Method for preparing fireproof material for cable, fire-resistant cable
The preparation of refractory paper by combining hydroxyapatite nanowires with titanium dioxide whiskers with aluminum silicate fibers has been solved, and the problems of cable fire resistance and service life are achieved at high temperatures have been achieved.
Patent Information
- Application Number
- CN202410964101.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-18
AI Technical Summary
The existing cables are not refractory enough, mica refractory paper cannot effectively prevent the spread of fire in large fires, and poor flexibility leads to the refractory paper being easily torn during use and transportation, affecting the service life of the cable.
Using hydroxyapatite nanowires combined with titanium dioxide whiskers, combined with aluminum silicate fibers and adhesives, refractory paper is prepared through specific mixing and treatment methods to enhance its flexibility and tear resistance, and is coated on the cable Surface to prevent the fire from spreading.
It improves the fire resistance and service life of the cable, can maintain integrity at high temperatures, extend the service life of the refractory paper, and buys time for fire rescue.
Smart Images

Figure CN118507129B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of cables, and more specifically, to a method for preparing a fireproof material for cables and a fire-resistant cable. Background Art
[0002] Cable is a device for transmitting electric energy or signals, usually composed of several or several groups of wires. However, if a high-voltage cable has a fire problem, the impact is serious, so the fire resistance of the cable is required to be high. In the event of a fire, by preventing the fire from spreading, time is bought for the evacuation of personnel and the fire fighting. Mica fire-resistant paper is often used on the surface of existing cables, but the high temperature resistance of mica fire-resistant paper is poor. When a large cable fire occurs, it is impossible to buy more time for the evacuation of personnel and the fire fighting.
[0003] Hydroxyapatite nanowires have high high temperature resistance and can generally withstand temperatures above 1000°C without being destroyed. Therefore, the use of hydroxyapatite nanowires to prepare fire-resistant paper for use on cables can better protect the cables and buy time for personnel evacuation and fire rescue.
[0004] However, hydroxyapatite material has certain brittleness and poor flexibility, which can easily affect the softness of the refractory paper and is not easy to be coated on the surface of the circular conductor. However, refractory paper with good flexibility is prone to tearing or breaking during use, storage or transportation, which affects the integrity of the refractory paper and thus the fire resistance and service life of the cable.
[0005] Therefore, how to prepare a new fire-resistant cable with better fire resistance and longer service life is a problem to be solved. Summary of the invention
[0006] In order to prepare a new fire-resistant cable with better fire resistance and longer service life, the present application provides a method for preparing a fire-resistant material for a cable and a fire-resistant cable.
[0007] The present application provides a method for preparing a fireproof material for cables, which adopts the following technical solution:
[0008] A method for preparing a fireproof material for a cable comprises the following steps:
[0009] Ⅰ. Mixing hydroxyapatite nanowire filaments and titanium dioxide whiskers uniformly at a mass ratio of 1:0.05-0.1 to obtain a nanowire mixture;
[0010] Ⅱ. Dispersing aluminum silicate fibers uniformly in water to prepare a suspension;
[0011] III. Add the nanowire mixture to the suspension, disperse it evenly, add the adhesive, stir it evenly to get the slurry, filter it, shape it, squeeze it, dry it, and make it into a finished product.
[0012] By adopting the above technical scheme, the surface of the conductor is coated with fire-resistant paper and silicone rubber layer in sequence. The fire-resistant effect of the fire-resistant paper can prevent the spread of fire, and the elasticity and toughness of the silicone rubber layer can ensure the service life of the fire-resistant cable, thereby making the fire-resistant cable have the advantages of good fire resistance and long service life.
[0013] In the preparation process of refractory paper, hydroxyapatite nanowire filaments and titanium dioxide whiskers are matched with each other. The good flexibility of hydroxyapatite nanowire filaments is combined with the supporting effect of titanium dioxide whiskers, and the mass ratio of the two is limited, so that the nanowire mixture has good flexibility and good strength supporting effect under the condition of interweaving and winding, and the refractory paper has good flexibility and tear resistance; combined with the flexibility of aluminum silicate fiber, when the aluminum silicate fiber and the nanowire mixture are evenly mixed, under the bonding action of the adhesive, a structure is formed with aluminum silicate fiber as support and solidification, and the adhesive is used as a connection, so that the hydroxyapatite nanowires are stably and evenly adhered to the surface of the aluminum silicate fiber, and the hydroxyapatite nanowire filaments and titanium dioxide whiskers are interwoven and wound on the surface of the aluminum silicate fiber, ensuring the density of the cross-linked structure, so that the refractory paper has the advantages of high flexibility and not easy to tear. It is coated on the surface of the cable, and its good fire resistance and mechanical stability are used to prevent the spread of fire and buy time for fire rescue and personnel evacuation.
[0014] Preferably, the hydroxyapatite nanowire filaments are prepared by the following method:
[0015] Water, ethanol and oleic acid are mixed and stirred evenly in a mass ratio of 22:3-6:4-8 to obtain a primary mixture; chitosan-loaded calcium chloride and tyrosine-loaded sodium dihydrogen phosphate are added to the primary mixture, the mass ratio of water, chitosan-loaded calcium chloride and tyrosine-loaded sodium dihydrogen phosphate is 22:2.5-2.8:5-5.6, the mixture is mixed and stirred for 10-20 minutes, sealed, reacted at 180-190°C for 14-16 hours, and then sodium hydroxide solution is added, the mass ratio of water to sodium hydroxide solution is 22:7-9, mixed and stirred evenly, sealed, and then the reaction is continued for 8-10 hours. After cooling, hydroxyapatite nanowire filaments are obtained by precipitation, washing and filtering.
[0016] By adopting the above technical scheme, chitosan-loaded calcium chloride and tyrosine-loaded sodium dihydrogen phosphate are matched and reacted at a relatively high temperature, thereby accelerating the release of calcium chloride in the chitosan-loaded calcium chloride and accelerating the release of sodium dihydrogen phosphate in the tyrosine-loaded potassium dihydrogen phosphate. The gradually released calcium chloride and sodium dihydrogen phosphate react to eventually generate hydroxyapatite nanowire filaments. Through the effect of gradual release, the hydroxyapatite nanowire filaments grow continuously and can reach a length of 200-1000 μm. If the temperature is high, although it can accelerate the reaction, it is easy to cause the hydroxyapatite nanowires to become shorter. The loading of chitosan and tyrosine enables the hydroxyapatite nanowires to grow gradually and continuously after the growth of the crystal nucleus, thereby accelerating the reaction while ensuring that the hydroxyapatite nanowires are long in length, so as to prepare ultra-long and flexible hydroxyapatite nanowire filaments.
[0017] During the reaction process, calcium chloride on the surface of chitosan and sodium dihydrogen phosphate on the surface of tyrosine react first to generate crystal nuclei; then hydroxyapatite nanowires gradually grow, and the positive charge of chitosan cooperates with the negative charge of tyrosine, so that adjacent chitosan-loaded calcium chloride and tyrosine-loaded sodium dihydrogen phosphate are easy to contact each other, and gradually react through the gradual release of calcium source and phosphorus source, thereby promoting the gradual growth of hydroxyapatite nanowires; at the same time, adjacent chitosan-loaded calcium chloride and adjacent tyrosine-loaded sodium dihydrogen phosphate are not easy to aggregate due to the mutual repulsion of charges, which limits the growth direction and growth trend of the hydroxyapatite nanowires and is not easy to cause the problem of multi-directional growth, thereby ensuring that the hydroxyapatite nanowire filaments can grow ultra-long.
[0018] After adding sodium hydroxide solution, the molecular chain of chitosan gradually breaks under the action of sodium hydroxide. In addition, under alkaline conditions, chitosan and tyrosine are both negatively charged, and their repulsion effect is used to prevent the hydroxyapatite nanowires from agglomerating with each other, thereby ensuring the ultra-long growth of the hydroxyapatite nanowires. Tyrosine can also gradually react under the action of sodium hydroxide, gradually releasing sodium dihydrogen phosphate, so that the bound calcium chloride and sodium dihydrogen phosphate are further released, completing the subsequent reaction, and continuing to grow at both ends of the shorter hydroxyapatite nanowires to form ultra-long hydroxyapatite nanowires. At the same time, sodium hydroxide can Promoting the directional growth of hydroxyapatite nanowires further ensures that the hydroxyapatite nanowires grow in the length direction, and is not prone to the problem of different growth forms, so that the generated hydroxyapatite nanowires have the advantages of being super long, flexible, uniform in form, and not prone to cracks and gaps, ensuring the flexibility and tear resistance of the hydroxyapatite nanowire filaments, thereby ensuring that the fire-resistant paper has good flexibility and tear resistance, ensuring the preparation of fire-resistant cables, and having high stability after a fire occurs, and is not prone to the problem of fire-resistant paper peeling off and spreading the fire, thereby improving the fire resistance of the fire-resistant cable and extending its service life.
[0019] Preferably, the chitosan-loaded calcium chloride is prepared by the following method:
[0020] Chitosan is immersed and stirred in a calcium chloride solution with a mass fraction of 0.4-0.6% at a mass ratio of 1:0.5-1, and then freeze-dried to obtain loaded chitosan; polyethylene glycol solution is evenly sprayed on the surface of the loaded chitosan, and then calcium chloride powder is added, the mass ratio of the loaded chitosan to the polyethylene glycol solution and the calcium chloride powder is 1:0.1-0.22:0.2-0.35, and the finished product is obtained after drying and dispersion.
[0021] By adopting the above technical scheme, polyethylene glycol solution is uniformly sprayed on the surface of the loaded chitosan, and calcium chloride is bonded to the surface of the chitosan by utilizing the viscosity of the polyethylene glycol solution. Under the action of moisture content, the calcium chloride on the surface of the chitosan can be gradually dissolved, and calcium ions participate in the reaction, thereby generating hydroxyapatite nanowire filament nuclei and ensuring the generation of short hydroxyapatite nanowires. The gradual mutual repulsion effect of adjacent chitosans and adjacent tyrosines is utilized to prevent the short hydroxyapatite nanowires from agglomerating with each other. As the chitosan is gradually destroyed under the action of sodium hydroxide, the calcium chloride adsorbed in the internal pores is further released. After the calcium chloride adsorbed in the chitosan pores is gradually released, the calcium ions further react and continue to extend at both ends of the short hydroxyapatite nanowires, thereby ensuring the ultra-long growth of the hydroxyapatite nanowires, making it convenient for ultra-long and flexible fire-resistant paper to be wrapped around the surface of the conductor to prepare a fire-resistant cable.
[0022] Preferably, the tyrosine-loaded sodium dihydrogen phosphate is prepared by the following method:
[0023] The polyethylene glycol solution is evenly sprayed on the surface of the tyrosine particles at a mass ratio of 1:0.4-0.55, and then sodium dihydrogen phosphate is added, and the mass ratio of tyrosine particles to sodium dihydrogen phosphate is 1:0.6-0.85. After drying and dispersion, a finished product is obtained.
[0024] By adopting the above technical scheme, the viscosity of the polyethylene glycol solution is used to bond sodium dihydrogen phosphate to the surface of the tyrosine particles. The combination of tyrosine and chitosan can prevent the precipitation of hydroxyapatite nanowires, ensure the ultra-long growth of hydroxyapatite nanowire filaments, and not easily affect the growth length due to aggregation; and the polyethylene glycol can provide guidance for the growth of hydroxyapatite nanowires, ensure the straight growth of hydroxyapatite nanowires, and not easily have the problem of uneven shape, thereby ensuring the flexibility and tear resistance of the fire-resistant paper, so that the fire-resistant cable has the advantages of good fire resistance and long service life.
[0025] Preferably, the titanium dioxide whiskers are prepared by the following method:
[0026] The titanium dioxide whisker is dispersed in ethanol, and then tyrosine is added, and the dispersion is continued. After uniform mixing, shellac is added and mixed uniformly. The mass ratio of the titanium dioxide whisker to tyrosine and shellac is 1:0.1-0.3:0.1-0.2. After drying and dispersion, a finished product is obtained.
[0027] By adopting the above technical scheme, titanium dioxide whiskers are evenly contacted with tyrosine after being dispersed in ethanol, and the viscosity of the shellac solution after being dissolved in ethanol is utilized to facilitate the bonding of tyrosine to the surface of the titanium dioxide whiskers. The hydroxyapatite nanowires are negatively charged, and the tyrosine-treated titanium dioxide whiskers are also negatively charged, so that the titanium dioxide whiskers and the hydroxyapatite nanowires are evenly dispersed. The pore structure produced by the even dispersion ensures the soft foldability of the refractory paper, which is convenient for winding and coating on the surface of the conductor to prepare the cable; and the mechanical strength of the titanium dioxide whiskers and the water resistance of the shellac are utilized to further improve the tear resistance and water resistance of the refractory paper, thereby extending the service life of the refractory paper, thereby ensuring the service life of the refractory cable.
[0028] Preferably, the adhesive is prepared by the following method:
[0029] Sodium silicate is placed in water at a mass ratio of 1:15-25 and stirred until it is completely dissolved to obtain a dissolving solution; nanoparticles and polyethylene glycol solution are added to the dissolving solution, the mass ratio of sodium silicate to nanoparticles and polyethylene glycol solution is 1:0.1-0.2:0.2-0.5, and the mixture is stirred evenly; finally, sodium polyacrylate coated calcium hydroxide is added, the mass ratio of sodium silicate to sodium polyacrylate coated calcium hydroxide is 1:0.1-0.3, and the mixture is stirred evenly to obtain an adhesive.
[0030] By adopting the above technical scheme, sodium silicate is used as the main adhesive, which gives the fire-resistant paper better fire resistance and water resistance; combined with the thickening effect of polyethylene glycol, the bonding effect of the adhesive is further improved, and the nanoparticles are dispersed and filled between the nanowire mixture and the aluminum silicate fiber. The nanoparticles can not only improve the tear resistance of the fire-resistant paper, but also further improve the fire resistance and water resistance, and extend the service life of the fire-resistant paper, so that the fire-resistant cable has the advantages of good fire resistance and long service life.
[0031] The sodium polyacrylate in the sodium polyacrylate coated calcium hydroxide dissolves slowly in water, so the calcium hydroxide is not completely released when the sodium silicate solution exerts a bonding effect. As the reaction temperature increases, the sodium polyacrylate gradually dissolves to release calcium hydroxide, and the calcium silicate precipitate and sodium hydroxide are gradually generated by the reaction of sodium silicate and calcium hydroxide; the calcium silicate precipitate not only has good high temperature resistance and fire resistance, but also has good water resistance, and the gradually generated sodium hydroxide is easy to gradually dissolve shellac and tyrosine under the action of water, so that the original position occupied by the titanium dioxide whisker is reduced, and the distance between the titanium dioxide whisker and the hydroxyapatite nanowire filament is lengthened, that is, the space originally occupied by the titanium dioxide whisker, when the tyrosine and shellac on the surface of the titanium dioxide whisker flow away from the surface of the titanium dioxide whisker, the pores around the titanium dioxide whisker increase, and the water-soluble sodium shellac can improve the bonding effect of the titanium dioxide whisker with the aluminum silicate fiber and the hydroxyapatite nanowire filament, and improve the porosity while improving the flexibility, thereby improving the flexibility of the finished fire-resistant paper.
[0032] Preferably, the nanoparticles are composed of fumed silicon dioxide and boron nitride in a mass ratio of 1:0.5-1.
[0033] By adopting the above technical scheme, the uniform dispersion effect of nanoparticles in the adhesive is utilized, combined with the fire resistance of fumed silica and boron nitride, the fire resistance of the fire-resistant paper is improved, and the filling effect of nanoparticles is combined to further improve the tear resistance and extend the service life of the fire-resistant paper.
[0034] Preferably, the sodium polyacrylate coated calcium hydroxide is made of a sodium polyacrylate solution and calcium hydroxide particles in a mass ratio of 1:0.5-1.
[0035] By adopting the above technical scheme, calcium hydroxide is coated with sodium polyacrylate solution. The sodium polyacrylate has a certain flexibility after film formation, which ensures the flexibility of the fire-resistant paper. The hydrophilicity of sodium polyacrylate makes it easy for the sodium polyacrylate-coated calcium hydroxide to approach the nanowire mixture. Tyrosine and shellac exist on the surface of the titanium dioxide whisker. Tyrosine contains hydrophilic groups such as amino and carboxyl groups, which facilitate mutual attraction and connection with sodium polyacrylate. After the sodium polyacrylate-coated calcium hydroxide gradually reacts with sodium silicate, although the porosity near the titanium dioxide whisker increases, under the bonding effect of the dissolved shellac, the titanium dioxide whisker can still stably bond with the aluminum silicate fiber and hydroxyapatite nanowire filament in contact with it, ensuring the porosity while ensuring the structural stability. The presence of porosity ensures flexibility, and the structural stability can give the fire-resistant paper a better tear resistance.
[0036] Preferably, after adding the adhesive to III, stir for 20-30 minutes, then heat to 70-85° C., and continue stirring for 5-10 minutes.
[0037] By adopting the above technical scheme, after adding the adhesive, it is first stirred to allow the sodium silicate solution and the polyethylene glycol solution to exert a bonding effect, and the nanowire mixture is adhered to the surface of the aluminum silicate fiber. As the temperature rises, the sodium polyacrylate gradually dissolves to expose the calcium hydroxide, and the calcium hydroxide gradually reacts with the sodium silicate. The reaction product, the sodium hydroxide solution, can dissolve shellac, increase the porosity around the titanium dioxide whiskers, and at the same time ensure the bonding stability, so that the refractory paper has flexibility and tear resistance.
[0038] Preferably, the aluminum silicate fiber is prepared by the following method:
[0039] The aluminum silicate fiber filaments are mixed and ground with aminosulfonic acid particles, and then the aluminum silicate fiber filaments are filtered and sieved to obtain aluminum silicate fibers.
[0040] By adopting the above technical scheme, the surface area of the aluminum silicate fiber is increased after being ground with aminosulfonic acid, which is convenient for bonding with the hydroxyapatite nanowire composite material, and the surface can be loaded with aminosulfonic acid. Aminosulfonic acid contains amino and sulfonic acid groups, which is convenient for cross-linking and bonding with the adhesive, and can also be connected with the hydroxyl groups in the hydroxyapatite nanowire filaments and the amino and carboxyl groups on the surface of the titanium dioxide whisker, thereby improving the bonding effect between the aluminum silicate fiber and the hydroxyapatite nanowire filaments and the titanium dioxide whiskers, and improving the cross-linking stability of the fire-resistant paper; and aminosulfonic acid can cross-link with the polyethylene glycol solution in the adhesive to generate sulfonate esters, which not only have good fire resistance, but also have good water resistance, thereby extending the service life of the fire-resistant paper.
[0041] Preferably, a fire-resistant cable comprises a conductor, the outer side of the conductor is coated with a layer of fire-resistant paper, and the outer side of the fire-resistant paper is also sequentially provided with a silicone rubber layer, an armor layer and an outer sheath.
[0042] Preferably, the silicone rubber layer is hollow and forms an air storage cavity, the inner cavity of the air storage cavity is filled with flame-retardant gas, and a plurality of partition plates are evenly spaced in the inner cavity of the air storage cavity, and the plurality of partition plates divide the air storage cavity into a plurality of unconnected sub-cavities.
[0043] In summary, this application has the following beneficial effects:
[0044] 1. The fire resistance of the cable is better, and it achieves good fire prevention effect and reduces losses.
[0045] 2. The surface of the conductor is coated with refractory paper in sequence, and hydroxyapatite nanowire filaments and titanium dioxide whiskers are matched. The good flexibility of hydroxyapatite nanowire filaments is combined with the supporting effect of titanium dioxide whiskers, and the mass ratio of the two is limited, so that the nanowire mixture has good flexibility and good strength supporting effect under the condition of interweaving and winding, and the refractory paper has good flexibility and tear resistance; combined with the flexibility of aluminum silicate fiber, when the aluminum silicate fiber and the nanowire mixture are evenly mixed, under the bonding action of the adhesive, a solidification with aluminum silicate fiber as support and adhesive as connection is formed, and the hydroxyapatite nanowires are stably and evenly adhered to the surface of the aluminum silicate fiber. The hydroxyapatite nanowire filaments and titanium dioxide whiskers are interwoven and wound on the surface of the aluminum silicate fiber, ensuring the density of the cross-linked structure, so that the refractory paper has the advantages of high flexibility and not easy to tear. It is coated on the surface of the cable and uses its good fire resistance to prevent the spread of fire and buy time for fire rescue and personnel evacuation.
[0046] 3. In the chitosan-loaded calcium chloride, polyethylene glycol cooperates with chitosan. The polyethylene glycol near the chitosan can induce the linear growth of hydroxyapatite nanowire filaments. Combined with the separation effect of chitosan and the dispersion effect of polyethylene glycol, the agglomeration problem of short hydroxyapatite nanowires is prevented, and the ultra-long growth of hydroxyapatite nanowires is ensured. The fire-resistant paper prepared from the soft hydroxyapatite nanowire filaments can be adhered to the surface of the conductor, thereby improving the fire resistance of the cable and extending the service life of the cable.
[0047] 4. Fire-resistant paper is highly flexible and can be curled at will. It is also resistant to high temperatures and can maintain its integrity even at 1000°C. It can be used for writing and color printing, and is expected to be used for the long-term safe preservation of books and important documents such as archives and certificates. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 The present invention is a schematic diagram of the structure of a fire-resistant cable in an embodiment of the present invention.
[0049] Figure 2 The present invention is a schematic diagram of a gas storage cavity formed in a silicone rubber layer in an embodiment of a fire-resistant cable.
[0050] Figure 3 The present invention is a schematic diagram of a fire-resistant cable embodiment in which a partition plate is installed in the air storage cavity.
[0051] Figure numerals: 1. conductor; 2. fire-resistant paper; 3. silicone rubber layer; 4. armor layer; 5. outer sheath; 6. gas storage cavity; 7. partition plate; 8. sub-cavity; 9. flame-retardant gas. DETAILED DESCRIPTION
[0052] The present application is further described in detail below in conjunction with embodiments.
[0053] First aspect: The present application discloses a method for preparing a fire retardant material for cables.
[0054] The preparation example of hydroxyapatite nanowire filaments
[0055] The following raw materials are all commercially available.
[0056] Preparation Example 1: Hydroxyapatite nanowire filaments are prepared by the following method:
[0057] 1 kg of chitosan was placed in 1 kg of 0.5% calcium chloride solution by mass, the calcium chloride solution was added at a speed of 200 g / min, the chitosan was stirred at a speed of 120 r / min during the addition process, the average particle size of the chitosan was 20 μm, the average porosity was 50%, and the chitosan was freeze-dried to obtain loaded chitosan; 0.2 kg of polyethylene glycol solution was evenly sprayed on the surface of 1 kg of loaded chitosan, and then 0.3 kg of calcium chloride powder was added, the calcium chloride powder was added at a speed of 100 g / min, and the loaded chitosan was stirred at a speed of 120 r / min during the addition process, the polyethylene glycol solution was a polyethylene glycol ethanol solution with a mass fraction of 5%, the polyethylene glycol was polyethylene glycol 2000, the mass fraction of ethanol was 75%, and the average particle size of the calcium chloride powder was 3 μm. After the addition was completed, the mixing and stirring was continued for 10 min, and then dried and dispersed to obtain chitosan loaded calcium chloride, and the chitosan loaded calcium chloride was sieved through a 400 mesh sieve;
[0058] 0.5 kg of polyethylene glycol solution is uniformly sprayed on the surface of 1 kg of tyrosine particles, and then 0.8 kg of sodium dihydrogen phosphate is added, dried, dispersed, and tyrosine-loaded sodium dihydrogen phosphate is obtained, and the tyrosine particles are sieved through a 400-mesh sieve; the average particle size of the tyrosine particles is 20 μm, the polyethylene glycol solution is a polyethylene glycol ethanol solution with a mass fraction of 5%, the polyethylene glycol is polyethylene glycol 2000, the mass fraction of ethanol is 75%, and the average particle size of potassium dihydrogen phosphate is 3 μm;
[0059] 22 kg of water, 5 kg of ethanol and 7 kg of oleic acid were mixed and stirred to obtain a primary mixture; 2.6 kg of chitosan-loaded calcium chloride and 5.4 kg of tyrosine-loaded sodium dihydrogen phosphate were added to the primary mixture, mixed and stirred for 15 minutes, sealed, and reacted at 185°C for 14 hours, and then 8 kg of sodium hydroxide solution was added, the sodium hydroxide solution was 8% by mass of sodium hydroxide aqueous solution, mixed and stirred to obtain a uniform mixture, sealed, and then continued to react for 9 hours. After cooling, the mixture was precipitated, and the precipitate was washed with ethanol 3 times, washed with water 2 times, and the water was filtered out to obtain hydroxyapatite nanowire filaments.
[0060] Preparation Example 2: This preparation example differs from Preparation Example 1 in that:
[0061] 1 kg of chitosan was placed in 0.5 kg of 0.4% calcium chloride solution, the calcium chloride solution was added at a speed of 200 g / min, the chitosan was stirred at a speed of 120 r / min during the addition process, and the chitosan was freeze-dried to obtain loaded chitosan; 0.1 kg of polyethylene glycol solution was evenly sprayed on the surface of 1 kg of loaded chitosan, and then 0.2 kg of calcium chloride powder was added, and the calcium chloride powder was added at a speed of 100 g / min. During the addition process, the loaded chitosan was stirred at a speed of 120 r / min. After the addition was completed, the mixing and stirring was continued for 10 minutes, and then dried and dispersed to obtain chitosan loaded calcium chloride, and the chitosan loaded calcium chloride was sieved through a 400-mesh sieve;
[0062] 0.45 kg of polyethylene glycol solution was evenly sprayed on the surface of 1 kg of tyrosine particles, and then 0.6 kg of sodium dihydrogen phosphate was added, and the mixture was dried and dispersed to obtain tyrosine-loaded sodium dihydrogen phosphate;
[0063] 22 kg of water, 3 kg of ethanol and 4 kg of oleic acid were mixed and stirred to obtain a primary mixture; 2.5 kg of chitosan-loaded calcium chloride and 5 kg of tyrosine-loaded sodium dihydrogen phosphate were added to the primary mixture, mixed and stirred for 10 minutes, sealed, and reacted at 180° C. for 16 hours, and then 7 kg of sodium hydroxide solution was added, the sodium hydroxide solution was 8% by mass of sodium hydroxide aqueous solution, mixed and stirred evenly, sealed, and then continued to react for 8 hours. After cooling, hydroxyapatite nanowire filaments were obtained by precipitation, washing and filtration.
[0064] Preparation Example 3: This preparation example differs from Preparation Example 1 in that:
[0065] 1 kg of chitosan was placed in 1 kg of 0.6% calcium chloride solution, the calcium chloride solution was added at a speed of 200 g / min, the chitosan was stirred at a speed of 120 r / min during the addition process, the average particle size of chitosan was 20 μm, the average porosity was 50%, and the chitosan was freeze-dried to obtain loaded chitosan; 0.22 kg of polyethylene glycol solution was evenly sprayed on the surface of 1 kg of loaded chitosan, and then 0.35 kg of calcium chloride powder was added, and the calcium chloride powder was added at a speed of 100 g / min. During the addition process, the loaded chitosan was stirred at a speed of 120 r / min. After the addition was completed, the mixing and stirring were continued for 10 minutes, and then dried and dispersed to obtain chitosan loaded calcium chloride;
[0066] 0.55 kg of polyethylene glycol solution was evenly sprayed on the surface of 1 kg of tyrosine particles, and then 0.85 kg of sodium dihydrogen phosphate was added, and the mixture was dried and dispersed to obtain tyrosine-loaded sodium dihydrogen phosphate;
[0067] 22 kg of water, 6 kg of ethanol and 8 kg of oleic acid were mixed and stirred to obtain a primary mixture; 2.8 kg of chitosan-loaded calcium chloride and 5.6 kg of tyrosine-loaded sodium dihydrogen phosphate were added to the primary mixture, mixed and stirred for 20 minutes, sealed, and reacted at 190° C. for 14 hours, and then 9 kg of sodium hydroxide solution was added, the sodium hydroxide solution was 8% by mass of sodium hydroxide aqueous solution, mixed and stirred evenly, sealed, and then continued to react for 10 hours. After cooling, hydroxyapatite nanowire filaments were obtained by precipitation, washing and filtration.
[0068] Preparation Example of Titanium Dioxide Whiskers
[0069] The following raw materials are all commercially available.
[0070] Preparation Example 4: Titanium dioxide whiskers are prepared by the following method:
[0071] 1 kg of titanium dioxide whiskers were placed in 10 kg of ethanol and ultrasonically dispersed at 20 kHz for 10 minutes. The average length of the titanium dioxide whiskers was 20 μm, the average diameter was 10 nm, and the mass fraction of ethanol was 99%. Then, 0.2 kg of tyrosine was added, and the average particle size of tyrosine was 100 nm. The dispersion was continued for 10 minutes. After mixing evenly, 0.15 kg of shellac was added and stirred at a speed of 200 r / min until the shellac was completely dissolved. After drying and dispersion, a finished product was obtained. The finished product was sieved through a 400-mesh sieve.
[0072] Preparation Example 5: This preparation example differs from Preparation Example 4 in that:
[0073] 1 kg of titanium dioxide whiskers were placed in 10 kg of ethanol and ultrasonically dispersed at 20 kHz for 10 minutes; then 0.1 kg of tyrosine was added and the dispersion was continued for 10 minutes. After uniform mixing, 0.1 kg of shellac was added and stirred at a speed of 200 r / min until the shellac was completely dissolved. After drying and dispersion, the finished product was obtained.
[0074] Preparation Example 6: This preparation example differs from Preparation Example 4 in that:
[0075] 1 kg of titanium dioxide whiskers were placed in 10 kg of ethanol and ultrasonically dispersed at 20 kHz for 10 minutes; then 0.3 kg of tyrosine was added and the dispersion was continued for 10 minutes. After uniform mixing, 0.2 kg of shellac was added and stirred at a speed of 200 r / min until the shellac was completely dissolved. After drying and dispersion, the finished product was obtained.
[0076] Preparation example of adhesive
[0077] The following raw materials are all commercially available.
[0078] Preparation Example 7: The adhesive is prepared by the following method:
[0079] Sodium polyacrylate was placed in water and stirred at 80°C until the sodium polyacrylate was completely dissolved to prepare a sodium polyacrylate solution with a mass fraction of 10%;
[0080] 1 kg of sodium polyacrylate solution was evenly sprayed on the surface of 1 kg of calcium hydroxide particles, the average particle size of the calcium hydroxide particles was 5 μm, and the particles were immediately air-dried after spraying, and finally dispersed until the calcium hydroxide particles did not stick to each other and agglomerated, so as to obtain sodium polyacrylate coated calcium hydroxide;
[0081] 1 kg of sodium silicate was placed in 20 kg of water and stirred until it was completely dissolved to obtain a dissolving solution; 0.15 kg of nanoparticles and 0.35 kg of polyethylene glycol solution were added to the dissolving solution, the addition rate of the nanoparticles and the polyethylene glycol solution was 60 g / min, and the mixture was stirred and mixed at a speed of 500 r / min during the addition process. After the addition was completed, the mixture was mixed and stirred for 20 minutes, and finally 0.2 kg of sodium polyacrylate coated calcium hydroxide was added at a rate of 60 g / min. The mixture was stirred continuously during the addition process to obtain an adhesive; the adhesive was used as prepared; the nanoparticles were composed of fumed silica and boron nitride in a mass ratio of 1:1, the average particle size of the fumed silica was 80 nm, and the average particle size of the boron nitride was 80 nm; the polyethylene glycol solution was a 5% by mass polyethylene glycol ethanol solution, the polyethylene glycol was polyethylene glycol 2000, and the mass fraction of ethanol was 75%.
[0082] Preparation Example 8: This preparation example differs from Preparation Example 7 in that:
[0083] 0.5 kg of sodium polyacrylate solution was evenly sprayed on the surface of 1 kg of calcium hydroxide particles, and air-dried immediately after spraying, and finally dispersed until the calcium hydroxide particles did not stick to each other and agglomerated, so as to obtain sodium polyacrylate coated calcium hydroxide;
[0084] 1 kg of sodium silicate was placed in 15 kg of water and stirred until completely dissolved to obtain a dissolving solution; 0.1 kg of nanoparticles and 0.2 kg of polyethylene glycol solution were added to the dissolving solution at a rate of 60 g / min, and the mixture was stirred and mixed at a speed of 500 r / min during the adding process. After the addition was completed, the mixture was stirred and mixed for 20 minutes, and finally 0.1 kg of sodium polyacrylate coated calcium hydroxide was added at a rate of 60 g / min. The mixture was stirred continuously during the adding process to obtain an adhesive; the nanoparticles were composed of fumed silica and boron nitride in a mass ratio of 1:0.5.
[0085] Preparation Example 9: This preparation example differs from Preparation Example 7 in that:
[0086] 1 kg of sodium polyacrylate solution was evenly sprayed on the surface of 1 kg of calcium hydroxide particles, and air-dried immediately after spraying, and finally dispersed until the calcium hydroxide particles did not stick to each other and agglomerated, so as to obtain sodium polyacrylate coated calcium hydroxide;
[0087] 1 kg of sodium silicate was placed in 25 kg of water and stirred until completely dissolved to obtain a dissolving solution; 0.2 kg of nanoparticles and 0.5 kg of polyethylene glycol solution were added to the dissolving solution at a rate of 60 g / min. During the adding process, the mixture was stirred and mixed at a speed of 500 r / min. After the addition was completed, the mixture was stirred and mixed for 20 minutes. Finally, 0.3 kg of sodium polyacrylate coated calcium hydroxide was added at a rate of 60 g / min. The mixture was stirred continuously during the adding process to obtain an adhesive.
[0088] Preparation example of fire-resistant paper
[0089] The following raw materials are all commercially available.
[0090] Preparation Example 10: Preparation method of fire-resistant paper:
[0091] Ⅰ. After 1 kg of hydroxyapatite nanowire filaments and 0.1 kg of titanium dioxide whiskers are mixed evenly, 8.9 kg of water is added, and the mixture is stirred evenly to obtain a nanowire mixture; the hydroxyapatite nanowire filaments are selected from the hydroxyapatite nanowire filaments prepared in Preparation Example 1; the titanium dioxide whiskers are selected from the titanium dioxide whiskers prepared in Preparation Example 4;
[0092] Ⅱ. Mix the aluminum silicate fiber and aminosulfonic acid particles and grind them for 5 minutes, then filter and screen the aluminum silicate fiber to obtain aluminum silicate fiber, the average length of which is 5 μm; evenly disperse 1 kg of aluminum silicate fiber in 99 kg of water to obtain a suspension, in which the aluminum silicate fiber accounts for 10% of the suspension;
[0093] III. Add 60 kg of the nanowire mixture to 100 kg of the suspension and ultrasonically disperse it at 20 kHz for 5 min. After it is evenly dispersed, add 20 kg of the adhesive prepared in Preparation Example 7 and stir it for 25 min at room temperature of 25 ° C and a speed of 1000 r / min. Then raise the temperature to 80 ° C and continue stirring for 10 min to obtain a slurry. After filtering water, forming, pressing and drying, a refractory paper is prepared. The average thickness of the refractory paper is 200 μm.
[0094] Preparation Example 11: This preparation example differs from Preparation Example 10 in that:
[0095] Ⅰ. After 1 kg of hydroxyapatite nanowire filaments and 0.05 kg of titanium dioxide whiskers are mixed evenly, 8.95 kg of water is added, and after mixing evenly, a nanowire mixture is obtained; the hydroxyapatite nanowire filaments are selected from the hydroxyapatite nanowire filaments prepared in Preparation Example 2; the titanium dioxide whiskers are selected from the titanium dioxide whiskers prepared in Preparation Example 5;
[0096] Ⅱ. Mix the aluminum silicate fiber and aminosulfonic acid particles and grind them for 5 minutes, then filter and screen the aluminum silicate fiber to obtain aluminum silicate fiber, the average length of which is 5 μm; evenly disperse 1 kg of aluminum silicate fiber in 99 kg of water to obtain a suspension, in which the aluminum silicate fiber accounts for 10% of the suspension;
[0097] III. Add 60 kg of the nanowire mixture to 100 kg of the suspension, ultrasonically disperse it at 20 kHz for 5 min, and after it is evenly dispersed, add 20 kg of the adhesive prepared in Preparation Example 8, stir it at room temperature of 25 ° C and a speed of 1000 r / min for 20 min, then raise the temperature to 70 ° C, continue stirring for 10 min to obtain a slurry, filter it, shape it, press it, and dry it to make refractory paper.
[0098] Preparation Example 12: This preparation example differs from Preparation Example 10 in that:
[0099] Ⅰ. After 1 kg of hydroxyapatite nanowire filaments and 0.1 kg of titanium dioxide whiskers are mixed evenly, 8.9 kg of water is added, and after mixing evenly, a nanowire mixture is obtained; the hydroxyapatite nanowire filaments are selected from the hydroxyapatite nanowire filaments prepared in Preparation Example 3; the titanium dioxide whiskers are selected from the titanium dioxide whiskers prepared in Preparation Example 6;
[0100] Ⅱ. Mix the aluminum silicate fiber and aminosulfonic acid particles and grind them for 5 minutes, then filter and screen the aluminum silicate fiber to obtain aluminum silicate fiber, the average length of which is 5 μm; evenly disperse 1 kg of aluminum silicate fiber in 99 kg of water to obtain a suspension, in which the aluminum silicate fiber accounts for 10% of the suspension;
[0101] III. Add 60 kg of the nanowire mixture to 100 kg of the suspension, ultrasonically disperse it at 20 kHz for 5 minutes, and after it is evenly dispersed, add 20 kg of the adhesive prepared in Preparation Example 9, stir it at room temperature of 25 ° C and a speed of 1000 r / min for 30 minutes, then raise the temperature to 85 ° C, continue stirring for 10 minutes to obtain a slurry, filter it, shape it, press it, and dry it to make refractory paper. Example
[0102] The polyurethane solution among the following raw materials was purchased from Lvyuan Baisui Chemical Technology (Beijing) Co., Ltd., brand PU850; the silicone rubber sheet was purchased from the silicone rubber sheet produced by Hebei Anyou Fluid Equipment Technology Co., Ltd., with a thickness of 5 mm; the heat-sealed polyethylene outer sheath was purchased from Hebei Liankuo Pipeline Co., Ltd.; other raw materials and equipment are all commonly available on the market.
[0103] Example 1: A method for preparing a fireproof material for cables:
[0104] S1, wrapping the conductor surface with fire-resistant paper, coating both sides of the fire-resistant paper with polyurethane solution, one side adheres to the conductor surface, and the other side of the fire-resistant paper is wrapped with two layers and bonded to the fire-resistant paper surface to form a fire-resistant layer, wrapping the fire-resistant layer surface with a silicone rubber sheet, bonding the polyurethane solution on both sides of the silicone rubber sheet, one side of the silicone rubber sheet is sticky to the fire-resistant paper surface, and the other side is wrapped with one layer and bonded to the fire-resistant paper surface, the silicone rubber sheet forms a silicone rubber layer, and a semi-finished product is obtained; the fire-resistant paper is the fire-resistant paper prepared in Preparation Example 10;
[0105] S2. Double steel belt armor is used to form an armor layer on the surface of the semi-finished product. The gap between the steel belts is 10mm, the steel belt overlap is 5mm, and the outermost surface is heat-sealed with a polyethylene outer sheath to obtain a finished fire-resistant cable.
[0106] Embodiment 2: This embodiment differs from Embodiment 1 in that:
[0107] The fire-resistant paper used is the fire-resistant paper prepared in Preparation Example 11.
[0108] Embodiment 3: This embodiment differs from Embodiment 1 in that:
[0109] The fire-resistant paper used is the fire-resistant paper prepared in Preparation Example 12.
[0110] Embodiment 4: This embodiment differs from Embodiment 1 in that:
[0111] In the preparation process of hydroxyapatite nanowire filaments, the chitosan-loaded calcium chloride is replaced by the same mass of calcium chloride, and the tyrosine-loaded sodium dihydrogen phosphate is replaced by the same mass of sodium dihydrogen phosphate.
[0112] Embodiment 5: This embodiment differs from Embodiment 1 in that:
[0113] Preparation process of hydroxyapatite nanowire filaments:
[0114] 22 kg of water, 5 kg of ethanol and 7 kg of oleic acid were mixed and stirred to obtain a primary mixture; 2.6 kg of chitosan-loaded calcium chloride and 5.4 kg of tyrosine-loaded sodium dihydrogen phosphate were added to the primary mixture, mixed and stirred for 15 minutes, 8 kg of sodium hydroxide solution was added, and the sodium hydroxide solution was an 8% sodium hydroxide aqueous solution by mass, mixed and stirred to obtain a uniform mixture, sealed, reacted at 185 ° C for 24 hours, cooled, precipitated, washed, filtered and separated to obtain hydroxyapatite nanowire filaments.
[0115] Embodiment 6: This embodiment differs from Embodiment 1 in that:
[0116] Preparation of chitosan-loaded calcium chloride for hydroxyapatite nanofilaments:
[0117] 0.2 kg of polyethylene glycol solution was evenly sprayed on the surface of 1 kg of chitosan, and then 0.35 kg of calcium chloride powder was added. The addition rate of calcium chloride powder was 100 g / min. During the addition, chitosan was stirred at a speed of 120 r / min. The polyethylene glycol solution was a 5% by mass polyethylene glycol ethanol solution, the polyethylene glycol was polyethylene glycol 2000, the mass fraction of ethanol was 75%, and the average particle size of the calcium chloride powder was 3 μm. After the addition was completed, the mixing and stirring was continued for 10 minutes, and then dried and dispersed to obtain chitosan-loaded calcium chloride.
[0118] Embodiment 7: This embodiment differs from Embodiment 1 in that:
[0119] Preparation of chitosan-loaded calcium chloride for hydroxyapatite nanofilaments:
[0120] 1 kg of chitosan was placed in 2 kg of 1% calcium chloride solution. The calcium chloride solution was added at a rate of 200 g / min. During the addition process, the chitosan was stirred at a speed of 120 r / min. The average particle size of the chitosan was 20 μm, and the average porosity was 50%. After freeze-drying, chitosan-loaded calcium chloride was obtained.
[0121] Embodiment 8: This embodiment differs from Embodiment 1 in that:
[0122] The titanium dioxide whiskers were ordinary commercially available silicon dioxide whiskers that had not been treated with tyrosine and shellac.
[0123] Embodiment 9: This embodiment differs from Embodiment 1 in that:
[0124] No nanoparticles were added during the preparation of the adhesive.
[0125] Embodiment 10: This embodiment differs from Embodiment 1 in that:
[0126] During the preparation of the adhesive, no polyethylene glycol solution was added.
[0127] Embodiment 11: This embodiment differs from Embodiment 1 in that:
[0128] During the preparation of the adhesive, no sodium polyacrylate-coated calcium hydroxide was added.
[0129] Embodiment 12: This embodiment differs from Embodiment 1 in that:
[0130] The aluminum silicate fiber is common commercially available aluminum silicate fiber and has not been ground with aminosulfonic acid particles. Comparative Example
[0131] Comparative Example 1: The difference between this comparative example and Example 1 is that:
[0132] No titanium dioxide whiskers were added to the raw materials.
[0133] Comparative Example 2: The difference between this comparative example and Example 1 is that:
[0134] The nanowire mixture was replaced by bamboo fiber of equal mass in the raw materials.
[0135] Comparative Example 3: The difference between this comparative example and Example 1 is that:
[0136] No fire-resistant paper is added to the fire-resistant cable.
[0137] Performance testing
[0138] 1. Flexible detection
[0139] Fire-resistant paper was prepared by the preparation methods of fire-resistant materials for cables according to Examples 1-8, 11 and Comparative Example 2, and the longitudinal softness of the fire-resistant paper was tested using a softness tester (purchased from Jinan Hengfengyuan Instrument Co., Ltd., model HFY-207), and the data was recorded.
[0140] 2. Tear resistance test
[0141] Fire-resistant paper was prepared by the preparation method of fire-resistant material for cable according to Examples 1-11 and Comparative Example 1 respectively, and the tensile strength was tested by a computer tensile tester (the computer tensile tester was purchased from Jinan Alpha Electronic Equipment Co., Ltd., model XLW-PC). The computer tensile tester detected the tensile strength, which is equal to the tensile strength. The greater the tensile strength, the better the tear resistance. The data was recorded.
[0142] 3. Length detection
[0143] Ultra-long hydroxyapatite nanowires were prepared by the preparation methods of fireproof materials for cables in Examples 1-7 respectively, and the average length was observed and measured using a scanning electron microscope (Hitachi scanning electron microscope, model FlexSEM 1000 II purchased from Shanghai Xinu Optical Technology Co., Ltd.) to record the data.
[0144] 4. Fire resistance test
[0145] Refractory paper was prepared by the preparation methods of fire-resistant materials for cables according to Examples 1-3, 9-10, 12 and Comparative Example 2, and the refractory paper was heated at 1000°C using an alcohol burner. The alcohol burner nozzle was 10 cm away from the surface of the refractory paper. Heating was stopped after 1 min. If there was any burning after stopping heating, the fire should be extinguished immediately. Finally, the surface integrity of the refractory paper was observed and the proportion of the burning area to the total area was recorded. The larger the burning proportion, the larger the burning area and the worse the integrity.
[0146] 5. Water resistance test
[0147] The fire-resistant paper was prepared by the preparation method of the fire-resistant material for cables in Examples 1-3, 8-10 and 12 respectively, the contact angle was tested and the data was recorded; and the fire-resistant paper was completely immersed in water for 48 hours. After the fire-resistant paper was taken out, the tensile strength was tested again using a computer tensile tester (the computer tensile tester was purchased from Jinan Alpha Electronic Equipment Co., Ltd., model XLW-PC) and the data was recorded.
[0148] Table 1 Performance test table (“ / ” in the following table means that the corresponding embodiment or comparative example did not test the item, so there is no data)
[0149]
[0150] From Examples 1-3 and Table 1, it can be seen that the hydroxyapatite nanowire filaments prepared in the present application have the advantage of being super long, so that the prepared refractory paper has good softness and good tear resistance, as well as good fire resistance, a large contact angle, and a small loss of strength after immersion, indicating good water resistance. After being prepared into a cable, it can give the cable good fire resistance. Even if a fire occurs, it can buy time for personnel evacuation and fire rescue. During the preparation process, the refractory paper can be attached to the surface of the conductor, and combined with its good mechanical properties, the service life of the fire-resistant cable can be further extended.
[0151] Combining Example 1 and Examples 4-12 and Table 1, it can be seen that in the preparation process of hydroxyapatite nanowire filaments in Example 4, the chitosan-loaded calcium chloride is replaced by an equal mass of calcium chloride, and the tyrosine-loaded sodium dihydrogen phosphate is replaced by an equal mass of sodium dihydrogen phosphate. Compared with Example 1, the refractory paper prepared in Example 4 has poorer flexibility than that in Example 1, lower tensile strength than that in Example 1, and the length of the prepared hydroxyapatite nanowire filaments is lower than that in Example 1; this indicates that the hydroxyapatite nanowire filaments prepared by the reaction of ordinary calcium chloride and sodium dihydrogen phosphate are shorter in length, while the hydroxyapatite nanowires prepared by the combination of chitosan-loaded calcium chloride and tyrosine-loaded sodium dihydrogen phosphate are longer in length and have better strength.
[0152] In the preparation process of hydroxyapatite nanowire filaments in Example 5, sodium hydroxide solution is first added. Compared with Example 1, the flexibility of the refractory paper prepared in Example 5 is worse than that in Example 1, the tensile strength is lower than that in Example 1, and the length of the prepared hydroxyapatite nanowire filaments is shorter than that in Example 1; it indicates that the sodium hydroxide solution is added after the hydroxyapatite nuclei and short hydroxyapatite nanowires are formed, and chitosan and tyrosine are both negatively charged, and their repulsive effect is utilized to prevent the hydroxyapatite nanowires from agglomerating with each other and affecting the growth of the hydroxyapatite nanowires; and the released sodium dihydrogen phosphate cooperates with calcium chloride to continue to grow at both ends of the short hydroxyapatite nanowires to form hydroxyapatite nanowire filaments; at the same time, sodium hydroxide can promote the directional growth of hydroxyapatite nanowires, so that the generated hydroxyapatite nanowire filaments have the advantages of ultra-long, good flexibility, uniform morphology, and not prone to cracks and gaps, thereby ensuring the flexibility and tear resistance of the hydroxyapatite nanowire filaments, thereby ensuring that the refractory paper has good flexibility and tear resistance.
[0153] In the preparation process of chitosan-loaded calcium chloride for hydroxyapatite nanowire filaments in Example 6, chitosan was not soaked in calcium chloride solution. Compared with Example 1, the flexibility of the refractory paper prepared in Example 6 was worse than that in Example 1, the tensile strength was lower than that in Example 1, and the length of the prepared hydroxyapatite nanowire filaments was shorter than that in Example 1; this indicates that the soaking treatment causes the calcium chloride to be loaded inside the chitosan pores. After the crystal nuclei and short hydroxyapatite nanowires are formed, the sodium hydroxide solution disintegrates the chitosan structure, releasing calcium chloride, which further promotes the growth of hydroxyapatite nanowires. The ultra-long hydroxyapatite nanowires have good flexibility, thereby improving the flexibility and tear resistance of the refractory paper.
[0154] In the preparation process of chitosan-loaded calcium chloride for hydroxyapatite nanowire filaments in Example 7, chitosan was only immersed in a calcium chloride solution, and calcium chloride was not bonded to the surface. Compared with Example 1, the flexibility of the refractory paper prepared in Example 7 was worse than that in Example 1, and the tensile strength was lower than that in Example 1. The length of the prepared hydroxyapatite nanowire filaments was lower than that in Example 1. This indicates that calcium chloride loaded on the surface of chitosan can ensure the first formation of crystal nuclei and short hydroxyapatite nanowires, and then further react with the calcium chloride loaded in the chitosan pores to form ultra-long hydroxyapatite nanowires, thereby ensuring the flexibility and tear resistance of the refractory paper.
[0155] The titanium dioxide whiskers in Example 8 are ordinary commercially available silicon dioxide whiskers that have not been treated with tyrosine and shellac. Compared with Example 1, the refractory paper prepared in Example 8 has lower flexibility and worse tear resistance than Example 1, and the tensile strength loss value after immersion is greater than the corresponding tensile strength loss value of Example 1; this indicates that the silicon dioxide whiskers have been modified with tyrosine and shellac, and the negative charge of hydroxyapatite nanowire filaments is utilized to repel the negative charge of tyrosine, so that the titanium dioxide whiskers and hydroxyapatite nanowire filaments are evenly dispersed, and the pore structure produced by the even dispersion ensures the soft foldability of the refractory paper, and the mechanical strength of the titanium dioxide whiskers and shellac are utilized to further improve the tear resistance of the refractory paper and extend the service life of the refractory paper.
[0156] During the preparation of the adhesive in Example 9, no nanoparticles were added. Compared with Example 1, the fire-resistant paper prepared in Example 9 had lower tensile strength than that in Example 1, a greater combustion ratio than that in Example 1, a smaller contact angle than that in Example 1, and a tensile strength loss value after immersion than the corresponding tensile strength loss value in Example 1. This shows that the addition of nanoparticles can not only increase the tensile strength, but also improve the fire resistance and water resistance.
[0157] During the preparation of the adhesive in Example 10, no polyethylene glycol solution was added. Compared with Example 1, the combustion ratio of the fire-resistant paper prepared in Example 10 was greater than that in Example 1, the contact angle was smaller than that in Example 1, and the tensile strength loss value after immersion was greater than the tensile strength loss value corresponding to Example 1; this indicates that polyethylene glycol can not only improve the bonding stability between the nanowire mixture and the aluminum silicate fiber and improve the tear resistance, but also can cooperate with aminosulfonic acid to form sulfonate esters and improve water resistance.
[0158] During the preparation of the adhesive in Example 11, sodium polyacrylate-coated calcium hydroxide was not added. Compared with Example 1, the fire-resistant paper prepared in Example 11 was less soft than that in Example 1, and its tensile strength was less than that in Example 1; this indicates that sodium silicate and calcium hydroxide react to generate calcium silicate precipitate and sodium hydroxide; the calcium silicate precipitate not only has good high temperature resistance and fire resistance, but also has good water resistance, and the sodium hydroxide solution is convenient for dissolving shellac and tyrosine, so that the position originally occupied by the titanium dioxide whiskers is reduced, and the pores around the titanium dioxide whiskers are increased, which further increases the connection pores between the titanium dioxide fibers and the hydroxyapatite nanowire filaments, thereby improving the flexibility of the finished fire-resistant paper and, at the same time, utilizing its filling effect to improve the tear resistance.
[0159] The aluminum silicate fiber in Example 12 is ordinary commercially available aluminum silicate fiber, which has not been ground with aminosulfonic acid particles. Compared with Example 1, the combustion ratio of the fire-resistant paper prepared in Example 12 is greater than that in Example 1, the contact angle is smaller than that in Example 1, and the tensile strength loss value after immersion is greater than the tensile strength loss value corresponding to Example 1; this indicates that aminosulfonic acid can cross-link with the polyethylene glycol solution in the adhesive to form sulfonate esters, which not only have good fire resistance, but also have good water resistance, thereby extending the service life of the fire-resistant paper.
[0160] It can be seen from Example 1 and Comparative Examples 1-2 and Table 1 that no titanium dioxide whiskers are added to the raw materials of Comparative Example 1. Compared with Example 1, the tensile strength of the refractory paper prepared in Comparative Example 1 is lower than that in Example 1, indicating that the addition of titanium dioxide whiskers can improve the tear strength of refractory paper.
[0161] In Comparative Example 2, the nanowire mixture is replaced with bamboo fiber of equal mass in the raw materials. Compared with Example 1, the fire-resistant paper prepared in Comparative Example 2 has higher softness, but poor fire resistance and completely burns at high temperature.
[0162] 6. Cable fire resistance test
[0163] Fire-resistant cables were prepared by the preparation methods of Examples 1-3 and Comparative Example 3, respectively. The cables were burned for 60 minutes under heating conditions with an alcohol burner at a temperature of 1000°C and a distance of 5 cm between the alcohol burner and the cable. It was then recorded whether the cables maintained normal conductivity.
[0164] Table 2 Fire resistant cable test table
[0165]
[0166] Combining Examples 1-3 and Comparative Example 3 with Table 2, it can be seen that after being heated by an alcohol burner, the wires in the cable are not easily burned and can conduct electricity normally, indicating that the fire-resistant cable has good fire resistance after being coated with fire-resistant paper.
[0167] Second aspect: The present application discloses a fire-resistant cable.
[0168] See attached Figure 1 -Attached Figure 3 A fire-resistant cable comprises a conductor 1, the outer side of the conductor 1 is coated with a layer of fire-resistant paper 2, wherein the fire-resistant paper 2 disclosed in this embodiment is prepared by the preparation method of the fire-resistant material for cables disclosed in the above embodiment. A silicone rubber layer 3, an armor layer 4 and an outer sheath 5 are sequentially arranged on the outer side of the fire-resistant layer.
[0169] The silicone rubber layer 3 is fireproof silicone rubber, the armor layer 4 is sleeved on the outside of the silicone rubber layer 3, the silicone rubber layer 3 is hollow and forms an air storage cavity 6, a plurality of partition plates 7 are evenly arranged in the inner cavity of the air storage cavity 6, and the plurality of partition plates 7 divide the air storage cavity 6 into a plurality of mutually unconnected sub-cavities 8. The material of the partition plates 7 is also silicone rubber. The silicone rubber layer 3 with the partition plates 7 can be manufactured by splicing processing or mold processing.
[0170] In each sub-chamber 8, a flame retardant gas 9 is filled by injection ventilation. When the cable encounters an open flame, in order to prevent the entire cable or part of the cable from being burned, when the open flame melts or leaks the sub-chamber 8, the flame retardant gas 9 is quickly released to block the burning part, thereby reducing the loss. In this embodiment, the flame retardant gas 9 is carbon dioxide or nitrogen.
[0171] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.
Claims
1. A method for preparing a fireproof material for a cable, characterized in that: The fireproof material for the cable is fireproof paper, and the preparation method of the fireproof paper comprises the following steps: Ⅰ. Mixing hydroxyapatite nanowire filaments and titanium dioxide whiskers uniformly at a mass ratio of 1:0.05-0.1 to obtain a nanowire mixture; Ⅱ. Dispersing aluminum silicate fibers uniformly in water to prepare a suspension; III. Add the nanowire mixture to the suspension, disperse it evenly, add the adhesive, stir it evenly to obtain a slurry, filter it, shape it, squeeze it, dry it, and make it into a finished product; the hydroxyapatite nanowire filaments are prepared by the following method: Water, ethanol and oleic acid are mixed and stirred evenly in a mass ratio of 22:3-6:4-8 to obtain a primary mixture; chitosan-loaded calcium chloride and tyrosine-loaded sodium dihydrogen phosphate are added to the primary mixture, the mass ratio of water, chitosan-loaded calcium chloride and tyrosine-loaded sodium dihydrogen phosphate is 22:2.5-2.8:5-5.6, the mixture is mixed and stirred for 10-20 minutes, sealed, reacted at 180-190°C for 14-16 hours, and then sodium hydroxide solution is added, the mass ratio of water to sodium hydroxide solution is 22:7-9, mixed and stirred evenly, sealed, and then the reaction is continued for 8-10 hours. After cooling, hydroxyapatite nanowire filaments are obtained by precipitation, washing and filtering.
2. The method for preparing a fireproof material for cables according to claim 1, characterized in that: The chitosan-loaded calcium chloride is prepared by the following method: Chitosan is immersed and stirred in a calcium chloride solution with a mass fraction of 0.4-0.6% at a mass ratio of 1:0.5-1, and then freeze-dried to obtain loaded chitosan; polyethylene glycol solution is evenly sprayed on the surface of the loaded chitosan, and then calcium chloride powder is added, the mass ratio of the loaded chitosan to the polyethylene glycol solution and the calcium chloride powder is 1:0.1-0.22:0.2-0.35, and the finished product is obtained after drying and dispersion.
3. The method for preparing a fireproof material for cables according to claim 1, characterized in that: The tyrosine-loaded sodium dihydrogen phosphate is prepared by the following method: The polyethylene glycol solution is evenly sprayed on the surface of the tyrosine particles at a mass ratio of 1:0.4-0.55, and then sodium dihydrogen phosphate is added, and the mass ratio of tyrosine particles to sodium dihydrogen phosphate is 1:0.6-0.
85. After drying and dispersion, a finished product is obtained.
4. The method for preparing a fireproof material for cables according to claim 1, characterized in that: The titanium dioxide whiskers are prepared by the following method: The titanium dioxide whisker is dispersed in ethanol, and then tyrosine is added, and the dispersion is continued. After uniform mixing, shellac is added and mixed uniformly. The mass ratio of the titanium dioxide whisker to tyrosine and shellac is 1:0.1-0.3:0.1-0.
2. After drying and dispersion, a finished product is obtained.
5. The method for preparing a fireproof material for cables according to claim 1, characterized in that: The adhesive is prepared by the following method: Sodium silicate is placed in water at a mass ratio of 1:15-25 and stirred until it is completely dissolved to obtain a dissolving solution; nanoparticles and polyethylene glycol solution are added to the dissolving solution, the mass ratio of sodium silicate to nanoparticles and polyethylene glycol solution is 1:0.1-0.2:0.2-0.5, and the mixture is stirred evenly; finally, sodium polyacrylate coated calcium hydroxide is added, the mass ratio of sodium silicate to sodium polyacrylate coated calcium hydroxide is 1:0.1-0.3, and the mixture is stirred evenly to obtain an adhesive.
6. The method for preparing a fireproof material for cables according to claim 5, characterized in that: The nanoparticles are composed of fumed silicon dioxide and boron nitride in a mass ratio of 1:0.5-1.
7. The method for preparing a fireproof material for cables according to claim 5, characterized in that: The sodium polyacrylate coated calcium hydroxide is made of a sodium polyacrylate solution and calcium hydroxide particles in a mass ratio of 1:0.5-1.
8. The method for preparing a fireproof material for cables according to claim 1, characterized in that: After adding the adhesive to the III, stir for 20-30 minutes, then heat to 70-85°C and continue stirring for 5-10 minutes.
9. The method for preparing a fireproof material for a cable according to claim 1, characterized in that: The aluminum silicate fiber is prepared by the following method: The aluminum silicate fiber filaments are mixed and ground with aminosulfonic acid particles, and then the aluminum silicate fiber filaments are filtered and sieved to obtain aluminum silicate fibers.
10. A fire-resistant cable, comprising a conductor (1), the outer side of the conductor (1) being coated with a layer of fire-resistant paper (2), wherein: The fire-resistant paper (2) is prepared by the method for preparing fire-resistant materials for cables according to any one of claims 1 to 9, and a silicone rubber layer (3), an armor layer (4) and an outer sheath (5) are sequentially arranged on the outside of the fire-resistant paper (2).
11. The fire-resistant cable according to claim 10, characterized in that: The silicone rubber layer (3) is hollow and forms a gas storage cavity (6), the inner cavity of the gas storage cavity (6) is filled with flame-retardant gas (9), and a plurality of partition plates (7) are evenly spaced in the inner cavity of the gas storage cavity (6), and the plurality of partition plates (7) divide the gas storage cavity (6) into a plurality of mutually unconnected sub-cavities (8).
Citation Information
Patent Citations
Water-based expansive type nano fireproof coating for cable and preparation method thereof
CN103740231A
Environment-friendly type fire-resistant and flame-retardant package for cable well
CN109054867A
Flame-retardant polyvinyl chloride insulation fireproof power cable
CN112820462A
Composite fire-resistant fireproof cable and preparation method thereof
CN112908524A