High performance heat-resistant concrete and preparation method thereof

Through microwave-assisted acid activation of sepiolite, nano-alumina filling and the combination of modified sepiolite and siloxane, the problem of high water absorption of sepiolite affecting the hardening of concrete has been solved, and the preparation of high-performance heat-resistant concrete has been achieved. Significantly improves thermal and mechanical properties and extends the survival rate of microbial remediation agents.

CN118515457BActive Publication Date: 2024-10-01禹城市霞光建筑材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410989336.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-01
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The high water absorption of sepiolite affects the hardening and strength of concrete, reduces the hydration rate of cement and the production of cementitious substances, resulting in a decrease in the mechanical properties of concrete.

Method used

The sepiolite is surface treated with a microwave-assisted acid activator to remove surface impurities and form nano-alumina to fill the pores of the sepiolite. The modified sepiolite is mixed with siloxane and expanded perlite to form an aerogel, and the nanoparticles are deposited to In the pores of the glass fiber, the microbial repair agent rice husk powder is loaded as the core material to form a microcapsule repair agent to improve the heat resistance and mechanical properties of the concrete.

Benefits of technology

It significantly improves the heat resistance and mechanical properties of concrete, avoids incomplete cement hydration caused by sepiolite's easy water absorption, prolongs the survival rate of microbial remediation agents, and improves the water resistance and toughness of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a high-performance heat-resistant concrete and a preparation method thereof, which belongs to the technical field of concrete processing, and comprises the following steps: using a microwave-assisted acid activator to surface-treat sepiolite to obtain pretreated sepiolite; mixing modified sepiolite, siloxane and expanded perlite to obtain composite aerogel; depositing nanoparticles into the pores of glass fibers to obtain modified glass fibers as capsule materials, and loading microbial repair agent rice husk powder as core materials to prepare microcapsule repair agents; mixing cement, basalt gravel, river sand, fly ash, mineral powder, microcapsule repair agents, composite aerogels, water reducers and water, and stirring to obtain heat-resistant concrete. A cobalt silicate layer is synthesized in situ on the surface of nano-alumina-loaded sepiolite, which is insoluble in water and has excellent water resistance, thereby avoiding the sepiolite from easily absorbing water, resulting in incomplete cement hydration, and reducing the mechanical properties of concrete, and the cobalt silicate layer can prevent water penetration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete processing, in particular to high-performance heat-resistant concrete and a preparation method thereof. Background Art

[0002] Concrete refers to a composite material in which aggregates are bonded into a whole by cementitious materials. It is made by mixing cement as the cementitious material, sand and stone as aggregates, with water, admixtures and additives in a certain proportion. Concrete has the advantages of wide application range, low price and easy casting and molding. Concrete is an important hydraulic construction and building material; high-performance concrete has the characteristics of ultra-high strength, high toughness and excellent durability, and has very broad application prospects in the fields of bridges, building structures, etc.; by mixing refractory materials and heat-resistant materials with cement matrix, the prepared concrete is suitable for thermal equipment in industries such as metallurgy, chemical industry, petroleum, light industry and building materials, and structures subjected to high temperature for a long time, such as the lining of industrial chimneys or flues, the refractory lining of industrial kilns, and the foundation and shell of high-temperature boilers.

[0003] High-performance concrete generally has excellent working performance, high strength and good durability, which can effectively improve construction quality and extend the service life of concrete components; sepiolite is a fibrous hydrated magnesium silicate with good heat resistance and can improve the heat resistance of concrete, but sepiolite has a high water absorption rate and will absorb moisture in the concrete, reduce the hydration rate of cement and the production of cementitious substances, and affect the hardening and strength of the concrete. Summary of the invention

[0004] The purpose of the present invention is to provide a high-performance heat-resistant concrete and a preparation method thereof: microwave-assisted acid activator surface treatment of sepiolite, so that free metal ions magnesium ions in the sepiolite structure are replaced and precipitated, surface impurities are removed, and the reaction of metal magnesium ions with calcium silicate of cement is avoided to cause the mechanical properties of concrete to decrease; pre-treated sepiolite is mixed with cobalt source and aluminum source, and after high-temperature heat treatment, an alumina precursor is formed in the pores of the sepiolite to form nano-alumina to fill the pores of the sepiolite, refine the pore size, improve the heat resistance, and then after high-temperature calcination, a cobalt silicate layer is synthesized in situ on the surface of the nano-alumina-loaded sepiolite, wherein the cobalt silicate is insoluble in water and has excellent water resistance, thereby avoiding seawater stagnation. Sepiolite easily absorbs water, resulting in incomplete cement hydration; modified sepiolite, siloxane and expanded perlite are mixed to form an aerogel with good heat resistance, and the gel and modified sepiolite are adsorbed in the pores of the expanded perlite, so that the expanded perlite is converted from hydrophilic to hydrophobic, and has excellent water resistance; nanoparticles are deposited in the pores of glass fibers as capsule materials, and rice husk powder, a microbial repair agent, is loaded as a core material to provide a living space for concrete repair bacteria to avoid inactivation of the bacteria due to the high alkaline environment of concrete, and glass fiber and rice husk powder are used as microcapsule wall materials, which have a synergistic effect in heat resistance, so that the microbial repair agent has a good survival rate at high temperatures.

[0005] Technical problems to be solved by the present invention: High-performance concrete generally has excellent working performance, high strength and good durability, which can effectively improve the construction quality and extend the service life of concrete components; sepiolite is a fibrous hydrated magnesium silicate with good heat resistance and can improve the heat resistance of concrete, but sepiolite has a high water absorption rate and will absorb moisture in concrete, reduce the hydration rate of cement and the production of gelling substances, and affect the hardening and strength of concrete.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing high-performance heat-resistant concrete comprises the following steps:

[0008] S1. The surface of sepiolite was treated with a microwave-assisted acid activator, and the pretreated sepiolite was obtained by grinding;

[0009] Furthermore, the microwave heating temperature is 70-100°C.

[0010] More preferably, the microwave heating temperature is 80°C.

[0011] Furthermore, the acid activator is selected from hydrochloric acid and sulfuric acid.

[0012] Further preferably, the acid activator is selected from hydrochloric acid.

[0013] Furthermore, the acid activator has a concentration of 0.5-1.5 mol / L.

[0014] More preferably, the acid activator has a concentration of 1 mol / L.

[0015] Furthermore, the sepiolite has a particle size of 0.3-1.5 μm and a pore size of 50-100 nm.

[0016] More preferably, the sepiolite has a particle size of 0.3-1 μm and a pore size of 50-80 nm.

[0017] More preferably, the sepiolite has a particle size of 0.5 μm and a pore size of 70 nm.

[0018] Further, the pretreated sepiolite is prepared by the following steps:

[0019] Place the sepiolite in a three-necked flask, add an acid activator with a concentration of 1 mol / L, stir evenly, place in a microwave oven, heat to 80°C, stir for 2 hours, cool to room temperature, wash with anhydrous ethanol 3 times, wash with deionized water until the washing liquid is neutral, dry in a 60°C oven for 10 minutes, and grind in a grinder to obtain pretreated sepiolite.

[0020] Among them, microwave-assisted acid activation of sepiolite is carried out. The sepiolite is treated with an acid activator, hydrochloric acid, so that the free metal ions magnesium ions in the sepiolite are replaced and precipitated, and surface impurities are removed to avoid the reaction of metal magnesium ions with calcium silicate of cement, which leads to a decrease in the mechanical properties of concrete. The internal pores of the sepiolite are opened, and the porous structure can adsorb aluminum chloride, a precursor of alumina, refine the pore size, and improve the heat resistance.

[0021] Furthermore, the dosage ratio of sepiolite to acid activator is (5.5-6.5) g:(40-60) mL.

[0022] S2. The modified sepiolite, siloxane and expanded perlite are mixed to obtain a composite aerogel;

[0023] Furthermore, the siloxane is selected from one of tetraethyl orthosilicate, trimethylchlorosilane, hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane.

[0024] More preferably, the siloxane is selected from one of tetraethyl orthosilicate, trimethylchlorosilane, hexamethylcyclotrisiloxane and octamethylcyclotetrasiloxane.

[0025] More preferably, the siloxane is selected from ethyl orthosilicate.

[0026] Furthermore, the expanded perlite has a particle size of 0.5-5 mm and a pore size of 0.5-2.5 μm.

[0027] More preferably, the expanded perlite has a particle size of 0.5-2.5 mm and a pore size of 0.5-2 μm.

[0028] More preferably, the expanded perlite has a particle size of 1.5 mm and a pore size of 1.3 μm.

[0029] Further, the composite aerogel is prepared by the following steps:

[0030] Siloxane, ethanol and deionized water were mixed and stirred evenly, modified sepiolite and hydrochloric acid with a mass fraction of 36% were added for acid-base titration to promote the hydrolysis reaction, and stirred for 30 minutes to obtain a gel solution, the gel solution was mixed with expanded perlite, vacuum adsorbed under a vacuum negative pressure of -0.08MPa, aged at 30°C for 4h, and dried in an oven at 90°C for 10min to obtain a composite aerogel;

[0031] Among them, ethyl orthosilicate is hydrolyzed and condensed to form a cross-linked network silica gel, and the cobalt silicate layer contained on the surface of the modified sepiolite has good compatibility with the silica gel, so that the modified sepiolite is dispersed in the silica gel. Under vacuum negative pressure, the gel and the modified sepiolite are adsorbed in the pores of the expanded perlite, so that the expanded perlite is converted from hydrophilic to hydrophobic, and has excellent water resistance. The sepiolite is filled into the pores of the expanded perlite, the porosity is increased, and the heat resistance is improved. The silica gel contained on the surface is combined with the cement particles through chemical bonds, so that the composite material is dispersed in the concrete matrix.

[0032] Furthermore, the dosage ratio of siloxane, ethanol, deionized water, and modified sepiolite is (1-2) g: (7-8) mL: (10-20) mL: (0.3-0.7) g.

[0033] Furthermore, the modified sepiolite is prepared by mixing the pretreated sepiolite with a cobalt source and an aluminum source, subjecting the pretreated sepiolite to high temperature heat treatment, and then subjecting the pretreated sepiolite to high temperature calcination.

[0034] Furthermore, the cobalt source is selected from one of cobalt nitrate hexahydrate, cobalt chloride, cobalt acetate, cobalt hydroxide, cobalt oleate, cobalt linoleate, cobalt octoate, cobalt stearate, cobalt phosphate, and cobalt sulfate.

[0035] More preferably, the cobalt source is selected from cobalt nitrate hexahydrate, cobalt chloride, cobalt hydroxide, cobalt phosphate and cobalt sulfate.

[0036] More preferably, the cobalt source is selected from cobalt nitrate hexahydrate, cobalt chloride and cobalt phosphate.

[0037] Further preferably, the cobalt source is selected from cobalt nitrate hexahydrate.

[0038] Furthermore, the aluminum source is selected from aluminum chloride, aluminum nitrate, and aluminum hydroxide.

[0039] More preferably, the aluminum source is selected from aluminum chloride and aluminum nitrate.

[0040] Further preferably, the aluminum source is selected from aluminum chloride.

[0041] Furthermore, the high temperature heat treatment temperature is 400-600°C and the time is 1-3h.

[0042] More preferably, the high temperature heat treatment temperature is 500° C. and the time is 2 hours.

[0043] Furthermore, the high temperature calcination temperature is 800-1000° C., and the calcination time is 2-5 hours.

[0044] More preferably, the high temperature calcination temperature is 900° C. and the calcination time is 3 h.

[0045] Further, the modified sepiolite is prepared by the following steps:

[0046] A1. Add urea and aluminum source aluminum chloride to deionized water, stir evenly, add pretreated sepiolite, ultrasonically treat for 30 minutes, stir and react at 120°C for 2 hours, cool to room temperature, filter, wash with deionized water 3 times, place in a 60°C oven to dry for 10 minutes, place in a high-temperature reactor, heat treat at 500°C for 2 hours, cool to room temperature, and obtain loaded nano-alumina sepiolite.

[0047] Among them, aluminum chloride is used as an aluminum source and urea is used as a precipitant. Aluminum hydroxide crystal nuclei are generated in a hydrothermal environment and deposited into the pores of the pretreated sepiolite, and in-situ growth is carried out in the pores of the pretreated sepiolite. After high-temperature treatment at 500°C, the aluminum hydroxide in the pores of the sepiolite is decomposed to produce nano-alumina with a particle size of 10-40nm, which fills the pores of the sepiolite, refines the pore size, and improves the heat resistance. The formed nano-alumina has a small size effect, high toughness and high temperature resistance.

[0048] Furthermore, the usage ratio of urea, aluminum source and pretreated sepiolite is (1-2) g:(2-3) g:(2.4-2.8) g.

[0049] A2. Add cobalt source, ammonium fluoride and urea to deionized water, stir for 30 minutes, add loaded nano-alumina sepiolite, place in an autoclave, heat treat at 120°C for 5 hours, cool to room temperature, wash the solid product with deionized water 3 times, ethanol 5 times, dry in an oven at 60°C for 10 minutes, place in a Ma furnace, calcine at 900°C for 3 hours, cool to room temperature, and obtain modified sepiolite.

[0050] Among them, the nano-alumina-loaded sepiolite is mixed with cobalt-source cobalt nitrate hexahydrate, and through a hydrothermal reaction, the cobalt-source cobalt nitrate hexahydrate undergoes dehydroxylation and decarbonization reactions to form cobalt oxide, which is then calcined at 900°C. The nano-alumina-loaded sepiolite is fibrous, and its main component is silicon dioxide, so that the formed cobalt oxide can react with silicon dioxide in the sepiolite, and combine with silicon-oxygen-cobalt bonds to form cobalt silicate, thereby realizing the in-situ synthesis of a cobalt silicate layer on the surface of the nano-alumina-loaded sepiolite. Cobalt silicate is insoluble in water and has excellent water resistance, which prevents the sepiolite from absorbing water easily, resulting in incomplete cement hydration and reducing the mechanical properties of the concrete.

[0051] Furthermore, the usage ratio of the cobalt source and the loaded nano-alumina sepiolite is (0.1-0.3) g:(0.1-0.2) g.

[0052] S3. Depositing nanoparticles into the pores of glass fibers to obtain modified glass fibers as capsule materials, and loading microbial remediation agent rice husk powder as core materials to prepare microcapsule remediation agents;

[0053] Furthermore, the glass fiber has a length of 1.5-2.5 μm and a diameter of 0.1-0.3 μm.

[0054] More preferably, the glass fiber has a length of 2.3 μm and a diameter of 0.2 μm.

[0055] Furthermore, the nanoparticles are selected from any one of nano-silicon dioxide, nano-zirconium dioxide, nano-titanium dioxide, nano-calcium oxide, and nano-diatomaceous earth.

[0056] Furthermore, the particle size of the nanoparticles is 20-50 nm.

[0057] More preferably, the particle size of the nanoparticles is 20-40 nm.

[0058] More preferably, the particle size of the nanoparticles is 30 nm.

[0059] Further, the microcapsule repair agent is prepared by the following steps:

[0060] B1. Add nanoparticles to ethanol and stir evenly to obtain a dispersion. Immerse glass fiber in the dispersion and stir for 30 minutes to allow the nanoparticles to be adsorbed on the surface and pores of the glass fiber. Place in an oven at 80°C for drying to volatilize the organic solvent ethanol to obtain modified glass fiber.

[0061] Among them, the slag fiber is impregnated into the nanoparticle dispersion, so that the nanoparticles are adsorbed on the surface and pores of the glass fiber. The nanoparticles can absorb the stress generated during the stirring process, improve the toughness of the glass fiber, and avoid the brittleness of the glass fiber causing the repair agent to be released prematurely and lose its self-repairing properties.

[0062] Furthermore, the dosage ratio of nanoparticles and ethanol slag fiber is (0.3-0.7) g: (25-35) mL: (0.5-0.6) g.

[0063] B2. Add epoxy resin and modified glass fiber to ethanol, stir, add polyethylene glycol diglycidyl ether, stir at 50°C for 10 minutes, after the reaction is completed, add rice husk powder loaded with microbial repair agent, stir for 30 minutes to form a gel, filter, wash with deionized water 3 times, and dry in an oven at 80°C for 10 minutes to obtain a microcapsule repair agent.

[0064] Among them, the epoxy group of the epoxy resin reacts with the hydroxyl group on the surface of the glass fiber, so that the modified glass fiber is dispersed in the epoxy resin matrix. Under the action of the cross-linking agent polyethylene glycol diglycidyl ether, a microcapsule repair agent with rice husk powder as the core material and modified glass fiber as the capsule material is formed, which provides a living space for concrete repair bacteria and avoids the inactivation of the bacteria due to the high alkaline environment of the concrete. In addition, the glass fiber and rice husk powder as microcapsule wall materials have a synergistic effect in heat resistance, which makes the microbial repair agent have a better survival rate at high temperatures.

[0065] Furthermore, the epoxy resin is selected from any one of epoxy resin EP-301, epoxy resin EP-360, and epoxy resin EP-365.

[0066] Furthermore, the usage ratio of epoxy resin, modified glass fiber, polyethylene glycol diglycidyl ether, and rice husk powder loaded with microbial remediation agent is (3-4) g: (2-3) g: (0.3-0.7) g: (2-2.6) g.

[0067] Furthermore, the rice husk powder loaded with the microbial remediation agent is prepared by adsorbing the microbial remediation agent on the rice husk powder.

[0068] Furthermore, the rice husk powder has a particle size of 2-5 μm and a pore size of 10-40 nm.

[0069] More preferably, the rice husk powder has a particle size of 2-4 μm and a pore size of 10-30 nm.

[0070] More preferably, the rice husk powder has a particle size of 3.5 μm and a pore size of 20 nm.

[0071] Furthermore, the microbial repair agent is selected from any one of Bacillus pseudofirmus, Nitrobacter, Bacillus, and Bacillus subtilis.

[0072] Furthermore, the rice husk powder loaded with microbial remediation agent is prepared by the following steps:

[0073] The rice husk was washed three times with deionized water, dried, added to a 5% hydrochloric acid solution, heated at 100°C for 3 hours, filtered, washed three times with deionized water, placed in a muffle furnace, and heated at 600°C for 4 hours to obtain rice husk ash. The microbial remediation agent was added to the culture medium and cultured at 30°C for 12 hours to obtain a bacterial solution. The rice husk ash and the bacterial solution were mixed, and the bacterial solution was adsorbed in the pores of the rice husk ash under a pressure of -0.06MPa. The solution was dried at 40°C for 10 minutes to obtain rice husk powder loaded with a microbial remediation agent.

[0074] The rice husk is washed with hydrochloric acid to remove surface impurities and calcined at 600°C, causing the rice husk containing a large amount of crude fiber, lignin, silica, carbon and other components to undergo pyrolysis reaction, generate gas and release it to form a porous structured rice husk ash. Under a negative pressure of -0.06MPa, the microbial remediation agent can be adsorbed into the rice husk ash, protecting the bacteria from damage and prolonging the survival time of the bacteria.

[0075] Furthermore, the culture medium is mixed with sucrose, yeast flavor, dipotassium hydrogen phosphate, calcium chloride, potassium chloride, magnesium sulfate, and manganese sulfate in a dosage ratio of (3.3-3.7) g:(3-5) g:(0.01-0.03) g:(0.15-0.19) g:(0.3-0.5) g:(0.1-0.3) g:(0.2-0.4) g.

[0076] Furthermore, the dosage ratio of rice husk ash and bacterial solution is (5-5.6) g: (15-25) mL.

[0077] S4. Mix cement, basalt crushed stone, river sand, fly ash, mineral powder, microcapsule repair agent, composite aerogel, water reducing agent and water.

[0078] Furthermore, the cement is silicate cement with a PO4 of 2.5 and a specific surface area of ​​386.5 m 2 / kg, and the compressive strength at 28d is 56.3MPa.

[0079] Furthermore, the basalt crushed stone is continuously graded from 5 to 25 mm and has a mud content of 0.2%.

[0080] Furthermore, the apparent density of river sand is 2680kg / m 3 The fineness modulus is 2.4, the particle size is 3.5mm, and the mud content is 0.9%.

[0081] Furthermore, the fly ash is Class F Grade I fly ash, the fineness of the fly ash is 45 μm, the loss on ignition is 2.8%, and the water content is 0.15%.

[0082] Furthermore, the mineral powder is S95 grade slag powder with a density of 2.9g / cm 3 , with a specific surface area of ​​450m2 / kg, water content is 0.2%, and 28d activity index is 95%.

[0083] Furthermore, the water reducer is PCE-102 polycarboxylate water reducer.

[0084] Furthermore, compared with the prior art, the present invention has the following beneficial effects:

[0085] (1) In the technical scheme of the present invention, microwave-assisted acid activation of sepiolite is performed. The sepiolite is treated with an acid activator, hydrochloric acid, so that the free metal ions magnesium ions in the sepiolite structure are replaced and precipitated, and surface impurities are removed to avoid the reaction of metal magnesium ions with calcium silicate of cement, which leads to a decrease in the mechanical properties of concrete. The porous structure of the sepiolite absorbs aluminum chloride, an alumina precursor, and the alumina precursor is adsorbed in the pores of the sepiolite. After high-temperature sintering at 600°C, the alumina precursor forms nano-alumina in the pores of the sepiolite, with a particle size of 10-40nm, filling the pores of the sepiolite, refining the pore size, and improving the heat resistance. The formed nano-alumina has high toughness and high temperature resistance, thereby improving the heat resistance and mechanical properties of the concrete.

[0086] (2) In the technical scheme of the present invention, the nano-alumina-loaded sepiolite is mixed with the cobalt source cobalt nitrate hexahydrate, and the cobalt nitrate hexahydrate is subjected to a hydrothermal reaction to undergo a dehydroxylation and decarbonization reaction to form cobalt oxide, which is then calcined at 900°C. The nano-alumina-loaded sepiolite is fibrous and its main component is silicon dioxide, so that the formed cobalt oxide can react with the silicon dioxide in the sepiolite to form cobalt silicate by a silicon-oxygen-cobalt bond, thereby realizing the in-situ synthesis of a cobalt silicate layer on the surface of the nano-alumina-loaded sepiolite. The cobalt silicate is insoluble in water and has excellent water resistance, which prevents the sepiolite from easily absorbing water. Water causes incomplete cement hydration, reducing the mechanical properties of concrete, and the cobalt silicate layer can prevent water penetration; ethyl orthosilicate forms a cross-linked network silica gel through hydrolysis and condensation, and the modified sepiolite is dispersed in the cross-linked network silica gel. The gel and the modified sepiolite are adsorbed in the pores of expanded perlite, so that the expanded perlite is converted from hydrophilic to hydrophobic, and has excellent water resistance. The sepiolite is filled into the pores of the expanded perlite, the porosity is increased, and the heat resistance is improved. The silica gel contained on the surface is combined with cement particles through chemical bonds, so that the composite material is dispersed in the concrete matrix;

[0087] (3) In the technical solution of the present invention, rice husk ash has a physical filling and chemical pozzolanic effect. Rice husk ash contains a large amount of minerals such as silica and alumina. These minerals can react with calcium hydroxide in concrete to generate expansive hydration products, reducing the risk of cracking. The porous structure of rice husk can adsorb microbial repair agents, protect bacteria from damage, and prolong the survival time of bacteria. The fine particle size of rice husk ash is used to fill tiny cracks, so that the microbial repair agent can combine with calcium ions in concrete in the cracks to produce precipitation to enhance the performance of concrete. Rice husk ash has high heat resistance. When cracks occur, the loaded microbial repair agent is released. Rice husk ash has good heat resistance, avoiding the direct release of the microbial repair agent in high-temperature concrete, resulting in the inactivation of the microbial repair agent. Nanoparticles are deposited in the pores of glass fibers. Nanoparticles can absorb the stress generated during the mixing process, improve the toughness of glass fibers, and avoid the premature release of the repair agent due to the brittleness of glass fibers, thereby losing the self-repairing performance.

[0088] (4) In the technical solution of the present invention, the epoxy group of the epoxy resin reacts with the hydroxyl group on the surface of the modified glass fiber, so that the modified glass fiber is dispersed in the epoxy resin matrix. Under the action of the cross-linking agent polyethylene glycol diglycidyl ether, a microcapsule repair agent loaded with rice husk powder as a core material and modified glass fiber as a capsule material is formed, which provides a living space for concrete repair bacteria to avoid the inactivation of the bacteria due to the high alkaline environment of concrete. In addition, the glass fiber and rice husk powder as microcapsule wall materials have a synergistic effect in terms of heat resistance, so that the microbial repair agent has a good survival rate at high temperatures. In addition, the nanoparticles attached to the glass fiber have a large specific surface area and interface effect, which can effectively improve the surface inertness and interface structure of the glass fiber, thereby improving the bonding strength between the glass fiber and concrete, so that the microcapsule repair agent is dispersed in the concrete matrix. DETAILED DESCRIPTION

[0089] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0090] Embodiment 1, pre-treatment sepiolite is prepared by the following steps:

[0091] Place 5.7 g of sepiolite in a 250 mL three-necked flask, add 50 mL of 1 mol / L hydrochloric acid, stir evenly, place in a microwave oven, heat to 80 ° C, stir for 2 hours, cool to room temperature, wash with anhydrous ethanol 3 times, wash with deionized water until the washing liquid is neutral, dry in a 60 ° C oven for 10 minutes, and grind in a grinder to obtain pretreated sepiolite.

[0092] Comparative Example 1: The difference between this comparative example and Example 1 is that the pretreated sepiolite is replaced by sepiolite.

[0093] Example 2: The composite aerogel is prepared by the following steps:

[0094] A1. 1.5 g urea and 2.5 g aluminum chloride were added to 50 mL deionized water, stirred evenly, 2.6 g pretreated sepiolite was added, ultrasonically treated for 30 min, stirred and reacted at 120 ° C for 2 h, cooled to room temperature, filtered, washed with deionized water 3 times, placed in a 60 ° C oven to dry for 10 min, placed in a high temperature reactor, heat treated at 500 ° C for 2 h, cooled to room temperature, and obtained nano-alumina-loaded sepiolite;

[0095] A2. Add 0.2 g of cobalt nitrate hexahydrate, 0.06 g of ammonium fluoride and 0.25 g of urea to 50 mL of deionized water, stir for 30 min, add 0.15 g of loaded nano-alumina sepiolite, place in an autoclave, heat treat at 120°C for 5 h, cool to room temperature, wash the solid product with deionized water 3 times, ethanol 5 times, dry in an oven at 60°C for 10 min, place in a Ma furnace, calcine at 900°C for 3 h, cool to room temperature to obtain modified sepiolite.

[0096] A3. Mix 1.5 g of tetraethyl orthosilicate, 7.5 mL of ethanol and 15 mL of deionized water, stir evenly, add 0.5 g of modified sepiolite and 0.5 mL of 36% hydrochloric acid, stir for 30 min to obtain a gel solution, mix 1.5 g of the gel solution with 15 g of expanded perlite, perform vacuum adsorption under a vacuum negative pressure of -0.08 MPa, age at 30 ° C for 4 h, and dry in an oven at 90 ° C for 10 min to obtain a composite aerogel.

[0097] Comparative Example 2: The difference between this comparative example and Example 1 is that the pretreated sepiolite is replaced by the material prepared in Comparative Example 1.

[0098] Comparative Example 3: The difference between this comparative example and Example 1 is that the nano-alumina-loaded sepiolite is replaced by pretreated sepiolite.

[0099] A1. Add 0.2 g of cobalt nitrate hexahydrate, 0.06 g of ammonium fluoride and 0.25 g of urea to 50 mL of deionized water, stir for 30 min, add 0.15 g of pretreated sepiolite, place in an autoclave, heat treat at 120 ° C for 5 h, cool to room temperature, wash the solid product with deionized water 3 times, ethanol 5 times, dry in an oven at 60 ° C for 10 min, place in a Ma furnace, calcine at 900 ° C for 3 h, cool to room temperature, and obtain modified sepiolite.

[0100] A2. Mix 1.5 g of tetraethyl orthosilicate, 7.5 mL of ethanol and 15 mL of deionized water, stir evenly, add 0.5 g of modified sepiolite and 0.5 mL of 36% hydrochloric acid, stir for 30 min to obtain a gel solution, mix 1.5 g of the gel solution with 15 g of expanded perlite, perform vacuum adsorption under a vacuum negative pressure of -0.08 MPa, age at 30 ° C for 4 h, and dry in an oven at 90 ° C for 10 min to obtain a composite aerogel.

[0101] Comparative Example 4: The difference between this comparative example and Example 1 is that no cobalt silicate layer is formed on the surface of the nano-alumina-loaded sepiolite.

[0102] Embodiment 3, microcapsule repair agent is prepared by the following steps:

[0103] B1. Wash 10g of rice husk with deionized water for 3 times, dry it, add it to 20mL of 5% hydrochloric acid solution, heat it at 100℃ for 3h, filter it, wash it with deionized water for 3 times, place it in a muffle furnace, and heat it at 600℃ for 4h to obtain rice husk ash. Mix 3.5g of sucrose, 4g of yeast flavor, 0.02g of dipotassium hydrogen phosphate, 0.17g of calcium chloride, 0.4g of potassium chloride, 0.2g of magnesium sulfate, and 0.3g of manganese sulfate to obtain a culture medium. Add 2.5g of Bacillus pseudofirmus and 2g of Bacillus subtilis to 100mL of the culture medium, culture it at 30℃ for 12h to obtain a bacterial solution. Mix 5.3g of rice husk ash with 20mL of the bacterial solution, adsorb the bacterial solution in the pores of the rice husk ash under a pressure of -0.06MPa, and dry it at 40℃ for 10min to obtain rice husk powder loaded with microbial remediation agent.

[0104] B2. Add 0.3g of nano-silicon dioxide and 0.2g of nano-zirconium dioxide to 30mL of ethanol, stir evenly to obtain a dispersion, immerse 0.54g of glass fiber into the dispersion, stir for 30min, and dry in an oven at 80°C for 10min to obtain modified glass fiber, add 3.6g of epoxy resin and 2.5g of modified glass fiber to 40mL of ethanol, stir, add 0.5g of polyethylene glycol diglycidyl ether, stir at 50°C for 10min, after the reaction is completed, add 2.3g of rice husk powder loaded with microbial remediation agent, stir for 30min to form a gel, filter, wash with deionized water 3 times, and dry in an oven at 80°C for 10min to obtain a microcapsule remediation agent.

[0105] Comparative Example 5: The difference between this comparative example and Example 2 is that the rice husk powder loaded with the microbial remediation agent is not coated with microcapsules.

[0106] Comparative Example 6: This comparative example differs from Example 2 in that rice husk powder is not added.

[0107] Embodiment 4: A method for preparing high-performance heat-resistant concrete, comprising the following steps:

[0108] 300 g of cement, 800 g of basalt gravel, 670 g of river sand, 65 g of fly ash, 55 g of mineral powder, 15 g of microcapsule repair agent, and 10 g of composite aerogel were mixed, and the above raw materials were mixed and stirred for 3 minutes, 6.6 g of PCE-102 polycarboxylate water reducer and 100 g of water were added, and stirring was continued for 10 minutes to obtain heat-resistant concrete.

[0109] Embodiment 5: A method for preparing high-performance heat-resistant concrete, comprising the following steps:

[0110] 317 g of cement, 850 g of basalt gravel, 685 g of river sand, 75 g of fly ash, 60 g of mineral powder, 20 g of microcapsule repair agent, and 15 g of composite aerogel were mixed, and the above raw materials were mixed and stirred for 3 minutes, 6.8 g of PCE-102 polycarboxylate water reducer and 120 g of water were added, and stirring was continued for 10 minutes to obtain heat-resistant concrete.

[0111] Embodiment 6: A method for preparing high-performance heat-resistant concrete, comprising the following steps:

[0112] 334 g of cement, 900 g of basalt gravel, 700 g of river sand, 85 g of fly ash, 65 g of mineral powder, 25 g of microcapsule repair agent, and 20 g of composite aerogel were mixed, and the above raw materials were mixed and stirred for 3 minutes, 7 g of PCE-102 polycarboxylate water reducer and 140 g of water were added, and stirring was continued for 10 minutes to obtain heat-resistant concrete.

[0113] Comparative Example 6: The difference between this comparative example and Example 5 is that the composite aerogel is replaced by the material prepared in Comparative Example 2.

[0114] Comparative Example 7: The difference between this comparative example and Example 5 is that the composite aerogel is replaced by the material prepared in Comparative Example 3.

[0115] Comparative Example 8: The difference between this comparative example and Example 5 is that the composite aerogel is replaced by the material prepared in Comparative Example 4.

[0116] Comparative Example 9: The difference between this comparative example and Example 5 is that the microcapsule repair agent is replaced by the substance prepared in Comparative Example 4.

[0117] Comparative Example 10: The difference between this comparative example and Example 5 is that the microcapsule repair agent is replaced by the substance prepared in Comparative Example 5.

[0118] The performance of the heat-resistant concrete prepared in Examples 4-6 and Comparative Examples 6-10 was tested;

[0119] According to GB / T50081-2016 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete", standard test blocks were made, and the compressive strength of the standard test blocks after 28 days of curing and the compressive strength at high temperature after 28 days were measured. The heat resistance of concrete was measured by the following method: after 28 days of standard curing, the concrete was placed in a high-temperature furnace and calcined at 200°C, 400°C and 600°C for 3 hours, and then naturally cooled to room temperature. The compressive strength of the sintered concrete was measured to measure the heat resistance of concrete;

[0120] Water penetration resistance: The water penetration depth of the standard test block was tested according to the step-by-step pressure test method in GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete"; the fine cracks in the concrete after 28 days were measured, and the crack width was less than 0.1mm, which had good repair performance; the mechanical properties of the concrete prepared above were tested according to DL / T5332-2005 standard; the test results are shown in Table 1 below:

[0121] Table 1

[0122]

[0123] It can be seen from the data in Table 1 that in Comparative Example 6, the pretreated sepiolite is replaced with sepiolite, and the prepared composite aerogel is added to the concrete, and its mechanical properties decrease. This may be because the microwave-assisted acid activation of sepiolite replaces and precipitates the free metal ions magnesium ions in the sepiolite structure, removes surface impurities, and avoids the reaction of metal magnesium ions with calcium silicate of cement, which leads to the decrease of mechanical properties of concrete; Comparative Example 7 is that the nano-alumina-loaded sepiolite is replaced with pretreated sepiolite, and the prepared composite aerogel is added to the concrete, and its toughness and heat resistance decrease. This may be because nano-alumina fills the pores of sepiolite, refines the pore size, improves the heat resistance, and nano-alumina has high toughness and high temperature resistance; Comparative Example 8 is that no cobalt silicate layer is formed on the surface of the nano-alumina-loaded sepiolite, and the prepared composite aerogel is added to the concrete, and its water resistance and mechanical properties decrease. This may be because in the negative A cobalt silicate layer is in situ synthesized on the surface of nano-alumina-loaded sepiolite. Cobalt silicate is insoluble in water and has excellent water resistance, which prevents sepiolite from absorbing water easily, resulting in incomplete cement hydration and reducing the mechanical properties of concrete, and the cobalt silicate layer can prevent moisture penetration; Comparative Example 9 is rice husk powder loaded with microbial repair agent but not coated with glass fiber microcapsules. The prepared microcapsule repair agent is added to concrete, and its repair performance decreases at high temperature. This may be because a living space is provided for the concrete repair bacteria to avoid the bacteria being inactivated by the high alkaline environment of the concrete; Comparative Example 10 is no rice husk powder added. The prepared microcapsule repair agent is added to concrete, and its repair performance decreases at high temperature. This may be because rice husk ash has high heat resistance. When cracks occur, the loaded microbial repair agent is released. Rice husk ash has good heat resistance, which avoids the microbial repair agent being directly released in high-temperature concrete, resulting in the inactivation of the microbial repair agent.

[0124] The data in Table 1 show that the heat-resistant concrete prepared in Examples 4-6 not only has good heat resistance, but also the composite aerogel and microcapsule repair agent can be evenly dispersed in the concrete. The surface of sepiolite is treated with a microwave-assisted acid activator to obtain pretreated sepiolite; modified sepiolite, siloxane and expanded perlite are mixed to obtain a composite aerogel; nanoparticles are deposited into the pores of glass fibers to obtain modified glass fibers as capsule materials, and rice husk powder loaded with microbial repair agent is used as core material to prepare a microcapsule repair agent; cement, basalt gravel, river sand, fly ash, mineral powder, microcapsule repair agent, composite aerogel, water reducer and water are mixed and stirred to obtain heat-resistant concrete that meets the test performance requirements, while the heat-resistant concrete prepared in Comparative Examples 6-10 does not meet the performance requirements, indicating that the heat-resistant concrete prepared by the present invention not only has good heat resistance, but also the composite aerogel and microcapsule repair agent can be evenly dispersed in the concrete.

[0125] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0126] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing high-performance heat-resistant concrete, It is characterized in that The preparation method comprises the following steps: S1. using microwave-assisted acid activator to surface treat sepiolite to obtain pretreated sepiolite; S2. The modified sepiolite, siloxane and expanded perlite are mixed to obtain a composite aerogel; The composite aerogel is prepared by the following steps: mixing siloxane, ethanol and deionized water, stirring evenly, adding modified sepiolite and hydrochloric acid with a mass fraction of 36% to perform acid-base titration to promote the hydrolysis reaction, stirring for 30 minutes to obtain a gel solution, mixing the gel solution with expanded perlite, performing vacuum adsorption at a vacuum negative pressure of -0.08MPa, performing aging treatment at 30°C for 4h, and drying in an oven at 90°C for 10min to obtain a composite aerogel; The modified sepiolite is prepared by mixing pretreated sepiolite with a cobalt source and an aluminum source, subjecting the mixture to high temperature heat treatment, and then subjecting the mixture to high temperature calcination; The high temperature heat treatment temperature is 400-600°C; the high temperature calcination temperature is 800-1000°C; The cobalt source is selected from one of cobalt nitrate, cobalt chloride, cobalt acetate, cobalt hydroxide, cobalt oleate, cobalt linoleate, cobalt octoate, cobalt stearate, cobalt phosphate, and cobalt sulfate; The aluminum source is selected from one of aluminum chloride, aluminum nitrate, and aluminum hydroxide; S3. Depositing nanoparticles into the pores of glass fibers to obtain modified glass fibers as capsule materials, and loading microbial remediation agent rice husk powder as core materials to prepare microcapsule remediation agents; The microcapsule repairing agent is prepared by the following steps: B1. Add the nanoparticles to ethanol and stir evenly to obtain a dispersion, immerse the glass fiber in the dispersion, stir for 30 minutes so that the nanoparticles are adsorbed on the surface and pores of the glass fiber, and place in an oven at 80°C for drying to volatilize the organic solvent ethanol to obtain a modified glass fiber; B2. Add epoxy resin and modified glass fiber to ethanol, stir, add polyethylene glycol diglycidyl ether, stir at 50°C for 10 minutes, add rice husk powder loaded with microbial repair agent after the reaction is completed, stir for 30 minutes to form a gel, filter, wash with deionized water 3 times, and dry in an oven at 80°C for 10 minutes to obtain a microcapsule repair agent; The rice husk powder loaded with microbial remediation agent is prepared by adsorbing the microbial remediation agent on the rice husk powder; The microbial repair agent is selected from any one of Bacillus pseudofirmus, Nitrobacter, Bacillus, and Bacillus subtilis; The rice husk powder has a particle size of 2-5 μm and a pore size of 10-40 nm; S4. Mix and stir cement, basalt crushed stone, river sand, fly ash, mineral powder, microcapsule repair agent, composite aerogel, water reducing agent and water to obtain heat-resistant concrete.

2. A method for preparing high performance heat-resistant concrete according to claim 1, It is characterized in that The microwave heating temperature is 70-100° C., and the acid activator is selected from hydrochloric acid and sulfuric acid.

3. A method for preparing high performance heat-resistant concrete according to claim 1, It is characterized in that The sepiolite has a particle size of 0.3-1.5 μm and a pore size of 50-100 nm.

4. The method for preparing high performance heat-resistant concrete according to claim 1, It is characterized in that The siloxane is selected from one of tetraethyl orthosilicate, trimethylchlorosilane, hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane; the expanded perlite has a particle size of 0.5-5 mm and a pore size of 0.5-2.5 μm.

5. The method for preparing high performance heat-resistant concrete according to claim 1, It is characterized in that The glass fiber has a length of 1.5-2.5 μm and a diameter of 0.1-0.3 μm.

6. The method for preparing high performance heat-resistant concrete according to claim 1, It is characterized in that The nanoparticles are selected from any one of nano silicon dioxide, nano zirconium dioxide, nano titanium dioxide, nano calcium oxide and nano diatomaceous earth.

7. The method for preparing high performance heat-resistant concrete according to claim 1, It is characterized in that The cement is silicate cement with a PO4 of 2.5 and a specific surface area of ​​386.5 m 2 / kg, and the compressive strength at 28d is 56.3MPa.

8. The method for preparing high performance heat-resistant concrete according to claim 1, It is characterized in that The basalt crushed stone is continuously graded with a diameter of 5-25 mm and a mud content of 0.2%. The fly ash is Class F Grade I fly ash with a fineness of 45 μm, a loss on ignition of 2.8% and a water content of 0.15%.

9. The method for preparing high performance heat-resistant concrete according to claim 1, It is characterized in that The apparent density of the river sand is 2680kg / m 3 The fineness modulus is 2.4, the particle size is 3.5mm, and the mud content is 0.9%; the mineral powder is S95 grade slag powder with a density of 2.9g / cm 3 , with a specific surface area of ​​450m 2 / kg, water content is 0.2%, and 28d activity index is 95%.

10. Heat-resistant concrete obtained according to the preparation method according to any one of claims 1 to 9.