Antibacterial, waterproof and breathable TPU for producing band-aids, preparation method and application thereof

By adding modified polyvinylidene fluoride and antibacterial agent to the preparation of TPU, and using a mixed solution of N,N-dimethylformamide and ethyl acetate, the problems of low yield and poor performance compatibility of TPU products are solved, and the problem of low yield and poor performance compatibility is achieved. It has efficient antibacterial, waterproof and moisture-permeable properties, and improves the applicability of Band-Aids.

CN118515847BActive Publication Date: 2024-11-12SHANDONG INOV POLYURETHANE
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410988157.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

At this stage, TPU products prepared by industrial electrospinning have problems such as low yield and difficult to compatible with antibacterial, waterproof and moisture permeability.

Method used

Using formulas containing polyester polyols, isocyanates, chain extenders, processing aids, catalysts, modified polyvinylidene fluoride and antibacterial agents, the preparation of Band-Aids is prepared by a twin-screw extruder and underwater cutting system. Antibacterial and waterproof and moisture-permeable TPU, and a mixed solution of N,N-dimethylformamide and ethyl acetate are used in the spinning liquid to improve the solubility and yield of the spinning liquid.

Benefits of technology

It significantly improves the spinning yield, antibacterial, waterproof, moisture permeable and high rebound properties of TPU, and enhances its applicability in the field of band-aid production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention discloses an antibacterial, waterproof and breathable TPU for producing band-aids, a preparation method and an application thereof, and belongs to the technical field of polyurethane elastomers. The technical scheme thereof is as follows: comprising raw materials of polyester polyol, isocyanate, chain extender, processing aid, catalyst, modified polyvinylidene fluoride and antibacterial agent; the preparation method of the antibacterial, waterproof and breathable TPU substrate is as follows: DMF and ethyl acetate are mixed to obtain a special solvent, TPU particles are dispersed in the mixed solvent to obtain a spinning solution and electrostatic spinning is performed to obtain an antibacterial, waterproof and breathable TPU substrate. Compared with the prior art, the solvent prepared by the present invention allows the mass fraction of TPU dissolved to reach 25%, so the spinning yield is greatly improved compared with the traditional DMF system. At the same time, the TPU substrate prepared by the present invention also has the characteristics of antibacterial, waterproof, breathable, high resilience, etc., which greatly improves its applicability in the field of band-aid production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane elastomers, and specifically relates to an antibacterial, waterproof and breathable TPU for producing band-aids, a preparation method and application thereof. Background Art

[0002] Band-Aid is one of the most commonly used surgical products in our lives. It is mainly composed of dry adhesive tape, medicated absorbent pad and isolation permeable membrane. In the Band-Aid, the medicated absorbent pad is in direct contact with the wound, and its main function is to stop bleeding and protect the wound. The main function of the dry adhesive tape is to fix the Band-Aid and ensure that the medicated absorbent pad continues to act on the wound. The main function of the isolation permeable membrane is to inhibit bacterial invasion, isolate water stains from infecting the wound, and ensure that the wound is breathable and dry, thereby reducing the risk of infection.

[0003] The nanofiber membrane obtained by electrospinning has a soft feel due to its ultra-fine fiber diameter. It uses high-voltage static electricity to form a jet of polymer solution, which is split and stretched in the electric field, and finally deposited on the surface of the receiving device as the solvent evaporates to form a nanofiber membrane with a three-dimensional network structure. The nanofiber membrane has a large specific surface area, so its coverage, warmth retention and fluffiness are better than other types of fibers. Its high porosity can improve the moisture permeability and effectively prevent the invasion of harmful gases, dust and bacteria. Electrospun nanofiber membranes also have high elongation at break and elastic deformation, so they have broad application prospects in the field of waterproof and breathable materials.

[0004] Films made of polyurethane are cheap, easy to obtain, simple to prepare, have good mechanical properties and chemical stability, are also waterproof and breathable, and are therefore widely used in the field of waterproof and breathable. With the development of electrospinning technology, polyurethane is blended with other polymers, natural polymer materials, etc. to improve the performance of polyurethane materials, which can make its application field more extensive. Studies have shown that the introduction of fluorine elements into membrane materials can improve the hydrophobicity of the materials. Polyvinylidene fluoride has a very small surface energy, strong hydrophobicity, and good chemical stability, heat resistance and mechanical properties. It is a polymer membrane material with excellent performance.

[0005] The solutions used for electrospinning TPU are mostly N,N-dimethylformamide (DMF) or dimethylacetamide (DMAC). These two solutions have low dispersibility for TPU, generally between 8% and 12%. The increase in solution concentration will increase the spinning output, but at the same time make the spinning liquid viscous, which makes the Taylor cone diameter under the electric field during the spinning process smaller. This phenomenon reduces the contact between the filament and the air, causing incomplete evaporation of the spinning solvent during the spinning process, and then causing the solvent to penetrate the film, which has a great impact on the quality of spinning.

[0006] From the above analysis, it can be seen that the TPU products prepared by industrial electrospinning at this stage have the problems of low output and incompatibility of antibacterial, waterproof and moisture permeability. Summary of the invention

[0007] The present invention provides an antibacterial, waterproof and breathable TPU for producing bandages, wherein the TPU has good dispersibility and solubility in a spinning solution. The present invention also provides a preparation method and application of the TPU, which is used to produce an isolation permeable membrane in a bandage structure. The TPU substrate has outstanding performance, mainly showing the characteristics of antibacterial, waterproof, breathable, high resilience and high yield.

[0008] The technical solution of the present invention is:

[0009] In the first aspect, an antibacterial, waterproof and breathable TPU for producing a band-aid is disclosed, comprising the following raw materials in parts by weight:

[0010] 60-80 parts of polyester polyol;

[0011] Isocyanate 17-33 parts;

[0012] 3-7 parts of chain extender;

[0013] Processing aid 0.8-1.2 parts;

[0014] Catalyst 0.01-0.02 parts;

[0015] 10-20 parts of modified polyvinylidene fluoride;

[0016] 1-2 parts of antibacterial agent.

[0017] Preferably, the polyester polyol is one of poly(1,4-butylene adipate hexanediol), poly(ethylene adipate glycol) and poly(1,4-butylene adipate glycol), and the number average molecular weight of the polyester polyol is 1000-2000.

[0018] Preferably, the isocyanate is 4,4'-diphenylmethane diisocyanate (MDI-100).

[0019] Preferably, the chain extender is one or more of dipropylene glycol, 1,4-butanediol and neopentyl glycol.

[0020] Preferably, the processing aids are antioxidants, lubricants and ultraviolet absorbers; the antioxidants are hindered phenol antioxidants 1010 and phosphite antioxidants 626; the lubricants are amide wax lubricants WAX-C and lignite wax lubricants WAX-E; the ultraviolet absorbers are methyl ether ultraviolet absorbers UV-1 and hindered ammonia ultraviolet absorbers 770; the catalyst is one of stannous octoate, triethylenediamine and butyl titanate.

[0021] Preferably, the preparation method of the modified polyvinylidene fluoride is: using terephthaloyl peroxide (BPO) as an initiator and 3-phenylacrylic acid (CA) as a monomer, initiating graft polymerization in an N,N-dimethylformamide solution in which polyvinylidene fluoride (PVDF) is dissolved, to obtain polyvinylidene fluoride grafted with 3-phenylacrylic acid, that is, modified polyvinylidene fluoride.

[0022] Preferably, the antibacterial agent is a ternary composite antibacterial material of reduced graphene oxide-titanium dioxide-nanosilver, wherein the mass ratio of reduced graphene oxide, titanium dioxide and nanosilver is 1:1:(1-3).

[0023] In the second aspect, a preparation method of the antibacterial, waterproof and breathable TPU for producing Band-Aids is disclosed, comprising the following steps: injecting a polyester polyol dissolved with a processing aid, a chain extender and an isocyanate into a twin-screw extruder at the same time, adding modified polyvinylidene fluoride and an antibacterial agent into the twin-screw extruder, and then injecting a catalyst into the twin-screw extruder; the mixed material reacts and plasticizes in the screw, and is granulated by an underwater cutting system to obtain the antibacterial, waterproof and breathable TPU for producing Band-Aids.

[0024] Preferably, the extrusion temperature of the twin-screw extruder is 130-220° C., and the screw speed is 170-230 r / min.

[0025] The third aspect discloses the application of the antibacterial, waterproof and breathable TPU in the production of antibacterial, waterproof and breathable TPU substrates for Band-Aids. The preparation method is as follows: N,N-dimethylformamide and ethyl acetate are mixed in a mass ratio of 1:(1-2) to obtain a mixed solution, and the antibacterial, waterproof and breathable TPU for the production of Band-Aids is dispersed into the mixed solution to obtain a spinning solution and electrospinning is performed to obtain an antibacterial, waterproof and breathable TPU substrate for the production of Band-Aids.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The mixed solution of solvent N,N-dimethylformamide and ethyl acetate prepared by the present invention allows the mass fraction of TPU dissolved in the spinning solution to reach 25%, so the spinning yield is greatly improved compared with the traditional DMF system. At the same time, the TPU substrate prepared by the present invention also has the characteristics of antibacterial, waterproof and breathable, high resilience, etc., which greatly improves its applicability in the field of band-aid production.

[0028] 2. The present invention greatly improves the waterproof and breathable properties of TPU by adding modified polyvinylidene fluoride in the process of preparing TPU; polyvinylidene fluoride has very small surface energy, strong hydrophobicity, and good chemical stability, heat resistance and mechanical properties, and is a polymer membrane material with excellent performance. The polyvinylidene fluoride can participate in the reaction process of TPU through modification, thereby improving the waterproof and breathable properties of TPU without affecting the mechanical properties of TPU.

[0029] 3. The present invention greatly improves the antibacterial effect of TPU by adding an antibacterial agent during the preparation of TPU. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.

[0031] Hindered phenol antioxidant 1010, purchased from BASF, Germany;

[0032] Phosphite antioxidant 626, purchased from BASF, Germany;

[0033] Amide wax lubricant WAX-C was purchased from Clariant, Germany;

[0034] Lignite wax lubricant WAX-E, purchased from Clariant, Germany;

[0035] Methyl ether ultraviolet absorber UV-1 was purchased from BASF, Germany;

[0036] Hindered ammonia UV absorber 770 was purchased from BASF, Germany;

[0037] 4,4'-diphenylmethane diisocyanate MDI-100, purchased from BASF, Germany;

[0038] Reduced graphene oxide was purchased from Aladdin Reagent Co., Ltd.

[0039] The specific preparation method of modified polyvinylidene fluoride in the embodiment and comparative example is: dissolve 10g of 3-phenylacrylic acid in 100mL of N,N-dimethylformamide (DMF), stir well, and transfer to a constant pressure dropping funnel for standby. Add 200mL of DMF to a four-necked flask equipped with a stirrer, a condenser, and an air guide tube, add 50g of polyvinylidene fluoride (PVDF) powder to the above four-necked flask, heat to 50°C, and stir at a constant temperature for 30min to fully disperse it. Seal the flask, then pass high-purity nitrogen to exclude the air in the system, while keeping stirring continuously to mix the system evenly, then raise the system temperature to 70°C, add 10g of initiator terephthaloyl peroxide (BPO), and under nitrogen protection, drip the DMF solution of 3-phenylacrylic acid after 30min, and control the drip rate at 0.15mL / min to polymerize, and end the reaction in 8h. The flask was taken out from the water bath, cooled to room temperature, and anhydrous ethanol was added to precipitate the modified polyvinylidene fluoride to remove 3-phenylacrylic acid homopolymer and impurities. The process was repeated three times, and then the obtained product was vacuum dried at 50° C. to constant weight to obtain grafted polyvinylidene fluoride PVDF-gP(CA), i.e., modified polyvinylidene fluoride.

[0040] The antibacterial agent (reduced graphene oxide-titanium dioxide-nanosilver ternary composite antibacterial material) in the embodiment and the comparative example is synthesized by a one-pot method. The specific preparation method is as follows: take a 30% silver nitrate aqueous solution in a beaker, add reduced graphene oxide and titanium dioxide to the silver nitrate solution, the mass ratio of reduced graphene oxide, titanium dioxide and nanosilver is 1:1:(1-3), and place the mixed solution in an ultrasonic device to fully mix; add excess L-ascorbic acid as a reducing agent, close the reactor, and then pass high-purity nitrogen to remove the air in the system, while keeping the reactor constantly stirred to make the system mixed evenly, keep the system temperature at 80°C, and end the reaction for 12 hours. The closed reactor is heated and stirred, and cooled at room temperature. The substance in the reactor is filtered through a suction filter, and continuously rinsed with distilled water during the suction filtration. After the suction filtration, the precipitate is vacuum dried at 70°C to constant weight to obtain a reduced graphene oxide-titanium oxide-nanosilver ternary composite antibacterial material.

[0041] The weight fractions of the raw materials, extrusion temperatures and screw speeds in the examples and comparative examples are shown in Table 1.

[0042] Table 1 Weight fractions of each raw material, extrusion temperature and screw speed in the examples and comparative examples

[0043]

[0044] The preparation method of the antibacterial, waterproof and breathable TPU substrate for producing band-aids in Examples 1-4 and Comparative Examples 1-4 is as follows:

[0045] The polyester polyol dissolved with processing aids, chain extender and isocyanate are injected into the twin-screw extruder from three injection ports of the twin-screw extruder, the modified polyvinylidene fluoride and antibacterial agent are added to the twin-screw extruder, and then the catalyst is injected into the twin-screw extruder. The mixture is plasticized in the screw and granulated by the underwater cutting system to obtain the antibacterial, waterproof and breathable TPU used in the production of band-aids.

[0046] The antibacterial, waterproof and breathable TPU particles used to produce Band-Aids are dispersed in a spinning solution formed by a solvent and dissolved until a transparent spinning solution is formed. The transparent spinning solution is electrospun at room temperature (25°C) and a relative humidity of 50% to obtain an antibacterial, waterproof and breathable TPU substrate used to produce Band-Aids.

[0047] The TPU substrates prepared in the examples and comparative examples were tested in the following manner:

[0048] (1) Hardness test: Test according to the method specified in ASTM D2240 Standard Test Method for Rubber Properties.

[0049] (2) Tensile strength test: The test shall be conducted in accordance with the method specified in the standard “ASTM D412 Tensile test method for vulcanized rubber and thermoplastic elastomers”.

[0050] (3) Elastic recovery test: Each group of TPU substrates (maintaining the same material thickness) was bonded to elastic fabrics of the same specifications and styles through a hot pressing process, and the bonded fabrics were cut into standard specimens and tested on a servo tensile machine (High-speed Railway Testing Instrument Co., Ltd.). The test method is: maintain a fixed stretch of 300% for 5 minutes, release and recover for 5 minutes, and measure the change in the distance between the fixed stretch test points of the specimen.

[0051] (4) Hydrostatic pressure test: The test shall be conducted in accordance with the method specified in the standard "AATCC 127 Water Resistance: Hydrostatic Pressure Test".

[0052] (5) Air permeability test: Test according to the method specified in the standard "ASTM E 96 Standard Test Method for Determining Water Vapor Permeability of Materials". Use a fully automatic air permeability meter to test the air permeability of the material.

[0053] (6) Moisture permeability test: Refer to "ASTM E E96 / E96M 16 Material Water Vapor Permeability Test Method" and use a water vapor permeability tester to measure the moisture permeability of the material.

[0054] (7) Antibacterial performance test: The test was conducted in accordance with the method specified in the standard "GB / T 31402-2015 Test method for antibacterial performance of plastic surfaces". Antibacterial tests were conducted on Staphylococcus aureus and Escherichia coli.

[0055] The test results of the TPU substrates prepared in the examples and comparative examples are shown in Table 2.

[0056] Table 2 Test results of TPU substrates prepared in Examples and Comparative Examples

[0057]

[0058] By comparing and analyzing the performance test data of Examples 1-4 and Comparative Examples 1-4, it can be seen that:

[0059] (1) By comparing and analyzing the data of Example 1 and Comparative Example 1, it can be seen that under the same hardness conditions, whether or not modified polyvinylidene fluoride is added will affect the waterproof performance of the material. Adding modified polyvinylidene fluoride will make the material have better waterproof performance.

[0060] (2) By comparing and analyzing the data of Example 1 and Comparative Example 2, it can be seen that under the condition of the same hardness of the materials, the addition of antibacterial agent can improve the antibacterial properties of the materials.

[0061] (3) By comparing and analyzing the data of Example 1 and Comparative Example 3, it can be seen that the solvent adapted by the present invention allows the mass fraction of TPU in the spinning solution to reach 25%. The spinning output of the present invention is greatly improved compared with the traditional DMF system.

[0062] (4) Comparative analysis of the data of Example 2 and Example 3 shows that the type of antibacterial agent added directly affects the antibacterial performance of the material. Among the three antibacterial agents compared in the present invention, the antibacterial agent with a ratio of reduced graphene oxide: titanium dioxide: nanosilver = 1:1:3 performs best.

[0063] (5) By comparing and analyzing the data of Example 4 and Comparative Example 4, it can be seen that the type of solvent will affect the dissolution amount of TPU. The spinning output of the present invention is greatly improved compared with the traditional ethyl acetate system.

[0064] (6) By comparing and analyzing the data of Example 1 and Comparative Example 4, it can be seen that under different hardness conditions, the higher the material hardness, the better its waterproof performance, and the correspondingly worse its air permeability.

[0065] (7) By comparing and analyzing the data of Example 1 and Example 3, it can be seen that under different hardness conditions, the higher the hardness of the material, the worse its elastic recovery performance.

Claims

1. Antibacterial, waterproof and breathable TPU for producing Band-Aids, characterized in that: Including the following raw materials by mass: 60-80 parts of polyester polyol; Isocyanate 17-33 parts; 3-7 parts of chain extender; Processing aid 0.8-1.2 parts; Catalyst 0.01-0.02 parts; 10-20 parts of modified polyvinylidene fluoride; 1-2 parts of antibacterial agent; The isocyanate is 4,4'-diphenylmethane diisocyanate; The preparation method of the modified polyvinylidene fluoride is as follows: using terephthaloyl peroxide as an initiator and 3-phenylacrylic acid as a monomer, initiating graft polymerization in an N,N-dimethylformamide solution in which polyvinylidene fluoride is dissolved, to obtain polyvinylidene fluoride grafted with 3-phenylacrylic acid, namely the modified polyvinylidene fluoride; The antibacterial agent is a ternary composite antibacterial material of reduced graphene oxide-titanium dioxide-nanosilver, wherein the mass ratio of reduced graphene oxide, titanium dioxide and nanosilver is 1:1:

3.

2. The antibacterial, waterproof and breathable TPU for producing bandages according to claim 1, characterized in that: The polyester polyol is one of poly(1,4-butylene adipate hexanediol), poly(ethylene adipate glycol) and poly(1,4-butylene adipate glycol), and the number average molecular weight of the polyester polyol is 1000-2000.

3. The antibacterial, waterproof and breathable TPU for producing bandages according to claim 1, characterized in that: The chain extender is one of dipropylene glycol, 1,4-butanediol and neopentyl glycol.

4. The antibacterial, waterproof and breathable TPU for producing bandages according to claim 1, characterized in that: The processing aids are antioxidants, lubricants and ultraviolet absorbers; the catalyst is one of stannous octoate, triethylenediamine and butyl titanate.

5. The method for preparing the antibacterial, waterproof and breathable TPU for producing adhesive bandages according to any one of claims 1 to 4, characterized in that: The following steps are involved: The polyester polyol dissolved with processing aid is injected into the twin-screw extruder together with the chain extender and isocyanate, the modified polyvinylidene fluoride and the antibacterial agent are added into the twin-screw extruder, and then the catalyst is injected into the twin-screw extruder; the mixture is reacted and plasticized in the screw, and granulated by the underwater cutting system to obtain the antibacterial, waterproof and breathable TPU for the production of Band-Aids.

6. The method for preparing the antibacterial, waterproof and breathable TPU for producing bandages according to claim 5, characterized in that: The extrusion temperature of the twin-screw extruder is 130-220° C., and the screw speed is 170-230 r / min.

7. Use of the antibacterial, waterproof and breathable TPU for producing band-aids as claimed in any one of claims 1 to 4 in producing antibacterial, waterproof and breathable TPU substrates for producing band-aids, characterized in that: The preparation method comprises the following steps: mixing N,N-dimethylformamide and ethyl acetate in a mass ratio of 1:(1-2) to obtain a mixed solution, dispersing the antibacterial, waterproof and breathable TPU for producing band-aids obtained according to any one of claims 1 to 4 into the mixed solution to obtain a spinning solution, and performing electrostatic spinning to obtain an antibacterial, waterproof and breathable TPU substrate for producing band-aids.

Citation Information

Patent Citations

  • Polypropylene graphene antibacterial composite material and preparation method thereof

    CN112745565A

  • High-strength electrostatic spinning polyurethane waterproof moisture-permeable film and preparation method thereof

    CN115595732A

  • TPU for medical antibacterial film and preparation method thereof

    CN116041941A

  • High-resilience TPU for electrostatic spinning and preparation method and application thereof

    CN116925315A