A preparation method of a special packaging adhesive film for heterojunction battery components and packaging adhesive film

By adopting radiation pre-crosslinking treatment and low-softening point tackifying resin, plasticizer and hollow design in the packaging film of heterojunction battery modules, the problems of film fluidity and welding tape slip are solved, and the problems of film flowability and welding tape slip are improved. The adhesive properties and light transmittance of the components enhance the reliability and power generation efficiency of the components.

CN118516059BActive Publication Date: 2024-11-05ZHEJIANG SOLARTRON TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411000698.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-05
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

Traditional packaging films are difficult to meet the demands of heterojunction batteries for bonding performance and high water resistance, and during the lamination of low-temperature welding tape and adhesive film, it is easy to cause film flow and penetration and welding tape slip, affecting the power generation efficiency of the components. and reliability.

Method used

The base layer and the bearing layer are used to reduce fluidity by irradiation pre-crosslinking treatment, and the viscosity-enhancing resin and plasticizer with low softening points are added to the bearing layer. Combined with a partial hollow design, it improves the bonding performance and light transmittance and prevents Film seepage and welding tape slip.

Benefits of technology

It effectively prevents the film from infiltration and the welding tape slip during the lamination process, improves the bonding performance and light transmittance of heterojunction battery components, reduces the risk of hidden cracks in the battery cells, and enhances the reliability and power generation efficiency of the components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118516059B_ABST
    Figure CN118516059B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of heterojunction battery packaging, and discloses a method for preparing a packaging film dedicated to heterojunction battery components and a packaging film, the preparation method comprising the following steps: (1) mixing the raw materials of a base layer and a bearing layer respectively, the raw materials of the base layer comprising a base resin, an initiator and a crosslinking agent, and the raw materials of the bearing layer comprising a base resin, a tackifying resin, a plasticizer, an initiator and a crosslinking agent; then extruding and casting them into films respectively, and then irradiating and pre-crosslinking them to obtain a base layer film and a bearing layer film respectively; (2) the bearing layer film comprises a plurality of long strip-shaped bearing strips, the bearing layer film is arranged on the base layer film, and the bearing strips are arranged at equal intervals, and then compounded by roller extrusion bonding to obtain a packaging film. The present invention reduces the fluidity of the film by irradiation pre-crosslinking treatment, and the bearing layer adopts a hollow design and adds a tackifying resin and a plasticizer, which can improve the light transmittance while ensuring the adhesion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of heterojunction battery packaging, and in particular to a preparation method of a packaging adhesive film dedicated to a heterojunction battery assembly and the packaging adhesive film. Background Art

[0002] Heterojunction cells (HJT cells) have become the focus of many photovoltaic module manufacturers due to their advantages such as high conversion efficiency, low attenuation, low temperature coefficient and high bifaciality. Heterojunction cells use a composite structure of N-type silicon wafers, amorphous silicon thin films and TCO thin films. Traditional packaging films are difficult to meet their requirements for bonding performance and high water resistance. In addition, in order to improve the power generation efficiency of components and reduce the cost of silver paste, heterojunction photovoltaic components using a main grid-free 0BB packaging solution will become the mainstream in the future. The heterojunction photovoltaic components also need to use low-temperature solder tapes, which are laminated with the film at the same time and welded to the battery cell. In this process, it is necessary to solve the problem of how to prevent the film from flowing and penetrating into the middle of the solder tape and the battery cell under the action of temperature and pressure to cause a circuit break, and to fix the solder tape to prevent the solder tape from slipping.

[0003] At present, most encapsulation film products adopt multi-layer composite means, in which the side that carries the solder strip and is in direct contact with the battery cell is mostly pre-crosslinked by electron beam irradiation and tackifying resin is added. The irradiation pre-crosslinking treatment can reduce its fluidity, thereby solving the problem of solder strip slippage and the film penetrating between the solder strip and the battery cell. However, after irradiation, the adhesive performance of the film with the battery cell and the solder strip decreases, and it is easy to delaminate with the battery cell, the fluidity is reduced, and the risk of hidden cracks in the battery cell is also increased. Adding tackifying resin to the film formula will reduce the transmittance and affect the power generation efficiency of the entire component. Summary of the invention

[0004] In order to solve the above-mentioned technical problems, the present invention provides a method for preparing a packaging film specially used for heterojunction battery assemblies and a packaging film. The base layer and the bearing layer are pre-crosslinked by radiation to reduce their fluidity, thereby solving the problem of the film penetrating between the welding strip and the battery cell; the bearing layer is directly in contact with the low-temperature welding strip and the battery cell, and a partial hollow design is adopted so that a part of the base layer can also be in contact with the battery cell. The bearing layer is added with a tackifying resin to solve the problem of welding strip slippage, and the selection of a tackifying resin with a low softening point and the addition of a plasticizer, together with the synergistic effect of the partial hollow design, reduce the degree of transmittance reduction.

[0005] The purpose of the present invention is achieved through the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a special packaging adhesive film for a heterojunction battery assembly, comprising the following steps:

[0007] (1) Mixing raw materials of a base layer and a bearing layer respectively, wherein the raw materials of the base layer include a base resin, an initiator and a cross-linking agent, and the raw materials of the bearing layer include a base resin, a tackifying resin, a plasticizer, an initiator and a cross-linking agent, wherein the softening point of the tackifying resin is 70-85° C.; then extruding and casting them into films respectively, and then irradiating and pre-cross-linking treatment, to obtain a base layer film with a torque value of 0.25-0.35 and a bearing layer film with a torque value of 0.35-0.60 respectively;

[0008] (2) The supporting layer film includes a plurality of long supporting strips. The supporting layer film is disposed on the base layer film, and the supporting strips are arranged at equal intervals, and then compounded by roller extrusion and bonding to obtain a packaging film.

[0009] The integrated encapsulation adhesive film for heterojunction battery components includes a bearing layer in contact with the battery cell and the welding strip and a base layer in contact with the glass / back plate. Initiators and crosslinking agents are added to the base layer and the bearing layer on the basis of the base resin. Through irradiation pre-crosslinking treatment, the fluidity is reduced during lamination, which effectively prevents the film from penetrating during the lamination process, hindering the contact between the welding strip and the battery cell to cause a short circuit, and the appearance of black spots after lamination. However, the bearing layer is in direct contact with the battery and the welding strip, and its irradiation pre-crosslinking treatment will make the bonding performance worse. The present invention can improve the bonding performance by adding a tackifying resin to the bearing layer, which not only plays a role in fixing the welding strip to prevent the welding strip from slipping during the lamination process, but also ensures a close bond with the base layer, but it will reduce the light transmittance.

[0010] Therefore, the bearing layer adopts a partially hollowed-out design, and several spaced and long bearing strips are parallel and in contact with the welding strips in the heterojunction battery assembly, which can ensure adhesion while improving light transmittance. And by adjusting the torque value of the base layer and the bearing layer after irradiation, the higher the torque value of the film after irradiation, the higher the pre-crosslinking degree of the film, and the lower the fluidity, so that the pre-crosslinking degree of the bearing layer is slightly higher than that of the base layer, and the degree of fluidity reduction is greater. Therefore, the bonding performance of the base layer is better than that of the bearing layer. The partially hollowed-out design allows a part of the base layer to contact the battery cell, thereby improving the bonding performance of the entire film and the battery cell, allowing a part of the base layer with better fluidity to contact the battery cell, and reducing the stress on the battery cell during the lamination process, thereby reducing the risk of hidden cracks in the battery cell to a certain extent.

[0011] In addition, the tackifying resin added in the bearing layer of the present invention is a low softening point tackifying resin, and a plasticizer is added for compounding. The light transmittance reduction after adding the tackifying resin in the bearing layer is mainly due to the poor compatibility between it and the matrix resin, and the light has additional loss at the interface between the two, and the matrix resin may crystallize and reduce the light transmittance. By adding a tackifying resin with a low softening point, while ensuring the bonding performance, by pulling in the softening point of the tackifying resin and the melting point of the matrix resin, the compatibility between the tackifying resin and the matrix resin is optimized, and the aggregated structure and morphology of the matrix resin molecules are more easily affected, the intermolecular interaction force is reduced, and then the crystalline form and crystallinity of the matrix resin are affected, thereby reducing the impact of the tackifying resin on the light transmittance. Also by adding a plasticizer, the intermolecular interaction of the matrix resin can also be weakened, the compliance of the matrix resin is improved, the diffusion capacity of the segment is increased, and it is made to meet the principle of similar diffusion capacity, optimize the compatibility between the matrix resin and the tackifying resin, affect the crystalline form and crystallinity of the matrix resin, and the impact of the tackifying resin on the light transmittance can be reduced equally. Therefore, the present invention reduces the degree of decrease in the light transmittance of the bearing layer by selecting a low softening point tackifying resin and adding an appropriate amount of plasticizer, and adopting a synergistic effect of a partial hollow design.

[0012] Preferably, in step (1), the raw materials of the base layer include, by weight, 93-98 parts of base resin, 0.4-0.8 parts of initiator, 0.3-1.2 parts of cross-linking agent, 0.2-0.6 parts of ultraviolet absorber, 0.1-0.6 parts of anti-aging agent and 0.2-0.6 parts of coupling agent.

[0013] Preferably, in step (1), the raw materials of the supporting layer include, by weight, 78-90 parts of base resin, 10-15 parts of tackifying resin, 0.1-0.4 parts of plasticizer, 0.8-2 parts of initiator, 0.3-1.2 parts of cross-linking agent, 0.2-0.6 parts of ultraviolet absorber, 0.1-0.6 parts of anti-aging agent and 0.2-0.6 parts of coupling agent.

[0014] Preferably, in step (1), the base resin is ethylene-vinyl acetate copolymer (EVA resin), polyolefin elastomer (POE resin), ethylene-acrylic acid copolymer (EAA resin) or ethyl methacrylate (EMA resin).

[0015] Preferably, in step (1), the plasticizer is one or more of dibutyl phthalate, dioctyl phthalate and epoxy tetrahydrophthalate.

[0016] Preferably, the tackifying resin is rosin resin or terpene resin.

[0017] Preferably, the initiator is one or more of tert-amyl peroxy 2-ethylhexyl carbonate (TAEC), tert-butyl peroxy 2-ethylhexyl carbonate (TBEC) and dicumyl peroxide (DCP).

[0018] Preferably, the crosslinking agent is one or more of triallyl isocyanurate (TAIC), trimethylolpropane trimethacrylate (TMPTA), ethoxylated trimethylolpropane trimethacrylate (EO-TMPTA) and trimethylolpropane trimethacrylate (TMPTMA).

[0019] Preferably, the coupling agent is a silane coupling agent containing a vinyl group or an epoxy group.

[0020] Preferably, the coupling agent is one or more of 3-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, 3-aminopropyltriethoxysilane, and 3-glycidylpropyltrimethoxysilane.

[0021] Preferably, the ultraviolet absorber is one or more of 2-hydroxy-4-n-octyloxybenzophenone and 2,4-di[2,2'-bis(5-butoxyphenol)]-6-(2,4-dibutoxybenzene)-1,3,5-triazine.

[0022] Preferably, the anti-aging agent is a light stabilizer and / or an antioxidant.

[0023] Preferably, the light stabilizer is a hindered amine light stabilizer.

[0024] Preferably, the light stabilizer is one or more of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinylethanol) succinate.

[0025] Preferably, the antioxidant is one or more of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol (antioxidant 1076) and tris(2,4-di-tert-butylphenyl) phosphite (antioxidant 168).

[0026] Preferably, in step (1), the radiation pre-crosslinking treatment is electron beam or UV radiation pre-crosslinking treatment.

[0027] Preferably, in step (1), the conditions for the electron beam irradiation pre-crosslinking treatment are: the electron beam irradiation dose is 15-35 kGY, and the irradiation line speed is 15-30 m / min.

[0028] Preferably, in step (2), the obtained encapsulation film comprises a base layer and a carrier layer, the base layer has a thickness of 400-800 μm, and the carrier layer has a thickness of 50-100 μm.

[0029] Preferably, in step (2), the support bars are arranged to correspond one-to-one with the welding strips in the heterojunction battery assembly, the width of the support bars is greater than the width of the welding strips, the width of the intervals between adjacent support bars is less than the width of the intervals between adjacent welding strips, and is not less than 30 mm.

[0030] The carrier bar is parallel to and fits with the welding strip in the heterojunction battery assembly. The width of the carrier bar is greater than the width of the welding strip, so that the carrier bar completely covers the corresponding welding strip; the width of the interval between adjacent carrier bars is less than the width of the interval between adjacent welding strips.

[0031] Preferably, in step (2), the extrusion temperature during the extrusion casting process is 75-90°C.

[0032] In the process of extrusion casting film formation, the present invention can optimize the compatibility between components by adding a tackifying resin and a plasticizer with a low softening point, and reduce the influence of the tackifying resin on the light transmittance by affecting the crystal form and crystallinity of the base resin.

[0033] Preferably, in step (2), when the composite is compounded by roller extrusion bonding, the extrusion molding direction is parallel to the length direction of the support strip.

[0034] Preferably, in step (2), when the composite is compounded by roller extrusion bonding, the linear speed of the lamination roller is 15-30 m / min, the temperature is 60-80° C., and the pressure is 0.5-1 MPa.

[0035] When compounding by roller extrusion bonding, the parameters will vary greatly depending on the equipment. The number and size of the pressing rollers (the position of extrusion bonding) of different equipment are different, so the contact area and time are different. The equipment used in the embodiment of the present invention includes four sets of pressing rollers. The linear speed of the pressing rollers is 15~30m / min, the temperature is 60~80℃, and the pressure is 0.5~1MPa.

[0036] In a second aspect, the present invention also provides a packaging adhesive film specifically for heterojunction battery components obtained by the above-mentioned preparation method.

[0037] Preferably, the encapsulation film comprises a base layer and a bearing layer arranged on the base layer; the bearing layer comprises a plurality of spaced-apart and elongated bearing strips, the bearing strips being parallel to and corresponding one to one with the welding strips in the heterojunction battery assembly.

[0038] Preferably, the thickness of the base layer is 400-800 μm, and the thickness of the bearing layer is 50-100 μm.

[0039] Preferably, the supporting bars are arranged to correspond one-to-one with the welding strips in the heterojunction battery assembly, the width of the supporting bars is greater than the width of the welding strips, the width of the intervals between adjacent supporting bars is less than the width of the intervals between adjacent welding strips, and is not less than 30 mm.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] (1) The integrated encapsulation film dedicated to heterojunction battery modules includes a carrier layer in contact with the battery cell and solder ribbon and a substrate layer in contact with the glass / backplane. Through irradiation pre-crosslinking treatment, the fluidity is reduced during lamination, which effectively prevents the film from penetrating during the lamination process, hindering the contact between the solder ribbon and the battery cell, resulting in a short circuit, and the appearance of black spots after lamination;

[0042] (2) The bearing layer adopts a partially hollowed-out design, and a number of spaced and long bearing strips are parallel to and in contact with the welding strips in the heterojunction battery assembly, which can ensure adhesion while improving light transmittance;

[0043] (3) Adding tackifying resin to the carrier layer can improve the bonding performance, which not only fixes the solder strip to prevent it from slipping during the lamination process, but also ensures a close bond with the substrate layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 It is a cross-sectional view of the packaging film specially used for heterojunction battery components in the present invention.

[0045] Figure 2 It is a top view of the packaging film specially used for heterojunction battery components in the present invention. DETAILED DESCRIPTION

[0046] The technical solution of the present invention is described below with specific embodiments, but the protection scope of the present invention is not limited thereto:

[0047] Example 1

[0048] In terms of weight, the raw materials of the bearing layer include: 88.0 parts of POE matrix resin, 10.0 parts of rosin resin (softening point 75°C, refined hydrogenated rosin RFHR of Dinghong Resin), 0.2 parts of plasticizer (dioctyl phthalate), 0.8 parts of initiator (tert-butyl peroxide-2-ethylhexyl carbonate), 0.3 parts of cross-linking agent (triallyl isocyanurate), 0.5 parts of coupling agent (0.2 parts of 3-methacryloxypropyltrimethoxysilane, 0.3 parts of vinyltrimethoxysilane), 0.2 parts of ultraviolet absorber (2-hydroxy-4-n-octyloxybenzophenone), and 0.15 parts of light stabilizer (poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate).

[0049] In parts by weight, the raw materials of the base layer include: 98.0 parts of POE base resin, 0.9 parts of initiator (0.5 parts of tert-butyl peroxide-2-ethylhexyl carbonate, 0.4 parts of tert-amyl peroxide 2-ethylhexyl carbonate), 0.3 parts of cross-linking agent (triallyl isocyanurate), 0.5 parts of coupling agent (0.2 parts of 3-methacryloxypropyltrimethoxysilane, 0.3 parts of vinyltrimethoxysilane), 0.2 parts of ultraviolet absorber (2-hydroxy-4-n-octyloxybenzophenone), and 0.2 parts of light stabilizer (poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate).

[0050] The preparation method of the encapsulation film comprises the following steps:

[0051] (1) The raw materials of the bearing layer and the substrate layer are mixed evenly in a double-screw conical mixer, and then extruded and cast into films at an extrusion temperature of 80° C. to obtain a bearing layer semi-finished product and a substrate layer semi-finished product, respectively.

[0052] (2) The semi-finished bearing layer film and the semi-finished base layer film prepared by extrusion casting were subjected to electron beam irradiation pre-crosslinking treatment. The irradiation dose of the bearing layer was 25 kGY and the line speed was 20 m / min. After irradiation, the torque value of the bearing layer film was 0.35. The irradiation dose of the base layer was 18 kGY and the line speed was 25 m / min. After irradiation, the torque value of the base layer film was 0.25.

[0053] (3) The bearing layer film includes a plurality of long strip-shaped bearing strips. The bearing layer film is placed on the base layer film, and the bearing strips are arranged at equal intervals. The width of the bearing strips is 10 mm, and the interval width between adjacent bearing strips is 35 mm. The bearing layer film and the base layer film are then compounded by roller extrusion bonding. There are four groups of lamination rollers (extrusion lamination positions). The rotation direction of the lamination rollers is parallel to the length direction of the bearing strips. The linear speed is 20 m / min, the temperature is 60 °C, and the pressure is 0.8 MPa. Figure 1 The encapsulation film includes a base layer and a carrier layer arranged on the base layer, as shown in FIG. Figure 2 As shown, the bearing layer is of hollow design, and includes a plurality of bearing strips arranged at intervals and in the shape of long strips. The thickness of the base layer is 500 μm, and the thickness of the bearing layer is 70 μm.

[0054] Example 2

[0055] In terms of weight, the raw materials of the bearing layer include: 88.0 parts of POE matrix resin, 10.0 parts of terpene resin (softening point 85°C, terpene resin BT from Kerry Petroleum Resins Co., Ltd.), 0.2 parts of plasticizer (dioctyl phthalate), 0.8 parts of initiator (tert-butyl peroxide-2-ethylhexyl carbonate), 0.3 parts of cross-linking agent (triallyl isocyanurate), 0.5 parts of coupling agent (0.2 parts of 3-methacryloxypropyltrimethoxysilane, 0.3 parts of vinyltrimethoxysilane), 0.2 parts of ultraviolet absorber (2-hydroxy-4-n-octyloxybenzophenone), and 0.15 parts of light stabilizer (poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate).

[0056] In parts by weight, the raw materials of the base layer include: 98.0 parts of POE base resin, 0.8 parts of initiator (tert-butyl peroxide-2-ethylhexyl carbonate), 0.3 parts of cross-linking agent (triallyl isocyanurate), 0.5 parts of coupling agent (0.2 parts of 3-methacryloxypropyltrimethoxysilane and 0.3 parts of vinyltrimethoxysilane), 0.2 parts of ultraviolet absorber (2-hydroxy-4-n-octyloxybenzophenone), and 0.2 parts of light stabilizer (poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate).

[0057] The preparation method of the encapsulation film comprises the following steps:

[0058] (1) The raw materials of the bearing layer and the substrate layer are mixed evenly in a double-screw conical mixer, and then extruded and cast into films at an extrusion temperature of 90° C. to obtain a bearing layer semi-finished product and a substrate layer semi-finished product, respectively.

[0059] (2) The semi-finished bearing layer film and the semi-finished base layer film prepared by extrusion casting were subjected to electron beam irradiation pre-crosslinking treatment. The irradiation dose of the bearing layer was 25 kGY and the line speed was 20 m / min. After irradiation, the torque value of the bearing layer film was 0.35. The irradiation dose of the base layer was 18 kGY and the line speed was 25 m / min. After irradiation, the torque value of the base layer film was 0.25.

[0060] (3) The bearing layer film includes a plurality of long strips of bearing strips. The bearing layer film is placed on the base layer film, and the bearing strips are arranged at equal intervals. The width of the bearing strips is 10 mm, and the interval width between adjacent bearing strips is 35 mm. The bearing layer film and the base layer film are then compounded by roller extrusion bonding. There are four groups of lamination rollers (extrusion lamination positions). The rotation direction of the lamination rollers is parallel to the length direction of the bearing strips. The linear speed is 20 m / min, the temperature is 60°C, and the pressure is 0.8 MPa to obtain an integrated packaging film. The packaging film includes a base layer and a bearing layer. The thickness of the base layer is 500 μm, and the thickness of the bearing layer is 70 μm.

[0061] Example 3

[0062] In terms of weight, the raw materials of the bearing layer include: 85.0 parts of POE matrix resin, 12.0 parts of rosin resin (softening point 75°C, refined hydrogenated rosin RFHR of Dinghong Resin), 0.3 parts of plasticizer (dibutyl phthalate), 0.8 parts of initiator (tert-butyl peroxide-2-ethylhexyl carbonate), 0.5 parts of cross-linking agent (triallyl isocyanurate), 0.6 parts of coupling agent (0.3 parts of 3-methacryloxypropyltrimethoxysilane, 0.3 parts of vinyltrimethoxysilane), 0.3 parts of ultraviolet absorber (2-hydroxy-4-n-octyloxybenzophenone), and 0.1 parts of light stabilizer (poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate).

[0063] In parts by weight, the raw materials of the base layer include: 95.0 parts of POE base resin, 1.1 parts of initiator (0.5 parts of tert-butyl peroxide-2-ethylhexyl carbonate, 0.4 parts of tert-amyl peroxide 2-ethylhexyl carbonate), 0.4 parts of cross-linking agent (triallyl isocyanurate), 0.6 parts of coupling agent (0.3 parts of 3-methacryloxypropyltrimethoxysilane, 0.3 parts of vinyltrimethoxysilane), 0.3 parts of ultraviolet absorber (2-hydroxy-4-n-octyloxybenzophenone), and 0.2 parts of light stabilizer (poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate).

[0064] The preparation method of the encapsulation film comprises the following steps:

[0065] (1) The raw materials of the bearing layer and the substrate layer are mixed evenly in a double-screw conical mixer, and then extruded and cast into films at an extrusion temperature of 80° C. to obtain a bearing layer semi-finished product and a substrate layer semi-finished product, respectively.

[0066] (2) The semi-finished bearing layer film and the semi-finished base layer film prepared by extrusion casting were subjected to electron beam irradiation pre-crosslinking treatment. The irradiation dose of the bearing layer was 25 kGY and the line speed was 20 m / min. After irradiation, the torque value of the bearing layer film was 0.35. The irradiation dose of the base layer was 18 kGY and the line speed was 25 m / min. After irradiation, the torque value of the base layer film was 0.25.

[0067] (3) The bearing layer film includes a plurality of long strips of bearing strips. The bearing layer film is placed on the base layer film, and the bearing strips are arranged at equal intervals. The width of the bearing strips is 10 mm, and the interval width between adjacent bearing strips is 35 mm. The bearing layer film and the base layer film are then compounded by roller extrusion bonding. There are four groups of lamination rollers (extrusion lamination positions). The rotation direction of the lamination rollers is parallel to the length direction of the bearing strips. The linear speed is 20 m / min, the temperature is 60°C, and the pressure is 0.8 MPa to obtain an integrated packaging film. The packaging film includes a base layer and a bearing layer. The thickness of the base layer is 500 μm, and the thickness of the bearing layer is 70 μm.

[0068] Example 4

[0069] In terms of weight, the raw materials of the bearing layer include: 88.0 parts of POE matrix resin, 10.0 parts of rosin resin (softening point 75°C, refined hydrogenated rosin RFHR of Dinghong Resin), 0.2 parts of plasticizer (dioctyl phthalate), 0.8 parts of initiator (tert-butyl peroxide-2-ethylhexyl carbonate), 0.3 parts of cross-linking agent (triallyl isocyanurate), 0.5 parts of coupling agent (0.2 parts of 3-methacryloxypropyltrimethoxysilane, 0.3 parts of vinyltrimethoxysilane), 0.2 parts of ultraviolet absorber (2-hydroxy-4-n-octyloxybenzophenone), and 0.15 parts of light stabilizer (poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate).

[0070] In parts by weight, the raw materials of the base layer include: 98.0 parts of POE base resin, 0.9 parts of initiator (0.5 parts of tert-butyl peroxide-2-ethylhexyl carbonate, 0.4 parts of tert-amyl peroxide 2-ethylhexyl carbonate), 0.3 parts of cross-linking agent (triallyl isocyanurate), 0.5 parts of coupling agent (0.2 parts of 3-methacryloxypropyltrimethoxysilane, 0.3 parts of vinyltrimethoxysilane), 0.2 parts of ultraviolet absorber (2-hydroxy-4-n-octyloxybenzophenone), and 0.2 parts of light stabilizer (poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate).

[0071] The preparation method of the encapsulation film comprises the following steps:

[0072] (1) The raw materials of the bearing layer and the substrate layer are mixed evenly in a double-screw conical mixer, and then extruded and cast into films at an extrusion temperature of 80° C. to obtain a bearing layer semi-finished product and a substrate layer semi-finished product, respectively.

[0073] (2) The semi-finished bearing layer film and the semi-finished substrate layer prepared by extrusion casting were subjected to electron beam irradiation pre-crosslinking treatment. The irradiation dose of the bearing layer was 33 kGY, the line speed was 15 m / min, and the torque value of the bearing layer film after irradiation was 0.45; the irradiation dose of the substrate layer was 20 kGY, the line speed was 22 m / min, and the torque value of the substrate layer film after irradiation was 0.30.

[0074] (3) The bearing layer film includes a plurality of long strips of bearing strips. The bearing layer film is placed on the base layer film, and the bearing strips are arranged at equal intervals. The width of the bearing strips is 10 mm, and the interval width between adjacent bearing strips is 35 mm. The bearing layer film and the base layer film are then compounded by roller extrusion bonding. There are four sets of lamination rollers (the position of extrusion lamination). The rotation direction of the lamination rollers is parallel to the length direction of the bearing strips. The linear speed is 20 m / min, the temperature is 60°C, and the pressure is 0.8 MPa to obtain an integrated packaging film. The packaging film includes a base layer and a bearing layer. The thickness of the base layer is 500 μm, and the thickness of the bearing layer is 90 μm.

[0075] Comparative Example 1

[0076] The difference from Example 1 is that there is no bearing layer.

[0077] In parts by weight, the raw materials of the base layer include: 98.0 parts of POE base resin, 0.8 parts of initiator (tert-butyl peroxide-2-ethylhexyl carbonate), 0.3 parts of cross-linking agent (triallyl isocyanurate), 0.5 parts of coupling agent (0.2 parts of 3-methacryloxypropyltrimethoxysilane and 0.3 parts of vinyltrimethoxysilane), 0.2 parts of ultraviolet absorber (2-hydroxy-4-n-octyloxybenzophenone), and 0.2 parts of light stabilizer (poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate).

[0078] The preparation method of the encapsulation film comprises the following steps:

[0079] (1) The raw materials of the substrate layer are mixed uniformly in a double-screw conical mixer, and then extruded and cast into films at an extrusion temperature of 80° C. to obtain a semi-finished supporting layer and a semi-finished substrate layer.

[0080] (2) The semi-finished product of the substrate layer prepared by extrusion casting was subjected to electron beam irradiation pre-crosslinking treatment, the irradiation dose was 18 kGY, the line speed was 25 m / min, the torque value of the film after irradiation was 0.25, and an integrated packaging film with a thickness of 500 μm was obtained.

[0081] Comparative Example 2

[0082] The difference from Example 2 is that the bearing layer has no hollow design.

[0083] The preparation method of the encapsulation film comprises the following steps:

[0084] (1) The raw materials of the bearing layer and the substrate layer are mixed evenly in a double-screw conical mixer, and then extruded and cast into films at an extrusion temperature of 90° C. to obtain a bearing layer semi-finished product and a substrate layer semi-finished product, respectively.

[0085] (2) The semi-finished bearing layer film and the semi-finished base layer film prepared by extrusion casting were subjected to electron beam irradiation pre-crosslinking treatment, the irradiation dose of the bearing layer was 25 kGY, the line speed was 20 m / min, and the torque value of the bearing layer film after irradiation was 0.35; the irradiation dose of the base layer was 18 kGY, the line speed was 25 m / min, and the torque value of the base layer film after irradiation was 0.25; an integrated packaging film was obtained, the packaging film comprising a base layer and a bearing layer, the thickness of the base layer was 500 μm, and the thickness of the bearing layer was 70 μm.

[0086] Comparative Example 3

[0087] The difference from Example 2 is that the width of the bearing bar is 19 mm, and the width of the interval between adjacent bearing bars is 26 mm.

[0088] The preparation method of the encapsulation film comprises the following steps:

[0089] (1) The raw materials of the bearing layer and the substrate layer are mixed evenly in a double-screw conical mixer, and then extruded and cast into films at an extrusion temperature of 90° C. to obtain a bearing layer semi-finished product and a substrate layer semi-finished product, respectively.

[0090] (2) The semi-finished bearing layer film and the semi-finished base layer film prepared by extrusion casting were subjected to electron beam irradiation pre-crosslinking treatment. The irradiation dose of the bearing layer was 25 kGY and the line speed was 20 m / min. After irradiation, the torque value of the bearing layer film was 0.35. The irradiation dose of the base layer was 18 kGY and the line speed was 25 m / min. After irradiation, the torque value of the base layer film was 0.25.

[0091] (3) The bearing layer film includes a plurality of long strips of bearing strips. The bearing layer film is placed on the base layer film, and the bearing strips are arranged at equal intervals. The width of the bearing strips is 19 mm, and the interval width between adjacent bearing strips is 26 mm. The bearing layer film and the base layer film are then compounded by roller extrusion bonding. There are four sets of lamination rollers (the position of extrusion bonding). The rotation direction of the lamination rollers is parallel to the length direction of the bearing strips. The linear speed is 20 m / min, the temperature is 60°C, and the pressure is 0.8 MPa to obtain an integrated packaging film. The packaging film includes a base layer and a bearing layer. The thickness of the base layer is 500 μm, and the thickness of the bearing layer is 70 μm.

[0092] Comparative Example 4

[0093] The difference from Example 2 is that no plasticizer is added to the bearing layer.

[0094] In terms of weight, the raw materials of the bearing layer include: 88.0 parts of POE matrix resin, 10.0 parts of terpene resin (softening point 85°C, terpene resin BT from Kerry Petroleum Resins Co., Ltd.), 0.8 parts of initiator (tert-butyl peroxide-2-ethylhexyl carbonate), 0.3 parts of cross-linking agent (triallyl isocyanurate), 0.5 parts of coupling agent (0.2 parts of 3-methacryloxypropyltrimethoxysilane, 0.3 parts of vinyltrimethoxysilane), 0.2 parts of ultraviolet absorber (2-hydroxy-4-n-octyloxybenzophenone), and 0.15 parts of light stabilizer (poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate).

[0095] In parts by weight, the raw materials of the base layer include: 98.0 parts of POE base resin, 0.8 parts of initiator (tert-butyl peroxide-2-ethylhexyl carbonate), 0.3 parts of cross-linking agent (triallyl isocyanurate), 0.5 parts of coupling agent (0.2 parts of 3-methacryloxypropyltrimethoxysilane and 0.3 parts of vinyltrimethoxysilane), 0.2 parts of ultraviolet absorber (2-hydroxy-4-n-octyloxybenzophenone), and 0.2 parts of light stabilizer (poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate).

[0096] The preparation method of the encapsulation film comprises the following steps:

[0097] (1) The raw materials of the bearing layer and the substrate layer are mixed evenly in a double-screw conical mixer, and then extruded and cast into films at an extrusion temperature of 90° C. to obtain a bearing layer semi-finished product and a substrate layer semi-finished product, respectively.

[0098] (2) The semi-finished bearing layer film and the semi-finished base layer film prepared by extrusion casting were subjected to electron beam irradiation pre-crosslinking treatment. The irradiation dose of the bearing layer was 25 kGY and the line speed was 20 m / min. After irradiation, the torque value of the bearing layer film was 0.35. The irradiation dose of the base layer was 18 kGY and the line speed was 25 m / min. After irradiation, the torque value of the base layer film was 0.25.

[0099] (3) The bearing layer film includes a plurality of long strips of bearing strips. The bearing layer film is placed on the base layer film, and the bearing strips are arranged at equal intervals. The width of the bearing strips is 10 mm, and the interval width between adjacent bearing strips is 35 mm. The bearing layer film and the base layer film are then compounded by roller extrusion bonding. There are four groups of lamination rollers (extrusion lamination positions). The rotation direction of the lamination rollers is parallel to the length direction of the bearing strips. The linear speed is 20 m / min, the temperature is 60°C, and the pressure is 0.8 MPa to obtain an integrated packaging film. The packaging film includes a base layer and a bearing layer. The thickness of the base layer is 500 μm, and the thickness of the bearing layer is 70 μm.

[0100] Comparative Example 5

[0101] The difference from Example 2 is that the softening point of the tackifying resin in the bearing layer is too high.

[0102] In terms of weight, the raw materials of the bearing layer include: 88.0 parts of POE matrix resin, 10.0 parts of terpene resin (softening point 130°C, terpene resin BT from Kerry Petroleum Resins Co., Ltd.), 0.05 parts of plasticizer (dioctyl phthalate), 0.8 parts of initiator (tert-butyl peroxide-2-ethylhexyl carbonate), 0.3 parts of cross-linking agent (triallyl isocyanurate), 0.5 parts of coupling agent (0.2 parts of 3-methacryloxypropyltrimethoxysilane, 0.3 parts of vinyltrimethoxysilane), 0.2 parts of ultraviolet absorber (2-hydroxy-4-n-octyloxybenzophenone), and 0.15 parts of light stabilizer (poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate).

[0103] In parts by weight, the raw materials of the base layer include: 98.0 parts of POE base resin, 0.8 parts of initiator (tert-butyl peroxide-2-ethylhexyl carbonate), 0.3 parts of cross-linking agent (triallyl isocyanurate), 0.5 parts of coupling agent (0.2 parts of 3-methacryloxypropyltrimethoxysilane and 0.3 parts of vinyltrimethoxysilane), 0.2 parts of ultraviolet absorber (2-hydroxy-4-n-octyloxybenzophenone), and 0.2 parts of light stabilizer (poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate).

[0104] The preparation method of the encapsulation film comprises the following steps:

[0105] (1) The raw materials of the bearing layer and the substrate layer are mixed evenly in a double-screw conical mixer, and then extruded and cast into films at an extrusion temperature of 90° C. to obtain a bearing layer semi-finished product and a substrate layer semi-finished product, respectively.

[0106] (2) The semi-finished bearing layer film and the semi-finished base layer film prepared by extrusion casting were subjected to electron beam irradiation pre-crosslinking treatment. The irradiation dose of the bearing layer was 25 kGY and the line speed was 20 m / min. After irradiation, the torque value of the bearing layer film was 0.35. The irradiation dose of the base layer was 18 kGY and the line speed was 25 m / min. After irradiation, the torque value of the base layer film was 0.25.

[0107] (3) The bearing layer film includes a plurality of long strips of bearing strips. The bearing layer film is placed on the base layer film, and the bearing strips are arranged at equal intervals. The width of the bearing strips is 10 mm, and the interval width between adjacent bearing strips is 35 mm. The bearing layer film and the base layer film are then compounded by roller extrusion bonding. There are four groups of lamination rollers (extrusion lamination positions). The rotation direction of the lamination rollers is parallel to the length direction of the bearing strips. The linear speed is 20 m / min, the temperature is 60°C, and the pressure is 0.8 MPa to obtain an integrated packaging film. The packaging film includes a base layer and a bearing layer. The thickness of the base layer is 500 μm, and the thickness of the bearing layer is 70 μm.

[0108] Comparative Example 6

[0109] The difference from Example 2 is that the torque values ​​of the bearing layer and the base layer are the same, both 0.25.

[0110] The preparation method of the encapsulation film comprises the following steps:

[0111] (1) The raw materials of the bearing layer and the substrate layer are mixed evenly in a double-screw conical mixer, and then extruded and cast into films at an extrusion temperature of 90° C. to obtain a bearing layer semi-finished product and a substrate layer semi-finished product, respectively.

[0112] (2) The semi-finished bearing layer film and the semi-finished substrate layer prepared by extrusion casting were subjected to electron beam irradiation pre-crosslinking treatment. The irradiation dose of the bearing layer was 20 kGY, the line speed was 25 m / min, and the torque value of the bearing layer film after irradiation was 0.25; the irradiation dose of the substrate layer was 18 kGY, the line speed was 25 m / min, and the torque value of the substrate layer film after irradiation was 0.25.

[0113] (3) The bearing layer film includes a plurality of long strips of bearing strips. The bearing layer film is placed on the base layer film, and the bearing strips are arranged at equal intervals. The width of the bearing strips is 10 mm, and the interval width between adjacent bearing strips is 35 mm. The bearing layer film and the base layer film are then compounded by roller extrusion bonding. There are four groups of lamination rollers (extrusion lamination positions). The rotation direction of the lamination rollers is parallel to the length direction of the bearing strips. The linear speed is 20 m / min, the temperature is 60°C, and the pressure is 0.8 MPa to obtain an integrated packaging film. The packaging film includes a base layer and a bearing layer. The thickness of the base layer is 500 μm, and the thickness of the bearing layer is 70 μm.

[0114] The encapsulation films in the above-mentioned embodiments and comparative examples were subjected to a light transmittance test and a peel strength test on the heterojunction battery cell, and then they were packaged with the heterojunction battery cell, and the obtained heterojunction battery assembly was subjected to an EL test.

[0115] Battery packaging steps: From bottom to top, the glass, packaging film (carrying layer on top), HJT (heterojunction) battery cell, low-temperature solder tape, packaging film (carrying layer on the bottom), and glass are laminated (lamination temperature 120°C, lamination pressure -75~-45MPa, lamination time 740s) to obtain a heterojunction battery assembly. The width of the low-temperature solder tape is 9mm, the interval is 36mm, and the carrying strip in the packaging film is parallel to the low-temperature solder tape and corresponds to each other and fits perfectly.

[0116] Peel strength test standard: GB / T 2790-1995 "Adhesive 180° Peel Strength Test Method".

[0117] Test standard for light transmittance: GB 2410-80 "Test method for light transmittance and haze of transparent plastics".

[0118] EL test standard: NB / T 11080-2023 Technical Specification for Photovoltaic Module Electroluminescence (EL) Testing; Test at room temperature to detect and identify whether the battery components have the following defects: hidden cracks, fragments, black edges, dark pieces, broken grids, pollution, etc.

[0119] Table 1

[0120]

[0121] As shown in Table 1, the encapsulation film of the present invention is suitable for heterojunction battery components, and can improve light transmittance while ensuring adhesion. Through irradiation pre-crosslinking treatment, the fluidity is reduced during lamination, which effectively prevents the film from penetrating during the lamination process, hindering the contact between the welding ribbon and the battery cell to cause a short circuit, and the appearance of black spots after lamination. A part of the base layer with better fluidity than the bearing layer contacts the battery cell, which can also reduce the stress on the battery cell during the lamination process, thereby reducing the risk of hidden cracks in the battery cell to a certain extent.

[0122] Comparative Example 1 shows that there is no bearing layer in the encapsulation film. Since the base layer is pre-crosslinked by radiation, the adhesion will be significantly reduced, and the peel strength between the encapsulation film and the battery cell will be reduced. In addition, the degree of radiation pre-crosslinking of the base layer is lower than that of the bearing layer, and it still has a certain fluidity. The film will still penetrate during the lamination process, resulting in severe blackening during the EL test. Although a bearing layer is provided in the encapsulation film in Comparative Example 6, due to the low degree of radiation pre-crosslinking of the bearing layer, partial blackening will still occur during the EL test.

[0123] In Comparative Example 2, the support layer of the encapsulation film does not adopt a hollow design. Compared with the support layer with a hollow design, the light transmittance of the encapsulation film will decrease. In addition, due to the high degree of cross-linking and low fluidity of the support layer, the stress on the battery cell during the lamination process cannot be well dispersed, which will lead to hidden cracks in the battery cell. In Comparative Example 3, the hollow design parameters of the support layer exceed the specified range, the width of the support strip is too large and the spacing is too small, resulting in the light transmittance being affected and increasing the risk of hidden cracks in the battery cell.

[0124] Comparative Examples 4 and 5 show that the addition of plasticizers and low softening point tackifying resins can improve the compatibility between the tackifying resin and the base resin and reduce the crystallization problem of the base resin. Therefore, the plasticizer can have a good synergistic effect with the low softening point tackifying resin to further improve the adhesion and transmittance.

[0125] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the specification of the present invention, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing a special packaging film for heterojunction battery components, characterized in that: The steps include: (1) The raw materials of the base layer and the bearing layer are mixed separately, wherein the raw materials of the base layer include base resin, initiator and cross-linking agent, and the raw materials of the bearing layer include base resin, tackifying resin, plasticizer, initiator and cross-linking agent, wherein the base resin is POE resin, and the tackifying resin is rosin resin or terpene resin, and the softening point of the tackifying resin is 70-85°C; then, the raw materials are extruded and cast into films, and then irradiated and pre-cross-linked, to obtain a base layer film with a torque value of 0.25-0.30 and a bearing layer film with a torque value of 0.35-0.60 respectively; (2) The supporting layer film includes a plurality of long supporting strips, which are arranged on the base layer film. The supporting layer is hollowed out, and the supporting strips are arranged at equal intervals. The supporting strips are arranged to correspond to the welding strips in the heterojunction battery module one by one. The width of the supporting strips is greater than the width of the welding strips, and the width of the interval between adjacent supporting strips is less than the width of the interval between adjacent welding strips, and is not less than 30 mm. The supporting strips are then compounded by roller extrusion and bonding to obtain a packaging film.

2. The method for preparing a special packaging adhesive film for heterojunction battery components according to claim 1, characterized in that: In step (1), the raw materials of the base layer include, by weight, 93-98 parts of base resin, 0.4-0.8 parts of initiator, 0.3-1.2 parts of cross-linking agent, 0.2-0.6 parts of ultraviolet absorber, 0.1-0.6 parts of anti-aging agent and 0.2-0.6 parts of coupling agent.

3. The method for preparing a special packaging adhesive film for heterojunction battery components according to claim 1, characterized in that: In step (1), the raw materials of the supporting layer include, by weight, 78-90 parts of base resin, 10-15 parts of tackifying resin, 0.1-0.4 parts of plasticizer, 0.8-2 parts of initiator, 0.3-1.2 parts of cross-linking agent, 0.2-0.6 parts of ultraviolet absorber, 0.1-0.6 parts of anti-aging agent and 0.2-0.6 parts of coupling agent.

4. The method for preparing a special packaging adhesive film for heterojunction battery components according to any one of claims 1 to 3, characterized in that: In step (1), the plasticizer is one or more of dibutyl phthalate, dioctyl phthalate and epoxy tetrahydrophthalate.

5. The method for preparing a special packaging adhesive film for heterojunction battery components according to any one of claims 1 to 3, characterized in that: In step (1), the radiation pre-crosslinking treatment is electron beam or UV radiation pre-crosslinking treatment.

6. The method for preparing the encapsulation adhesive film for heterojunction battery components according to claim 5, characterized in that: The conditions for the electron beam irradiation pre-crosslinking treatment are: the electron beam irradiation dose is 15~35kGY, and the irradiation line speed is 15~30m / min.

7. The method for preparing a special packaging adhesive film for heterojunction battery components according to claim 1, characterized in that: In step (2), the encapsulation film includes a base layer and a carrier layer, the base layer has a thickness of 400-800 μm, and the carrier layer has a thickness of 50-100 μm.

8. The method for preparing a special packaging adhesive film for heterojunction battery components according to claim 1 or 7, characterized in that: In step (2), the extrusion temperature during the extrusion casting process is 75-90°C.

9. A packaging adhesive film for heterojunction battery components prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The packaging film comprises a base layer and a bearing layer arranged on the base layer; the bearing layer comprises a plurality of bearing strips which are arranged at equal intervals and are in the shape of long strips.