A NbTi superconducting wire and a method for preparing the same

By setting a U-shaped groove on the outer periphery of the metal rod and performing cold drawing and thermal drawing, the high copper ultra-ratio NbTi superconducting wire is prepared, which solves the problem of insufficient critical current in high current and high magnetic field applications in the prior art, and reduces the Processing costs and improve performance.

CN118522500BActive Publication Date: 2024-11-22XIAN SUPERCONDUCTING WIRE TECHNOLOGIES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410985064.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-22
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The existing NbTi superconducting wires have insufficient critical current density in high current and high magnetic field applications and are highly processed, making it difficult to meet the needs of nuclear magnetic resonance instruments.

Method used

By setting multiple U-shaped grooves on the outer periphery of the metal rod, the NbTi/Cu superconducting composite wire is placed in the groove for cold drawing, avoiding the cable twisting step, and NbTi superconducting wire is prepared by braided belt wrap and online hot drawing.

Benefits of technology

The NbTi superconducting wire with high copper super ratio has high critical current and low loss drop, meeting the needs of high current and high magnetic field application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118522500B_ABST
    Figure CN118522500B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of superconducting wires, and relates to a NbTi superconducting wire and a preparation method thereof. The present invention provides a preparation method of a NbTi superconducting wire, which is prepared by arranging at least two U-shaped grooves on the periphery of a metal rod, placing a NbTi / Cu superconducting composite wire in the U-shaped grooves, and processing the NbTi superconducting wire after cold drawing. The present invention avoids the step of twisting cables, and solves the technical problems that when preparing NbTi superconducting wires with high current and high copper ratio, the increase in the diameter of the NbTi / Cu superconducting composite wire means a larger volume, higher loss and a more difficult processing method, and twisting cables inevitably leads to a loss of critical current and higher processing costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of superconducting wires and relates to a NbTi superconducting wire and a preparation method thereof. Background Art

[0002] NbTi superconductors belong to the second type of superconductors. When they are in the superconducting state, the magnetic flux quantum is not completely excluded from the superconductor, but can enter the superconductor, but must be pinned to the non-superconducting second phase. The non-superconducting second phase can be impurities, grain boundaries, dislocations, etc. The most important magnetic flux pinning center in NbTi superconductors is non-superconducting α-Ti. The second phase has no effect on the upper critical field and critical temperature of the superconductor, but has a great influence on the critical current density of the superconductor. When preparing NbTi superconducting wires, it is necessary to make both the superconducting phase and the second phase (pinning phase) exist in the wire, and the volume content of the second phase needs to reach a certain value, otherwise the critical current density will be affected. The critical current density of NbTi superconducting wires is a key parameter related to its practicality. At the same time, it is also affected by the preparation process. The critical current density of NbTi superconducting wires with the same alloy composition prepared by different processes may have great differences.

[0003] The NbTi superconductor is made into a superconducting wire, usually by processing the NbTi / Cu composite wire into a superconducting wire, which has the characteristics of a large copper-to-superconducting ratio and has the advantages of being economical and practical. Patent CN110970171A discloses a method for improving the RRR value and yield strength of NbTi superconducting wire, which uses a U-shaped copper slot wire and an unannealed NbTi / Cu superconducting round wire immersed in a tin bath, and selects a suitable inlay welding temperature for inlay welding to obtain the NbTi superconducting wire. Inlay welding and braiding insulation of NbTi / Cu composite wire and copper slot wire to make a rectangular high copper ratio wire is only suitable for superconducting magnets with low current and small magnetic field, and cannot meet the needs of preparing nuclear magnetic resonance instruments with large current and high magnetic field. Summary of the invention

[0004] In the preparation of NbTi superconducting wires, in the face of the demand for higher currents and higher magnetic fields, it is necessary to increase the diameter of a single NbTi / Cu superconducting composite wire or to combine multiple NbTi / Cu superconducting composite wires with U-shaped copper groove wires after twisting them into NbTi superconducting wires. Increasing the diameter of the NbTi / Cu superconducting composite wire means a larger volume, higher losses and more difficult processing methods, and twisting the cables inevitably leads to a decrease in critical current and higher processing costs.

[0005] In order to overcome the problems of the prior art, the present invention provides a NbTi superconducting wire and a preparation method thereof. The present invention can realize the manufacture of a plurality of NbTi / Cu superconducting composite wires into a NbTi superconducting wire by arranging a plurality of U-shaped grooves on the outer periphery of a metal rod without twisting cables.

[0006] On the one hand, the present invention relates to a method for preparing a NbTi superconducting wire, which comprises: setting at least two U-shaped grooves on the periphery of a metal rod, placing a NbTi / Cu superconducting composite wire in the U-shaped grooves, and processing the wire into the NbTi superconducting wire after cold drawing.

[0007] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the metal rod is a rectangle, the intersection of two adjacent straight lines of the rectangle is a transition arc, and the radius of the transition arc is 0.2 mm to 0.3 mm.

[0008] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the U-shaped grooves are evenly distributed on the periphery of the metal rod, and the R angles on both sides of the U-shaped grooves are 0.2 mm to 0.3 mm. The even distribution described in the present invention is a symmetrical distribution, the purpose of which is to reduce the degradation of performance caused by uneven distribution of the superconducting phase in the wire.

[0009] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the processing rate of the cold drawing is 5% to 10%, and the drawing speed is 20 m / min to 30 m / min;

[0010] The four R angles of the rectangular die used in the cold drawing are 0.4 mm to 0.6 mm.

[0011] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the NbTi / Cu superconducting composite wire is cold drawn, and then wrapped with a braided tape and hot drawn online to obtain the NbTi superconducting wire.

[0012] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the braided tape is a tin tape, the width of the tin tape is 1 mm to 2 mm, and the thickness of the tin tape is 0.05 mm to 0.10 mm;

[0013] The overlap factor of the wrapping is 50%.

[0014] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the heating temperature of the online hot drawing is 240° C. to 260° C., and the hot drawing speed is 5 m / min to 10 m / min.

[0015] Furthermore, in the method for preparing the NbTi superconducting wire provided by the present invention, the material of the metal rod is oxygen-free copper or aluminum.

[0016] Optionally, in the method for preparing the NbTi superconducting wire provided by the present invention, fixed die finishing is performed after the online hot drawing is completed, and the processing rate of the fixed die finishing is less than 5%.

[0017] On the other hand, the present invention relates to a NbTi superconducting wire, which is prepared by the preparation method.

[0018] In another aspect, the present invention relates to a nuclear magnetic resonance apparatus, comprising a main magnet, wherein the main magnet comprises the NbTi superconducting wire.

[0019] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects or advantages:

[0020] The present invention provides a method for preparing a NbTi superconducting wire, wherein the preparation method prepares a plurality of U-shaped grooves on an oxygen-free copper rod, and then places a plurality of strands of NbTi / Cu composite round wires in the U-shaped grooves and then cold-draws the wires to prepare the NbTi superconducting wires. The present invention avoids the step of twisting cables, and has the advantages of high critical current and low critical current loss when preparing a NbTi superconducting wire with a high copper superconducting ratio. The NbTi superconducting wire prepared by the present invention can meet the application scenario requirements of large current and high magnetic field, has the characteristics of high copper superconducting ratio, and still has a high critical current under high magnetic field. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 Schematic diagram of the structure after the metal rod with two U-shaped grooves and the NbTi / Cu superconducting composite wire are assembled.

[0023] Figure 2 Schematic diagram of the structure after the metal rod with three U-shaped grooves and the NbTi / Cu superconducting composite wire are assembled.

[0024] Figure 3 Schematic diagram of the structure after the metal rod with four U-shaped grooves and the NbTi / Cu superconducting composite wire are assembled.

[0025] Among them, 1 is a NbTi / Cu superconducting composite wire, and 2 is a metal rod with a U-shaped groove. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is described below in conjunction with embodiments; however, the present invention is not limited to the following embodiments.

[0027] The experimental methods and detection methods described in the following embodiments are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified.

[0028] Example 1

[0029] This embodiment provides a method for preparing a NbTi superconducting wire.

[0030] A rectangular oxygen-free copper rod is drawn into a shape of 6.0 mm wide × 5.0 mm high and 0.3 mm R angle by a die, and two U-shaped grooves are processed on both sides, with a groove depth of 1.7 mm, a groove width of 1.65 mm, and an inner R angle (R angle on both sides of the U-shaped groove) of 0.2 mm. Then, two strands of NbTi / Cu superconducting composite wires with a diameter of 1.6 mm, a copper ratio of 1.0, 85 NbTi cores, and a NbTi core wire diameter of 120 μm are placed in the U-shaped groove. The structure is as follows: Figure 1 shown.

[0031] They are initially combined together through die cold drawing. The dimensions after cold drawing are 5.7mm wide × 4.8mm high, 0.4mm R angle, 5.7% processing rate, and 30m / min cold drawing speed. A tin strip with a width of 1 mm and a thickness of 0.05 mm was selected for half-lapping (50% overlap coefficient). The tin strip was evenly wound on the surface of the wire, and then online hot drawing was carried out. The induction heating temperature was 240°C, and the hot drawing speed was 10 m / min. The tin strip was fully melted to firmly combine the copper slot wire and the multi-strand round wire. Finally, a fixed die with a width of 5.65 mm × a height of 4.75 mm and an R angle of 0.4 mm was used for finishing. The processing rate was 2%, and the surface of the wire was shaped. At the same time, online eddy current flaw detection was carried out to check the internal and external damage points of the wire. If serious defects were found by visual observation or eddy current flaw detection, the machine was immediately shut down and sheared. Finally, a NbTi superconducting wire with a critical current Ic (4.2K, 5T) of 6100A and a superconducting ratio (the ratio of the superconducting phase area to the non-superconducting phase area) of 11 was successfully prepared.

[0032] Example 2

[0033] This embodiment provides a method for preparing a NbTi superconducting wire.

[0034] A rectangular aluminum rod is drawn into a shape of 7.0 mm wide × 6.0 mm high and 0.3 mm R angle by die drawing, and then three U-shaped grooves are processed on the periphery, with a groove depth of 2.00 mm, a groove width of 1.95 mm, and an inner R angle of 0.2 mm. Then, three strands of NbTi / Cu superconducting composite wires with a diameter of 1.9 mm, a copper ratio of 1.0, 630 NbTi cores, and a NbTi core wire diameter of 54 μm are placed in the U-shaped grooves. The structure is as follows: Figure 2 shown.

[0035] They are initially combined together by cold drawing with a die. After cold drawing, the dimensions are 6.6mm wide × 5.6mm high, 0.6mm R angle, 8.1% processing rate, and 20m / min cold drawing speed. A 2mm wide and 0.10mm thick tin strip is selected for half-lapping. The tin strip is evenly wound on the surface of the wire, and then online hot drawing is performed. The induction heating temperature is 260℃, and the hot drawing speed is 5m / min. The tin strip is fully melted to firmly combine the aluminum slot wire and the multi-strand round wire. Finally, a 6.48mm wide × 5.48mm high and 0.6mm R angle fixed die is used for finishing. The processing rate is 4%, and the surface of the wire is shaped. At the same time, online eddy current flaw detection is performed to check the internal and external damage points of the wire. If serious defects are found by naked eye observation or eddy current flaw detection, the machine is immediately shut down and sheared. Finally, a NbTi superconducting wire with a critical current Ic (4.2K, 5T) of 12800A and a super ratio of 7 is successfully prepared.

[0036] Example 3

[0037] This embodiment provides a method for preparing a NbTi superconducting wire.

[0038] A rectangular oxygen-free copper rod is drawn into a shape of 8.0 mm wide × 7.0 mm high and 0.2 mm R angle by a die, and then four U-shaped grooves are processed on the periphery, with a groove depth of 0.90 mm, a groove width of 0.85 mm and an inner R angle of 0.2 mm. Then, four strands of NbTi / Cu superconducting composite wires with a diameter of 0.8 mm, a copper ratio of 1.0, 55 NbTi cores and a NbTi core wire diameter of 76 μm are placed in the U-shaped grooves. The structure is as follows: Figure 3 shown.

[0039] They are initially combined together by cold drawing with a die. After cold drawing, the dimensions are 7.6mm wide × 6.6mm high, 0.5mm R angle, 9.4% processing rate, and 25m / min cold drawing speed. A 2.0mm wide and 0.10mm thick tin strip is selected for half-lapping. The tin strip is evenly wrapped on the surface of the wire, and then online hot drawing is performed. The induction heating temperature is 250℃, and the hot drawing speed is 8m / min. The tin strip is fully melted to firmly combine the copper slot wire and the multi-strand round wire. Finally, a 7.50mm wide × 6.50mm high and 0.5mm R angle fixed die is used for finishing. The processing rate is 3%, and the surface of the wire is shaped. At the same time, online eddy current flaw detection is performed to check the internal and external damage points of the wire. If serious defects are found by naked eye observation or eddy current flaw detection, the machine is immediately shut down and sheared. Finally, a NbTi superconducting wire with a critical current Ic (4.2K, 5T) of 3040A and a copper superconducting ratio of 48 is successfully prepared.

[0040] Comparative Example

[0041] This comparative example provides a method for preparing a NbTi superconducting wire.

[0042] The multiple round wires are first twisted and formed, and then the formed cables are inlaid and welded. The cables are stably placed in a copper slot wire with a slot, and then soldered with solder. The two are then refined and sized through a mold.

[0043] Test Case

[0044] This test example provides NbTi superconducting wires prepared by different methods.

[0045] The same raw materials provided in Examples 1 to 3 were used to prepare NbTi superconducting wires by the method provided in the comparative example. The critical current Ic (4.2K, 5T) and loss drop were tested. The test results are shown in Table 1.

[0046] Loss reduction (%) = [1-(critical current of wire after inlay welding / critical current of wire before inlay welding)] × 100%.

[0047] Table 1: Test results

[0048]

[0049] As can be seen from Table 1, the present invention provides a method for preparing a NbTi superconducting wire, which is prepared by preparing a plurality of U-shaped grooves on an oxygen-free copper rod, and then placing a plurality of NbTi / Cu composite round wires in the U-shaped grooves and cold drawing them to obtain the NbTi superconducting wire. This method directly inlays a copper or aluminum groove wire with multiple grooves by multiple round wires, which can effectively improve the critical current of the NbTi superconducting wire and greatly reduce the loss to about 1 / 2 by comparing the method of inlaying a copper groove wire after twisting multiple round wires.

[0050] As described above, the basic principle, main features and advantages of the present invention are well described. The above embodiments and descriptions are only descriptions of the preferred implementation modes of the present invention, and the present invention is not limited by the above embodiments. Without departing from the spirit and scope of the present invention, various changes and improvements made by ordinary technicians in this field to the technical solution of the present invention should fall within the protection scope determined by the present invention.

Claims

1. A method for preparing a NbTi superconducting wire, characterized in that: include: At least two U-shaped grooves are arranged on the outer circumference of the metal rod, and the NbTi / Cu superconducting composite wire is placed in the U-shaped grooves, and processed into the NbTi superconducting wire after cold drawing; After the NbTi / Cu superconducting composite wire is cold drawn, the NbTi superconducting wire is wrapped with a braided tape and hot drawn online to obtain the NbTi superconducting wire; The braided tape is a tin tape, the width of the tin tape is 1 mm to 2 mm, and the thickness of the tin tape is 0.05 mm to 0.10 mm.

2. The method for preparing a NbTi superconducting wire according to claim 1, characterized in that: The metal rod is a rectangle, the intersection of two adjacent straight lines of the rectangle is a transition arc, and the radius of the transition arc is 0.2mm-0.3mm.

3. The method for preparing the NbTi superconducting wire according to claim 2, characterized in that: The U-shaped grooves are evenly distributed on the outer circumference of the metal rod, and the R angles on both sides of the U-shaped grooves are 0.2 mm to 0.3 mm.

4. The method for preparing the NbTi superconducting wire according to claim 2, characterized in that: The cold drawing processing rate is 5% to 10%, and the drawing speed is 20m / min to 30m / min; The four R angles of the rectangular die used in the cold drawing are 0.4 mm to 0.6 mm.

5. The method for preparing the NbTi superconducting wire according to claim 1, characterized in that: The overlap coefficient of the wrapping is 50%.

6. The method for preparing a NbTi superconducting wire according to claim 1, characterized in that: The heating temperature of the online hot drawing is 240° C. to 260° C., and the hot drawing speed is 5 m / min to 10 m / min.

7. The method for preparing a NbTi superconducting wire according to claim 1, characterized in that: The metal rod is made of oxygen-free copper or aluminum.

8. A NbTi superconducting wire, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 7.

9. A nuclear magnetic resonance apparatus, comprising a main magnet, characterized in that: The main magnet includes the NbTi superconducting wire according to claim 8 .