic percentage (at%). The purity of the above six metals is greater than 99.9%, and the particle size of the metal powder is 15-40μm. An electronic balance with an accuracy of 0.0001g is used to accurately weigh the six metal powders in molar proportions and put them into a ball mill. Three zirconium oxide ball milling beads with diameters of 10mm, 5mm and 3mm are used, and the weight ratio is 5:2:4. The powders are mixed evenly and vacuum ball milled, with a ball-to-material ratio of 12:1, a ball milling speed of 350r / min, and a ball milling time of 15-20h to obtain high entropy alloy powder.
[0067] The second step is to prepare a high entropy alloy rod. The high entropy alloy powder mixed in the first step is melted in a vacuum arc melting furnace and evacuated to Pa, argon gas is filled as a protective gas, and arc heating is used to repeatedly melt for 9 times to obtain a basic alloy ingot with uniform composition. In this embodiment, the current for arc melting the high entropy alloy powder is 300-400A.
[0068] The third step is mechanical treatment: the end surface of the copper alloy electrode body 2 is mechanically treated to remove surface oxides and various oil stains.
[0069] The fourth step is electrospark deposition. The prepared high entropy alloy rod is uniformly coated on the pretreated copper alloy electrode end surface by electrospark deposition process to form a high entropy alloy coating with a thickness of 150-520 μm, that is, a high entropy alloy wear-resistant layer 1. In this embodiment, the electrospark deposition process parameters are: voltage 65-83V, frequency 210-252Hz, and the interface forms a dense metallurgical bond.
[0070] Step 5: Finishing the end surface: The end surface of the copper alloy electrode body 2 is processed by mechanical processing to obtain a geometric structure size that meets the requirements of the resistance spot welding electrode.
[0071] Embodiment 5: A method for improving the wear resistance of an aluminum alloy resistance spot welding electrode end surface, comprising the following steps:
[0072] The first step is to prepare high entropy alloy powder. The high entropy alloy is composed of copper, tungsten, molybdenum, chromium, nickel and iron elements with a molar ratio of 1:1:1:1:1:1, and the chemical formula is CuWMoCrNiFe. The composition is 16.6% in terms of atomic percentage (at%). The purity of the above six metals is greater than 99.9%, and the particle size of the metal powder is 15-40μm. An electronic balance with an accuracy of 0.0001g is used to accurately weigh the six metal powders in molar proportion and put them into a ball mill. Three zirconium oxide ball milling beads with diameters of 10mm, 5mm and 3mm are used, and the weight ratio is 5:2:4. The powders are mixed evenly and vacuum ball milled, with a ball-to-material ratio of 12:1, a ball milling speed of 350r / min, and a ball milling time of 15-20h to obtain high entropy alloy powder.
[0073] The second step is to prepare a high entropy alloy rod. The high entropy alloy powder mixed in the first step is melted in a vacuum arc melting furnace and evacuated to Pa, argon gas is filled as a protective gas, and arc heating is used to repeatedly melt for 9 times to obtain a basic alloy ingot with uniform composition. In this embodiment, the current for arc melting the high entropy alloy powder is 300-400A.
[0074] The third step is mechanical treatment: the end surface of the copper alloy electrode body 2 is mechanically treated to remove surface oxides and various oil stains.
[0075] The fourth step is electrospark deposition. The prepared high entropy alloy rod is uniformly coated on the pretreated copper alloy electrode end surface by electrospark deposition process to form a high entropy alloy coating with a thickness of 150-520 μm, that is, a high entropy alloy wear-resistant layer 1. In this embodiment, the electrospark deposition process parameters are: voltage 65-83V, frequency 210-252Hz, and the interface forms a dense metallurgical bond.
[0076] Step 5: Finishing the end surface: The end surface of the copper alloy electrode body 2 is processed by mechanical processing to obtain a geometric structure size that meets the requirements of the resistance spot welding electrode.
[0077] The high entropy alloy composition and wear-resistant layer properties of the aluminum alloy resistance spot welding electrode end surface are shown in Table 1.
[0078] Table 1 Composition and performance index of high entropy alloy
[0079] As shown in Table 1, the resistance spot welding electrode prepared by the present invention according to the above process steps and ingredients has a resistivity of 5.2-15.5μΩ.cm of the high entropy alloy wear-resistant layer, which has good electrical conductivity; the thermal conductivity of the high entropy alloy wear-resistant layer is 130.8--164.3w / m﹒k, which has good thermal conductivity; the relative wear resistance of the high entropy alloy wear-resistant layer is 1.5-1.8 times that of the tungsten copper alloy electrode substrate. The method uses an electric spark process to deposit a layer of metallurgically bonded high entropy alloy wear-resistant layer on the end face of the copper alloy electrode, and avoids alloying and adhesion between the end face of the electrode and the material to be welded at the contact surface without reducing the electrical conductivity, thermal conductivity and high-temperature mechanical properties of the copper alloy electrode material. Under the same test conditions, the wear resistance of the end face of the resistance spot welding electrode can be effectively improved.
[0080] Note that the above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments described herein, and that various obvious changes, readjustments and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.
Claims
1. A method for improving the wear resistance of the copper alloy electrode end surface used in aluminum alloy resistance spot welding, characterized in that: The following steps are involved: A. Preparation of high entropy alloy powder: The high entropy alloy powder is prepared by mixing and vacuum ball milling any six metal powders of copper powder, tungsten powder, molybdenum powder, zirconium powder, niobium powder, vanadium powder, chromium powder, nickel powder and iron powder, the six metal elements have the same molar fraction, and the molar ratio is fixed at 1:1:1:1:1:1; the purity of the metals used is greater than 99.9%, and the particle size of the metal powder is 15-40μm; The ball milling process is as follows: six kinds of metal powders are accurately weighed in molar proportion and put into a ball milling jar, three kinds of zirconium oxide ball milling beads with diameters of 10 mm, 5 mm and 3 mm are used, the weight ratio is 5:2:4, the ball-to-material ratio is 12:1, the ball milling speed is 350 r / min, and the ball milling time is 15-20 h; B. Preparation of high entropy alloy rods: The high entropy alloy powder obtained in step A was melted in a vacuum arc melting furnace and evacuated to 6×10 -3 Pa, argon is filled as a protective gas, and arc heating is used to repeatedly melt for 9 times to obtain a basic alloy ingot with uniform composition; the current for arc melting high entropy alloy powder is 300-400A; C. Mechanically treating the end surface of the copper alloy electrode body (2) to remove surface oxides and various oil stains; the thickness of the high entropy alloy coating is 150-520 μm; D. Electrospark deposition: The prepared high entropy alloy rod is uniformly coated on the end surface of the pretreated copper alloy electrode body (2) by an electrospark deposition process to form a high entropy alloy wear-resistant layer (1); the electrospark deposition process parameters are: voltage 65-83V, frequency 210-252Hz, and the interface forms a dense metallurgical bond; E. End face finishing: The end face of the copper alloy electrode is processed by mechanical processing methods to obtain the geometric structure dimensions that meet the resistance spot welding electrode.
2. The copper alloy electrode for resistance spot welding prepared by the method for improving the wear resistance of the end surface of the copper alloy electrode for aluminum alloy resistance spot welding according to claim 1 is characterized in that: It comprises a copper alloy electrode body (2), the end surface of which is coated with a layer of a high entropy alloy wear-resistant layer (1) with metallurgical bonding and deposited by an electric spark process, wherein the thickness of the high entropy alloy wear-resistant layer (1) is 150-520 μm.
Citation Information
Patent Citations
Preparation method of high-entropy AlCoNiCrFeMo alloy coating
CN103757631A
Six-element or more-element eutectic high-entropy alloy and preparation method thereof
CN116240439A
Electrode for spot welding
US5334814A