A kind of nano nickel and preparation method thereof
By adding 1,4-butynediol and pre-plating treatment to the electrodeposition method to reduce the current density, nano-nickel with high hardness and high thermal stability was successfully prepared, solving the problems of high current density and fine grain size in the existing technology. Solve the problem of chemical difficulty and realize the excellent mechanical properties and industrial application potential of nano-nickel.
Patent Information
- Application Number
- CN202410971234.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The current density for preparing nano-nickel in the existing technology is relatively large, which leads to increased energy consumption and industrialization costs. At the same time, it is difficult to refine the grain size of nano-nickel to less than 10 nm, which affects its mechanical properties.
Using the DC electrodeposition method, by adding 1,4-butynediol as an additive to the plating solution, reducing the current density to 1~5mA/cm², combined with pre-plating treatment and pickling activation, a grain size of 5-10nm was prepared. of nano-nickel.
Nano-nickel with a grain size less than 10nm was successfully prepared at low current density, which significantly improved its hardness and thermal stability. The hardness can reach 9.32GPa and the yield strength is as high as 4GPa. It is suitable for ultra-hard surface coatings and high-temperature applications.
Smart Images

Figure CN118497831B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of nanocrystalline metal materials, and in particular relates to nano nickel and a preparation method thereof. Background Art
[0002] Nanocrystalline materials refer to materials whose structural unit scale is at the nanometer level (i.e., less than 100nm) in at least one dimension. Since the grain size of nanocrystalline materials is extremely small, the proportion of atoms at the interface in the material increases significantly, and the influence of grain boundaries on the mechanical properties and physical and chemical properties of the material cannot be ignored. When the grain size is reduced to a certain extent, the macroscopic properties of the material will be dominated by the grain boundaries, and the material will show a new structure-performance law, and the macroscopic performance is different from the traditional coarse-grained materials. Excellent properties, such as high strength, low-temperature plasticity, friction and wear resistance, electromagnetic properties, etc. Thanks to these excellent properties, nanocrystalline materials have been used in many fields such as electronic information, aerospace, energy, transportation, and military.
[0003] Electrodeposition is the most widely used and also one of the earliest methods for preparing nanocrystalline materials. The principle of electrodeposition is to use an electrolytic cell, that is, when an external current passes through, an oxidation reaction occurs on the surface of the anode plated material to produce metal cations, which move in a directional manner toward the cathode plated part under the action of the electric field, and then a reduction reaction occurs on the surface of the plated part to deposit a layer of nanocrystalline coating. This process is repeated continuously to form a bulk nanocrystalline material.
[0004] In the prior art, by adding W alloy, Ni grains are refined to 10nm or less, and tungsten-nickel alloys with excellent properties such as high hardness and high wear resistance are obtained. They are widely used in machinery, electronics, medical equipment, automotive parts, aerospace and military industries, daily hardware parts, industrial work molds, etc. However, due to the common defects of rough coating, uneven composition, pitting, etc. in the electroplating process of tungsten-nickel alloys, these defects affect the performance during service, thus seriously restricting its application development. Therefore, further refining pure Ni to make it have high strength, high hardness and high surface quality is the key to promoting the application of electrodeposited Ni. At present, many scholars have improved the conventional coarse-grained nickel plating process to prepare nano-nickel and studied its structure and properties, but there are still two limitations: (1) The nano-nickel grain size range prepared by this method is limited, and it is difficult to prepare small-sized nano-nickel below 10nm; (2) The current density required for preparing nano-nickel by this method is relatively high. The current density range of the traditional Watt-type bright nickel plating system is 100-250mA / cm². If the grain size of the coating is reduced to the nanoscale, a current density of more than 100mA / cm² is required. In order to obtain a coating with an average grain size of 30nm, the current density needs to be increased to more than 250mA / cm², which greatly increases energy consumption and increases industrial costs. At the same time, the nano-nickel coating prepared based on high current density has higher internal stress, which affects the strength of the nano-nickel and the quality of the coating. Summary of the invention
[0005] Therefore, the present invention provides a nano nickel and a preparation method thereof, the purpose of which is to obtain small-sized nano nickel with excellent mechanical properties at a lower current density.
[0006] The present invention provides a method for preparing nano nickel, comprising the following steps:
[0007] Preparation of plating solution: dissolving nickel sulfate hexahydrate NiSO4·6H2O, nickel chloride hexahydrate NiCl2·6H2O, boric acid H3BO3 and sodium dodecyl sulfate in deionized water, stirring and dissolving, and filtering with filter paper; then adding additives of saccharin sodium and 1,4-butynediol to the filtrate to obtain the plating solution;
[0008] Electrodeposition: The nano nickel is prepared by direct current electrodeposition;
[0009] The process parameters of the DC electrodeposition are as follows: the current density is 1-5 mA / cm 2 .
[0010] Furthermore, in the plating solution preparation step, the concentrations of nickel sulfate hexahydrate NiSO4·6H2O, nickel chloride hexahydrate NiCl2·6H2O, boric acid H3BO3 and sodium dodecyl sulfate are 100-300 g / L, 20-50 g / L, 20-50 g / L and 0.05-0.2 g / L respectively; the concentrations of saccharin sodium and 1,4-butynediol are 3-6 g / L and 0.5-1 g / L respectively.
[0011] Furthermore, the pH range of the plating solution is 4-6.
[0012] Furthermore, in the plating solution preparation step, a pre-plating treatment is performed in the filtrate after filtering with filter paper, and then an additive is added to the filtrate after the pre-plating treatment;
[0013] The pre-plating treatment time is 20-30 hours.
[0014] Furthermore, in the electroplating step, the temperature of the plating solution is 30-60°C.
[0015] Furthermore, in the electrodeposition step, the anode is a nickel plate with a purity of 99.6%, and the cathode is a nickel sheet with a grain size of 10-40 μm.
[0016] Furthermore, before the electrodeposition, the nickel sheet is sequentially ground, polished and surface degreased, and pickled in a mixed solution of sulfuric acid and hydrochloric acid, followed by electrolytic polishing activation;
[0017] Preferably, the nickel sheet is mechanically polished using 400#, 1000# and 2000# sandpaper in sequence, and surface activated using an electrolytic polishing method to increase the possibility of deposition at a low current density.
[0018] The nano nickel and the preparation method thereof provided by the present invention have the following beneficial effects:
[0019] 1. The present invention adds 1,4-butynediol as an additive during the electro-deposition process, and by reducing the current density, nano nickel with a grain size of 5-10nm can be obtained. Since electrochemical deposition itself is a process of rapidly cooling and solidifying the cathode electro-crystallization droplets through chemical reactions, 1,4-butynediol has an adsorption effect, which can disperse the droplets, block epitaxial growth, and refine the grains; under extremely low current density, it can ensure that each electro-crystallization droplet is completely solidified, 1,4-butynediol is adsorbed on a new site, and a new round of discharge and crystallization process is carried out again, which is more conducive to the role of 1,4-butynediol, further refines the grains, and obtains a bulk nano nickel with a thickness of hundreds of microns, uniform grain size less than 10nm, and a minimum size of 5nm; the method of the present application breaks through the current limit of the minimum grain size of nano Ni preparation. On the other hand, this uniform, block-like, extremely hard, extremely small grain size pure Ni structure is currently unattainable by pure nickel materials prepared by other methods.
[0020] 2. The nano Ni with extremely small grain size prepared by the method of the present invention has a Vickers hardness of up to 9.32 GPa at room temperature, which is the highest hardness structure in pure Ni at present. The hardness of Ni-W alloy with the same grain size is only about 5.3 GPa, and the highest hardness of Ni-W alloy is about 7 GPa. Therefore, the pure Ni material with high strength, high hardness and good plasticity can replace most of the current application fields of Ni-W alloy.
[0021] 3. The nano-Ni with extremely small grain size obtained by the method of the present invention also has very excellent thermal stability. After annealing at 450°C, the grain size remains below 10nm, which is higher than the application temperature of most coatings and micro-electromechanical systems (MEMS). In contrast, the grain coarsening temperature of Ni deposited by traditional methods is only about 200°C. Therefore, the nano-nickel prepared in this application significantly increases the use temperature of the material, laying the foundation for its industrial application.
[0022] 4. The yield strength of the nano-Ni with extremely small grain size obtained by the method of the present invention can be as high as 4 GPa, and it is still uniformly deformed when the compression strain reaches 60%, and has extremely excellent plastic deformation ability.
[0023] 5. The yield strength of the nano-Ni with extremely small grain size obtained by the method of the present invention can be as high as 4 GPa, and it is still uniformly deformed when the compression strain reaches 60%, and has extremely excellent plastic deformation ability.
[0024] 6. The nanocrystalline Ni structure prepared by the method of the present application exhibits extremely high hardness and excellent mechanical properties, and has industrial application prospects as a superhard surface coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0026] Figure 1 : Figures (a), (b), and (c) are respectively the macroscopic morphology, structural schematic diagram, and cross-sectional view of the nano-nickel sample prepared by electrodeposition in Example 1 of the present invention;
[0027] Figure 2 XRD curves and average grain sizes of the nano-nickel samples prepared in Examples 1-3 of the present invention;
[0028] Figure 3 Middle: Figures (a), (b), and (c) are respectively TEM dark field image, high resolution imaging, and grain size distribution of the sample with a grain size of 7 nm according to Example 1 of the present invention;
[0029] Figure 4 The Hall-Petch curves of the electrodeposited nano-nickel samples with different grain sizes in Examples 1-3 of the present invention;
[0030] Figure 5 The in-situ compression curves of the electrodeposited nano-nickel samples with different grain sizes in Examples 1-3 of the present invention;
[0031] Figure 6 This is the tensile curve of the electrodeposited nano-nickel sample of Example 1 of the present invention;
[0032] Figure 7 This is a TEM dark field image of the nano-nickel in Example 1 of the present invention after isothermal annealing at 450° C. for 1 hour. DETAILED DESCRIPTION
[0033] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0034] The present invention adopts direct current electrodeposition method to prepare a block of extremely small grains of nanocrystalline pure nickel with a thickness of hundreds of microns and uniformity. The specific scheme is as follows:
[0035] The present invention provides a method for preparing nano nickel, comprising the following steps:
[0036] Preparation of plating solution: dissolve nickel sulfate hexahydrate NiSO4·6H2O, nickel chloride hexahydrate NiCl2·6H2O, boric acid H3BO3 and sodium dodecyl sulfate in deionized water, stir and dissolve, and then filter with filter paper; then add additives of saccharin sodium and 1,4-butynediol to the filtrate to obtain a plating solution;
[0037] Electrodeposition: Nano nickel is prepared by direct current electrodeposition;
[0038] The process parameters of DC electrodeposition are: current density is 1~5mA / cm 2 .
[0039] In some embodiments, in the plating solution preparation step, the concentrations of nickel sulfate hexahydrate NiSO4·6H2O, nickel chloride hexahydrate NiCl2·6H2O, boric acid H3BO3 and sodium dodecyl sulfate are 100-300 g / L, 20-50 g / L, 20-50 g / L and 0.05-0.2 g / L, respectively; the concentrations of saccharin sodium and 1,4-butynediol are 3-7 g / L and 0.5-1 / L, respectively.
[0040] In some embodiments, the pH of the plating solution is in the range of 4-6.
[0041] In some embodiments, in the plating solution preparation step, a pre-plating treatment is performed in the filtrate after filtering with filter paper, and then an additive is added to the filtrate after the pre-plating treatment; wherein the pre-plating treatment time is 20-30 hours, and the current density of the pre-plating treatment is 1-5 mA / cm 2 The above chemical reagents are all of analytical grade. The impurity ions in the chemical reagents can be removed by pre-plating treatment, and then nano-pure nickel can be obtained by subsequent electrodeposition.
[0042] In some embodiments, during the electrodeposition step, the temperature of the plating solution is 30-60°C.
[0043] In some embodiments, in the electrodeposition step, the anode is a nickel plate with a purity of 99.6%, and the cathode is a nickel sheet with a grain size of 10-40 μm.
[0044] In some embodiments, before electrodeposition, the nickel sheet is sequentially ground, polished, and surface degreased, and pickled in a mixed solution of sulfuric acid and hydrochloric acid, and then electrolytically polished and activated;
[0045] Preferably, 400#, 1000# and 2000# sandpaper are used in sequence to mechanically polish the nickel sheet. The purpose of polishing the substrate (i.e., the nickel sheet) is to remove the surface oxide layer and macroscopic defects such as burrs and scratches, so that the substrate surface is flat and smooth, and the quality of the coating is improved; the purpose of pickling the substrate surface is to further remove the substrate surface oxide layer, obtain a fresh metal surface, improve the bonding strength of the coating, and ensure the electrodeposition effect. In the implementation of this method, 5% sulfuric acid + 1% hydrochloric acid is used to pickle the substrate surface. After pickling, the substrate nickel is electrolytically polished to activate its surface, and then placed in clean water, and immediately placed in an electrodeposition solution for electrodeposition.
[0046] Based on the above method, the additive 1,4-butynediol is added during the electro-deposition process, and by reducing the current density, nano-pure nickel with a grain size of 5-30nm can be obtained. Since electrochemical deposition itself is a process of rapidly cooling and solidifying the cathode electro-crystallization droplets through chemical reactions, 1,4-butynediol has an adsorptive effect, which can disperse the droplets, block epitaxial growth, and refine the grains; at extremely low current densities, it can ensure that each electro-crystallization droplet is completely solidified, 1,4-butynediol is adsorbed on a new site, and a new round of discharge and crystallization process is carried out again, which is more conducive to the role of 1,4-butynediol, further refines the grains, and improves the hardness of nano-nickel.
[0047] By reducing the current density during the electrodeposition process, the current density is reduced by more than 60% compared with the existing electrodeposition nanocrystalline metal nickel process, and a bulk nano-nickel with a thickness of hundreds of microns, uniformity and a grain size of less than 10nm can be prepared; the nano-nickel coating is bright and flat, with uniform thickness and excellent mechanical properties, breaking through the inverse Hall-Petch relationship when the grain size of traditional Ni alloy is reduced to less than 10nm. At room temperature, the Vickers hardness can reach 9.32GPa, which is the hardest structure in pure Ni at present, 6 times that of traditional electrodeposited coarse-grained nickel, and more than twice the hardness of ordinary electrodeposited nanocrystalline Ni; the hardness of Ni-W alloy with the same grain size is only about 5.3GPa, so the nanocrystalline Ni structure prepared by the method of the present application shows extremely high hardness and can be used as an ultra-hard surface coating; Ni with extremely small grain size (grain size less than 10nm) also shows very excellent thermal stability. After annealing at 450°C, the grain size is still maintained below 10nm, which is higher than the application temperature of most coatings and MEMS. In contrast, the grain coarsening temperature of Ni deposited by the traditional method is only about 200° C. Therefore, the nano nickel prepared by the method of the present application significantly increases the use temperature of the material and can be used as a stable protective coating for metals such as steel, Cu and their alloys used in industry.
[0048] On the other hand, the present invention also provides a nano nickel, the thickness of the nano nickel is 100-200 microns; the grain size of the nano nickel is 5-10nm;
[0049] Preferably, the nano nickel is obtained by any of the above preparation methods.
[0050] In some embodiments, the hardness of the nano-nickel is 7.02-9.32 GPa.
[0051] In some embodiments, the grain coarsening temperature of the nano-nickel exceeds 250-450°C.
[0052] The present invention is further described below in conjunction with specific embodiments.
[0053] Example 1
[0054] This embodiment provides a method for preparing nano nickel, which specifically comprises the following steps:
[0055] Preparation of plating solution: 300g / L NiSO4·6H2O, 50g / L NiCl2·6H2O, 50g / L H3BO3 and 0.05g / L sodium dodecyl sulfate were dissolved in deionized water, stirred on a magnetic stirring heating table, and the temperature was controlled to 30±1℃. After stirring and dissolving, the solution was filtered with filter paper. The filtrate after filtering with filter paper was pre-plated for 30 hours, with a pure nickel plate as the anode and a coarse-grained nickel sheet as the cathode, and the current density was 50mA / cm². Then, 6g / L saccharin sodium and 0.6g / L 1,4-butynediol were added to the filtrate after pre-plating to obtain a plating solution. A peristaltic pump was used to add 1g / L 1,4-butynediol at a rate of 200uL / min to control the concentration of additives to remain constant during the electrodeposition process.
[0056] Electrodeposition: Nano-nickel was prepared by direct current electrodeposition. The process parameters of direct current electrodeposition were as follows: pure nickel plate was used as sacrificial anode, coarse-grained nickel sheet with a grain size of 40 μm was used as cathode, the current density was continuously controlled to be constant at 1 mA / cm² by a computer program, and the deposition time was 336 h.
[0057] The macroscopic picture and model diagram of the nano nickel material prepared in this embodiment are as follows: Figure 1 As shown in the figure, it can be seen that the thickness of the nano-nickel sample is about 150μm, which is consistent with the uniform bulk sample. The sample surface is bright and has high flatness; Figure 2 It can be seen from the X-ray diffraction pattern of the nano-nickel material of this embodiment that the nano-nickel material has a random orientation distribution, and the grain size calculated based on the half-width height of the (111) peak of the X-ray diffraction pattern is 5 nm; Figure 4 For the microhardness test, it can be seen that the nano nickel material of this embodiment has an ultra-high hardness (9.52GPa); Figure 5This is the in-situ compression result of the nano-nickel material of this embodiment at room temperature. It can be seen that its compressive yield strength is as high as 4 GPa, which is the pure Ni material with the highest strength at present. Figure 6 This is the tensile result of the nano-nickel material of this embodiment at room temperature. It can be seen that the tensile strength can reach 3 GPa, which is the pure Ni material with the highest strength at present.
[0058] Figure 7 After the nano-nickel material of this embodiment was annealed at 450° C., transmission electron microscopy was used to observe that the grain size of the dark field image was still less than 10 nm, indicating that the nano-crystals did not grow.
[0059] Example 2
[0060] This embodiment provides a method for preparing nano nickel, which specifically comprises the following steps:
[0061] Preparation of plating solution: 300g / L NiSO4·6H2O, 45g / L NiCl2·6H2O, 40g / L H3BO3 and 0.1g / L sodium dodecyl sulfate were dissolved in deionized water, stirred on a magnetic stirring heating table, and the temperature was controlled to 35±1℃. After stirring and dissolving, the solution was filtered with filter paper; the filtrate after filtering with filter paper was pre-plated for 24 hours, with a pure nickel plate as the anode and a coarse-grained nickel sheet as the cathode, and the current density was 50mA / cm²; then 6g / L saccharin sodium and 0.6g / L 1,4-butynediol were added to the filtrate after pre-plating to obtain a plating solution; and a peristaltic pump was used to add 1g / L 1,4-butynediol at a rate of 200uL / min to control the concentration of additives to remain constant during the electrodeposition process;
[0062] Electrodeposition: Nano-nickel was prepared by direct current electrodeposition. The process parameters of direct current electrodeposition were as follows: pure nickel plate was used as sacrificial anode, coarse-grained nickel sheet with a grain size of 25 μm was used as cathode, the current density was continuously controlled to be constant at 2 mA / cm² by computer program, and the deposition time was 168 h.
[0063] from Figure 2 It can be seen that the average grain size of the nano-nickel sample prepared in this embodiment is 7nm, and the hardness of the sample is 8.14GPa ( Figure 4 as shown); Figure 3 As shown, the cross-sectional structure is characterized by dark field image (a) and high resolution image (b). The grain size statistics are performed based on the dark field image, and the grain size of the nano-nickel in this embodiment is 7 nm, which is consistent with the grain size calculated based on the (111) peak frame of the XRD curve, indicating the reliability of the XRD calculation data. Figure 5 This is the in-situ compression result of the nano-nickel material of this example at room temperature. It can be seen that its compressive yield strength is as high as 3 GPa.
[0064] Example 3
[0065] This embodiment provides a method for preparing nano nickel, which specifically comprises the following steps:
[0066] Preparation of plating solution: 300g / L NiSO4·6H2O, 45g / L NiCl2·6H2O, 40g / L H3BO3 and 0.1g / L sodium dodecyl sulfate were dissolved in deionized water, stirred on a magnetic stirring heating table, and the temperature was controlled to 35±1℃. After stirring and dissolving, the solution was filtered with filter paper; the filtrate after filtering with filter paper was pre-plated for 24 hours, with a pure nickel plate as the anode and a coarse-grained nickel sheet as the cathode, and the current density was 50mA / cm²; then 6g / L saccharin sodium and 0.6g / L 1,4-butynediol were added to the filtrate after pre-plating to obtain a plating solution; and a peristaltic pump was used to add 1g / L 1,4-butynediol at a rate of 200uL / min to control the concentration of additives to remain constant during the electrodeposition process;
[0067] Electrodeposition: Nano-nickel was prepared by direct current electrodeposition. The process parameters of direct current electrodeposition were as follows: pure nickel plate was used as sacrificial anode, coarse-grained nickel sheet with a grain size of 25 μm was used as cathode, the current density was continuously controlled to be constant at 5 mA / cm² by a computer program, and the deposition time was 60 h.
[0068] like Figure 2 As shown, the average grain size of the nano-nickel sample prepared in this embodiment is 10nm, and the hardness of the sample is 7.02GPa ( Figure 4 shown). Figure 5 This is the in-situ compression result of the nano-nickel material of this example at room temperature. It can be seen that its compressive yield strength is as high as 3 GPa.
[0069] Example 4
[0070] This embodiment provides a method for preparing nano nickel, which specifically comprises the following steps:
[0071] Preparation of plating solution: 100 g / L NiSO4·6H2O, 20 g / L NiCl2·6H2O, 20 g / L H3BO3 and 0.2 g / L sodium dodecyl sulfate were dissolved in deionized water, stirred on a magnetic stirring heating table, and the temperature was controlled to 60±1°C. After stirring and dissolving, the solution was filtered with filter paper; the filtrate after filtration with filter paper was pre-plated for 20 hours, with a pure nickel plate as the anode and a coarse-grained nickel sheet as the cathode, and the current density was 50 mA / cm²; then 3 g / L saccharin sodium and 0.5 g / L 1,4-butynediol were added to the filtrate after pre-plating to obtain a plating solution;
[0072] Electrodeposition: Nano-nickel was prepared by direct current electrodeposition. The process parameters of direct current electrodeposition were as follows: pure nickel plate was used as sacrificial anode, coarse-grained nickel sheet with a grain size of 10 μm was used as cathode, the current density was continuously controlled to be constant at 5 mA / cm² by a computer program, and the deposition time was 60 h.
[0073] The grain size of the nano nickel prepared in this embodiment is 9 nm.
[0074] Example 5
[0075] This embodiment provides a method for preparing nano nickel, which specifically comprises the following steps:
[0076] Preparation of plating solution: 200g / L NiSO4·6H2O, 35g / L NiCl2·6H2O, 35g / L H3BO3 and 0.1g / L sodium dodecyl sulfate were dissolved in deionized water, stirred on a magnetic stirring heating table, and the temperature was controlled to 45±1℃. After stirring and dissolving, the solution was filtered with filter paper; the filtrate after filtering with filter paper was pre-plated for 25 hours, with a pure nickel plate as the anode and a coarse-grained nickel sheet as the cathode, and the current density was 50mA / cm²; then 5g / L saccharin sodium and 0.4g / L 1,4-butynediol were added to the filtrate after pre-plating to obtain a plating solution; and a peristaltic pump was used to add 1g / L 1,4-butynediol at a rate of 200uL / min to control the concentration of additives to remain constant during the electrodeposition process;
[0077] Electrodeposition: Nano-nickel was prepared by direct current electrodeposition. The process parameters of direct current electrodeposition were as follows: pure nickel plate was used as sacrificial anode, coarse-grained nickel sheet with a grain size of 20 μm was used as cathode, the current density was continuously controlled to be constant at 3 mA / cm² by a computer program, and the deposition time was 160 h.
[0078] The grain size of the nano nickel prepared in this embodiment is 8 nm.
[0079] Comparative Example 1
[0080] This comparative example provides a method for preparing nano nickel, which specifically comprises the following steps:
[0081] Preparation of plating solution: 300g / L NiSO4·6H2O, 45g / L NiCl2·6H2O, 40g / L H3BO3 and 0.1g / L sodium dodecyl sulfate were dissolved in deionized water, stirred on a magnetic stirring heating table, and the temperature was controlled to 35±1℃. After stirring and dissolving, the solution was filtered with filter paper; the filtrate after filtering with filter paper was pre-plated for 24 hours, with a pure nickel plate as the anode and a coarse-grained nickel sheet as the cathode, and the current density was 50mA / cm²; then 6g / L saccharin sodium and 0.6g / L 1,4-butynediol were added to the filtrate after pre-plating to obtain a plating solution; and a peristaltic pump was used to add 1g / L 1,4-butynediol at a rate of 200uL / min to control the concentration of additives to remain constant during the electrodeposition process;
[0082] Electrodeposition: Nano-nickel was prepared by direct current electrodeposition. The process parameters of direct current electrodeposition were as follows: pure nickel plate was used as sacrificial anode, coarse-grained nickel sheet with a grain size of 25 μm was used as cathode, the current density was continuously controlled to be constant at 10 mA / cm² by a computer program, and the deposition time was 30 h.
[0083] The average grain size of the nano-nickel sample prepared in this comparative example is 30 nm, which is larger than that of the sample in Example 1, and the hardness of the sample is 4.89 GPa, which is lower than that of the sample in Example 1. This is because the current density in this comparative example is large and the current efficiency is low, resulting in relatively poor deposition quality.
[0084] Comparative Example 2
[0085] This comparative example provides a method for preparing nano nickel, which specifically comprises the following steps:
[0086] Preparation of plating solution: 300 g / L NiSO4·6H2O, 45 g / L NiCl2·6H2O, 40 g / L H3BO3 and 0.1 g / L sodium dodecyl sulfate were dissolved in deionized water, stirred on a magnetic stirring heating table, and the temperature was controlled to 35±1°C. After stirring and dissolving, the solution was filtered with filter paper. The filtrate after filtration with filter paper was pre-plated for 24 hours. The pre-plating process used a pure nickel plate as an anode and a coarse-grained nickel sheet as a cathode. The current density was 50 mA / cm 2 ; Then, 6 g / L of sodium saccharin and 0.2 g / L of 1,4-butynediol were added to the filtrate after the pre-plating treatment to obtain a plating solution; and 1 g / L of 1,4-butynediol was added at a rate of 200 uL / min using a peristaltic pump to control the concentration of the additive to remain constant during the electrodeposition process;
[0087] Electrodeposition: Nano-nickel was prepared by direct current electrodeposition. The process parameters of direct current electrodeposition were as follows: pure nickel plate was used as sacrificial anode, coarse-grained nickel sheet with a grain size of 25 μm was used as cathode, the current density was continuously controlled to be constant at 150 mA / cm² by a computer program, and the deposition time was 3 h.
[0088] The average grain size of the nano nickel sample prepared in this comparative example is 35nm, which is larger than the sample in Example 4, and the hardness of the sample is 3.8GPa, which is lower than the sample in Example 4. This is because the current density in this comparative example is large and the current efficiency is low, resulting in poor deposition quality. However, by reducing and adjusting the additives and processes, the 5nm Ni surface prepared by us is smooth and bright, and the hardness is as high as 9.52GPa, which is 2-3 times the hardness of the sample.
[0089] Comparative Example 3
[0090] This comparative example provides a method for preparing nano nickel, which specifically comprises the following steps:
[0091] Preparation of plating solution: 300 g / L NiSO4·6H2O, 45 g / L NiCl2·6H2O, 40 g / L H3BO3 and 0.1 g / L sodium dodecyl sulfate were dissolved in deionized water, stirred on a magnetic stirring heating table, and the temperature was controlled to 35±1°C. After stirring and dissolving, the solution was filtered with filter paper. The filtrate after filtration with filter paper was pre-plated for 24 hours. The pre-plating process used a pure nickel plate as an anode and a coarse-grained nickel sheet as a cathode. The current density was 50 mA / cm 2 ; Then, 6 g / L of sodium saccharin and 0.6 g / L of 1,4-butynediol were added to the filtrate after the pre-plating treatment to obtain a plating solution; and 1 g / L of 1,4-butynediol was added at a rate of 200 uL / min using a peristaltic pump to control the concentration of the additive to remain constant during the electrodeposition process;
[0092] Electrodeposition: Nano nickel was prepared by direct current electrodeposition. The process parameters of direct current electrodeposition were: pure nickel plate was used as sacrificial anode, coarse-grained nickel sheet with a grain size of 25 μm was used as cathode, and the current density was continuously controlled at a constant 0.05 mA / cm² by a computer program.
[0093] When 0.05 mA / cm 2 Even at lower current densities, we found that due to the high ion solubility, effective deposition could not be achieved for a long time, and the activated substrate Ni plate would lose its activity, resulting in the inability to deposit the nanocrystalline Ni layer and complete the electrodeposition process.
[0094] Comparative Example 4
[0095] This comparative example provides a method for preparing nano nickel, which specifically comprises the following steps:
[0096] Preparation of plating solution: 300g / L NiSO4·6H2O, 45g / L NiCl2·6H2O, 40g / L H3BO3 and 0.1g / L sodium dodecyl sulfate were dissolved in deionized water, stirred on a magnetic stirring heating table, and the temperature was controlled to 55±1℃. After stirring and dissolving, the solution was filtered with filter paper. The filtrate after filtering with filter paper was pre-plated for 24 hours, with a pure nickel plate as the anode and a coarse-grained nickel sheet as the cathode, and the current density was 50mA / cm². Then, 6g / L saccharin sodium and 2g / L 1,4-butynediol were added to the filtrate after pre-plating to obtain a plating solution. A peristaltic pump was used to add 1g / L 1,4-butynediol at a rate of 200uL / min to control the concentration of additives to remain constant during the electrodeposition process.
[0097] Electrodeposition: Nano nickel is prepared by direct current electrodeposition; the process parameters of direct current electrodeposition are: pure nickel plate is used as sacrificial anode, coarse-grained nickel sheet with a grain size of 25μm is used as cathode, and the current density is continuously controlled by a computer program to be constant at 1mA / cm².
[0098] When using too high a concentration of 1,4-butynediol, we found that due to the excessive adsorption sites of 1,4-butynediol, effective deposition cannot be achieved at low current density. The activated base Ni plate loses its activity, resulting in the inability to deposit the nanocrystalline Ni layer, and the electrodeposition process cannot be completed.
[0099] Comparative Example 5
[0100] This comparative example provides a method for preparing nano nickel, which specifically comprises the following steps:
[0101] Preparation of plating solution: 300g / L NiSO4·6H2O, 45g / L NiCl2·6H2O, 40g / L H3BO3 and 0.1g / L sodium dodecyl sulfate are dissolved in deionized water, stirred on a magnetic stirring heating table, and the temperature is controlled to 55±1℃, and then filtered with filter paper after stirring and dissolving; the filtrate after filtering with filter paper is pre-plated for 24 hours, and the pre-plating process uses a pure nickel plate as an anode and a coarse-grained nickel sheet as a cathode, and the current density is 50mA / cm²; then 6g / L saccharin sodium is added to the filtrate after pre-plating to obtain a plating solution;
[0102] Electrodeposition: Nano nickel is prepared by direct current electrodeposition; the process parameters of direct current electrodeposition are: pure nickel plate is used as sacrificial anode, coarse-grained nickel sheet with a grain size of 25μm is used as cathode, and the current density is continuously controlled by a computer program to be constant at 1mA / cm².
[0103] The average grain size of the nano nickel sample prepared in this comparative example is 32nm and the hardness is 4.5GPa. Since the additive of this comparative example does not contain 1,4-butynediol, the effect of grain refinement cannot be achieved, thereby reducing the hardness of the nano nickel. However, by adding a certain amount of 1,4-butynediol, the hardness of the 5nm Ni prepared in this application is as high as 9.52GPa, which is 2-3 times the hardness of the superhard protective coating.
[0104] It is easy for those skilled in the art to understand that, without conflict, the advantageous technical features of the above-mentioned methods can be freely combined and superimposed.
[0105] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing nano nickel, characterized in that: The following steps are involved: Preparation of plating solution: dissolving nickel sulfate hexahydrate, nickel chloride hexahydrate, boric acid and sodium dodecyl sulfate in deionized water, stirring and dissolving, and filtering with filter paper; then adding additives of saccharin sodium and 1,4-butynediol to the filtrate to obtain the plating solution; Among them, the concentrations of nickel sulfate hexahydrate, nickel chloride hexahydrate, boric acid, sodium dodecyl sulfate and sodium saccharin are 100-300 g / L, 20-50 g / L, 20-50 g / L, 0.05-0.2 g / L and 3-6 g / L respectively; the concentration of 1,4-butynediol is greater than 0.5 g / L and less than or equal to 1 g / L; Electrodeposition: The nano nickel is prepared by direct current electrodeposition; The anode is a nickel plate with a purity of 99.6%, and the cathode is a nickel sheet with a grain size of 10-40 μm. The process parameters of the DC electrodeposition are: the current density is 1-5 mA / cm 2 .
2. The method for preparing nano nickel according to claim 1, characterized in that: The pH range of the plating solution is 4-6.
3. The method for preparing nano nickel according to claim 1, characterized in that: In the plating solution preparation step, a pre-plating treatment is performed in the filtrate after filtering with filter paper, and then an additive is added to the filtrate after the pre-plating treatment; The pre-plating treatment time is 20-30 hours.
4. The method for preparing nano nickel according to claim 1, characterized in that: In the electrodeposition step, the temperature of the plating solution is 30-60°C.
5. The method for preparing nano nickel according to claim 4, characterized in that: Before electrodeposition, the nickel sheet is sequentially ground, polished and surface degreased, pickled in a mixed solution of sulfuric acid and hydrochloric acid, and then electrolytically polished and activated; The nickel sheet was mechanically polished using 400#, 1000# and 2000# sandpapers in sequence.
6. A nano nickel, characterized in that: The thickness of the nano nickel is 100-200 microns; the grain size of the nano nickel is 5-10 nm; The nano nickel is obtained by the preparation method described in any one of claims 1 to 5.
7. The nano nickel according to claim 6, characterized in that: The hardness of the nano nickel is 7.02-9.32 GPa.
8. The nano nickel according to claim 6, characterized in that: The grain coarsening temperature of the nano nickel is 450°C.