A kind of cold heading steel wire rod for 13.9 grade non-quenched and tempered bolts and its manufacturing method
Through the C-Si-Mn-Cr-Nb chemical composition and online molten salt second-stage cooling technology, high-strength and high-plastic cold heading steel strips are formed, solving the problems of high material costs and long production cycles in the existing technology. , realizes the efficient manufacturing of 13.9-level non-temperature bolts.
Patent Information
- Application Number
- CN202410987161.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The existing cold heading steel strips for grade 13.9 non-temperature bolts have challenges in improving strength and delayed fracture performance, especially the problems of high material costs, long production cycles and easy breakage, which are difficult to meet the needs of high strength and high plasticity. .
The chemical composition design of C-Si-Mn-Cr-Nb is combined with the second-stage online molten salt cooling and roller slow cooling technology to control the carbon content and alloy content to form a tissue mainly composed of tempered pearlite, combined with NbC Dispersed phases are degraded, reduced tissue stress and dislocation density, and improved tensile strength and plasticity.
It has achieved tensile strength of 1260~1310MPa and cross-section shrinkage of 46%~50%, reducing the risk of drawing and breaking wire and cold heading cracking, improving the resistance to delay fracture, and is suitable for the manufacturing of 13.9-level non-temperature bolts. Good industrial adaptability and yield rate.
Smart Images

Figure CN118531322B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cold heading steel wire rods, and in particular relates to a cold heading steel wire rod for 13.9-grade non-quenched and tempered bolts and a manufacturing method thereof. Background Art
[0002] High-strength fasteners can greatly improve the service environment of equipment and increase the service life of equipment. With the improvement of the strength of fastener materials, especially when the tensile strength exceeds 1200MPa, the problem of delayed fracture becomes prominent. At present, the 13.9 grade high-strength fasteners produced by steel mills mainly add high Cr, Ni, Mo or micro-alloy components on the basis of medium carbon components, combined with the post-rolling Stelmor air cooling to adjust the organization, and then the downstream manufacturing enterprises anneal to improve the drawing and cold heading performance, and temper to achieve the final performance level. For example: CN116288056A discloses a bolt steel and its production method and heat treatment method, which adopts a medium C-Si-Mn-Al-Mo-Cr-Ni-Tb component design, combined with the Stelmor wire insulation cooling after low-temperature wire drawing, to obtain To the structure of pearlite + ferrite + a small amount of bainite, and then further heat treatment to achieve strength level 13.9 and delayed fracture resistance. However, on the one hand, the high alloy content makes the steel material cost higher. After reducing the alloy content or eliminating the alloy component, it is difficult to control the organizational state of the Stelmor cooling line during continuous cooling, which will cause a large loss of strength; on the other hand, the wire rod obtained after hot rolling cooling contains a hard and brittle bainite structure. Although the strength is improved, the plasticity is significantly reduced, and it is easy to break during downstream unwinding, wire rod transportation and even winding, which seriously damages the yield rate. At the same time, further heat treatment is required, which increases the process and energy consumption. Therefore, the development of 13.9 grade non-quenched and tempered bolts for cold heading steel wire rod is of great significance to simplify fastener manufacturing, reduce energy consumption and improve manufacturing efficiency.
[0003] At present, domestic 13.9-grade non-quenched and tempered bolts are often produced by hot-rolled round steel for blank processing, annealing, and cold heading processes. Not only is the production cycle long, but it is also more suitable for the production of larger bolts. However, the development of raw materials for cold heading steel wire rods for 13.9-grade non-quenched and tempered bolts, which are smaller in size, relatively simple and fast to manufacture, and suitable for the manufacture of small-size bolts, is difficult, and is mainly concentrated in the research and development of non-quenched and tempered wire rods of grade 10.9 and below. Taking low-grade non-quenched and tempered cold heading steel wire rods as an example, it is difficult to further improve the performance to meet the manufacturing and application requirements of 13.9-grade non-quenched and tempered bolts. The technical difficulties and causes are:
[0004] (1) The existing lower-grade non-quenched and tempered cold heading steel wire rods mainly improve the strength of the wire rods by adding high alloy content or micro-alloy components on the basis of low and medium carbon components, and further improve the strength by adding a certain amount of bainite or martensite in the structure during controlled cooling, or increase the soft phase structure to improve the plasticity. For example, CN118256824A discloses a 12.9-grade non-quenched and tempered steel hot-rolled wire rod and a manufacturing method, which adopts a medium C-Si-Mn-Cr-Al component design, combined with low-temperature salt bath spray quenching and medium-temperature salt bath distribution heat treatment after wire drawing, to obtain a structure dominated by martensite and a small amount of residual austenite and tempered martensite, achieving a tensile strength of more than 1200MPa, but the strength is not high enough and the plasticity is obviously insufficient, and there is still a problem of yield rate damage. In the non-quenched and tempered production process of 13.9-grade bolts, it is necessary to increase the strength by a large area reduction rate, which aggravates the risk of wire breakage during drawing and cracking during cold heading.
[0005] (2) In order to reduce material costs, the carbon content in the steel is increased and the alloy content is reduced. For example, patent CN113802063A discloses a method for producing medium-high carbon quenching-free cold heading steel wire rod, which adopts a composition design of C-Si-Mn-Cr-Mo-V-Al with C=0.50~0.60, combined with continuous casting secondary cooling, low-temperature wire drawing, and first fast and then slow cooling after rolling to obtain a metallographic structure of fine pearlite + a small amount of broken network ferrite. The hot-rolled tensile strength of the wire rod is ≥1020MPa, and the area reduction rate is ≥40%. Not only is the production cycle long, but the strength of the wire rod is obviously insufficient. If the carbon content in the structure is further increased, on the one hand, the high carbon content increases the risk of carbides precipitating in a network along the grain boundaries during cooling and forming network carbides. The presence of carbon-like carbides weakens the connection between grains and destroys the continuity of wire rod, which will cause a sharp drop in the mechanical properties of steel, especially impact toughness, and aggravate the problem of delayed fracture. On the other hand, high carbon content increases the bainite phase transformation temperature. The bainite content obtained by continuous cooling on the Stelmor air cooling line is relatively high, and the microstructure stress and dislocation density after pearlite inoculation are relatively high. The coarsening of grains and the increase in the thickness of pearlite lamellae will aggravate the difficulty of pearlite melting, which will seriously affect the plastic and toughness properties and yield rate of wire rod, and delayed fracture will occur at the stress concentration part of the notch. In the process of controlled rolling and controlled cooling, as the precipitated phase coarsens, it will also make it difficult to play the role of micro-alloy strengthening, and then in the non-quenched and tempered production process of 13.9 grade bolts, it also aggravates the risk of wire breakage during drawing and cracking during cold heading. Summary of the invention
[0006] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a cold heading steel wire rod for 13.9-grade non-quenched and tempered bolts and a manufacturing method thereof, which can be applicable to the application of 13.9-grade non-quenched and tempered bolts, reduce the risk of wire breakage during drawing and cracking during cold heading, improve the delayed fracture resistance, and have good industrial adaptability and application prospects.
[0007] The technical solution adopted by the present invention to solve its technical problem is:
[0008] A 13.9-grade cold heading steel wire rod for non-quenched and tempered bolts. The chemical composition and mass percentage of the cold heading steel wire rod include C: 0.70%-0.74%, Si: 0.15%-0.35%, Mn: 0.57%-0.77%, Cr: 0.20%-0.32%, Nb: 0.026%-0.050%, P≤0.015%, S≤0.015%, and the rest is Fe and unavoidable impurities; its microstructure includes tempered pearlite accounting for 80%-86% by volume, tempered bainite accounting for ≥7% by volume, and the rest is ferrite and fused pearlite.
[0009] The design basis of the chemical composition and mass percentage of the above-mentioned cold heading steel wire rod includes:
[0010] (1) Carbon: Element C is the main strengthening element of the present invention. It is more economical in steel than other elements. High carbon content helps to provide matrix strength of the material through solid solution strengthening and precipitation strengthening, but at the same time increases the risk of decarburization and the risk of cementite being distributed in a network along the pearlite grain boundary. If the C content is too high, the temperature of the bainite phase region will be higher, which is not conducive to microstructure control. Therefore, in order to enable the cold heading steel wire rod to achieve the final performance level of 13.9 grade fasteners through a short-time aging treatment under the annealing-free and tempering-free process, so as to facilitate microstructure control and take into account the cold deformation performance of the cold heading steel wire rod, the mass percentage of C is controlled to be 0.70%~0.74%.
[0011] (2) Silicon: Si is a good deoxidizing element during steel smelting. It can dissolve in ferrite and austenite to improve the hardness and strength of steel, inhibit grain coarsening in the first stage of molten salt controlled cooling, and is beneficial to the melting of pearlite lamellae. However, excessive silicon will increase the risk of non-metallic inclusions and decarburization, which is not conducive to the cold plastic deformation of steel. Therefore, the mass percentage of Si is controlled to be 0.20%~0.35%.
[0012] (3) Manganese: Mn is a good deoxidizer and desulfurizer in the steelmaking process. It has a solid solution strengthening effect, can improve the hardenability of steel, and promote the bainite phase transformation of the structure after a short period of controlled cooling. However, while improving the strength of steel, too high Mn content will aggravate the segregation during the solidification process of the steel billet, resulting in poor uniformity of the steel, increased overheating sensitivity and coarse grain risk of the steel, and too high Mn content will also increase material costs. Therefore, the mass percentage of Mn is controlled to be 0.57%~0.77%.
[0013] (4) Chromium: Cr is a medium-strong carbide-forming element that can significantly enhance the hardenability of the matrix and steel, promote the bainite phase transformation after a short period of controlled cooling, delay the pearlite phase transformation, and refine the pearlite plate spacing to increase the hardness. However, if the Cr content is too high, there is a risk of coarse grains under long-term high temperature in the second-stage molten salt, which will reduce the plasticity and toughness of the material. Therefore, the mass percentage of Cr is controlled to be 0.20%~0.32%.
[0014] (5) Niobium: Nb can induce precipitation through high-temperature rolling strain, which has the effect of refining the austenite grain size. At the same time, Nb can form nano-scale NbC precipitation phase through online molten salt two-stage controlled cooling, thereby improving the matrix strength of the material and the delayed fracture resistance of the material after two-stage molten salt controlled cooling. However, the cost of Nb element alloy is relatively high, which will increase the material cost. Therefore, the mass percentage of Nb is controlled to be 0.026%~0.050%.
[0015] (6) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.
[0016] The cold heading steel wire rod is designed with C-Si-Mn-Cr-Nb chemical composition, and uses high C to reduce the content of alloys such as Mn and Cr, thereby reducing material costs. Combined with the dispersion precipitation of NbC to strengthen the matrix, it also contains a certain amount of martensite or bainite hard and brittle phase structure compared to the existing low and medium C wire rods. The cold heading steel wire rod is mainly composed of tempered pearlite. Compared with troostite, the interlamellar spacing of pearlite is larger and the plasticity is better. The strength is moderate, but compared with martensite or even bainite, it has significantly higher plasticity. After tempering, the organizational stress and dislocation density are reduced, and a small amount of pearlite lamellae are melted into melted pearlite, which is beneficial to improving the plasticity and delayed fracture resistance of the cold heading steel wire rod. The cold heading steel wire rod also has It contains a small amount of tempered bainite. Bainite has significantly improved strength compared with pearlite, but as a hard and brittle phase structure, it obviously damages the plasticity of the wire rod. After tempering and transformation into tempered bainite, the dislocation density and distortion are significantly reduced. It has both the strength characteristics of bainite and significantly improved plasticity, and then cooperates with the high carbon component system, nano-scale NbC precipitation phase and tempered pearlite structure to provide higher matrix strength. The structure also contains a small amount of inevitable soft phase ferrite structure. Combined with the tempering of pearlite and bainite, and a small amount of fused pearlite, the plasticity of the wire rod is significantly improved, so that the cold heading steel wire rod has both high strength and high plasticity, which can meet the cold heading performance and performance grade requirements of 13.9 grade non-quenched and tempered bolts.
[0017] Preferably, the lamellar spacing of the tempered pearlite is 150-200 nm, which is relatively small, which is beneficial to the melting of pearlite lamellae to form fused pearlite and softening the matrix, and also avoids the disadvantage of too small lamellar spacing on the plasticity and cold heading performance of the wire rod.
[0018] Preferably, the volume percentage of the tempered bainite is 7% to 13%, and the volume percentage of the ferrite is 2% to 6%. The higher the proportion of tempered bainite, the higher the strength of the cold heading steel wire rod and the lower the plasticity. The higher the proportion of ferrite is accompanied by an increase in the spacing between pearlite lamellae, which is unfavorable to the strength of the cold heading steel wire rod and the melting of pearlite lamellae. Therefore, the proportion of tempered bainite and ferrite can be further controlled to adjust the strength and plasticity matching of the cold heading steel wire rod.
[0019] Preferably, the network carbide of the cold heading steel wire rod is level 0, which can effectively reduce the level of the network carbide, improve the continuity of the metal, avoid the deterioration of the plasticity and toughness of the wire rod by the network carbide, and further improve the cold deformation performance of the cold heading steel wire rod.
[0020] Preferably, the diameter of the cold heading steel wire rod is 6.0~12.0mm, the tensile strength is 1260~1310MPa, and the cross-sectional shrinkage rate is 46%~50%. It has significantly improved tensile strength and a high cross-sectional shrinkage rate. The risk of wire breakage and cold heading cracking is reduced under the annealing-free and tempering-free process. The performance grade of 13.9 can be achieved through drawing with a small area reduction rate and simple aging treatment. Compared with blank processing, it is also suitable for the manufacture of small-specification bolts and has good application prospects.
[0021] A manufacturing method for a 13.9-grade non-quenched and tempered cold heading steel wire rod for bolts, the manufacturing method comprising: producing a wire rod by controlled rolling according to the chemical composition of the above-mentioned 13.9-grade non-quenched and tempered cold heading steel wire rod, after the wire rod is spun into a wire rod at a spinning temperature of ≥880°C, performing an online molten salt two-stage controlled cooling treatment, so that the wire rod first undergoes a first-stage molten salt controlled cooling, is cooled to a bainite phase region at a cooling rate of ≥35°C / s for a transient phase transformation, then undergoes a second-stage molten salt controlled cooling, is heated to a pearlite phase region for an isothermal transformation, and simultaneously promotes high-temperature tempering of bainite and pearlite, melts and transforms pearlite lamellae into melted pearlite, softens the matrix, disperses and precipitates NbC, and finally undergoes roller slow cooling to produce a cold heading steel wire rod having a microstructure including 80% to 86% by volume of tempered pearlite, ≥7% by volume of tempered bainite, and the rest being ferrite and melted pearlite.
[0022] The above manufacturing method adopts an appropriate spinning temperature based on the high C-Si-Mn-Cr-Nb chemical composition to avoid the precipitation of network carbides during the spinning process. After spinning, the online molten salt two-stage controlled cooling treatment is directly carried out. The wire rod undergoes the first stage of molten salt controlled cooling. On the one hand, compared with the Stelmore air-cooling rapid cooling process, it can quickly skip the temperature range in which carbides precipitate in a network along the grain boundary, thereby reducing the level of network carbides. At the same time, compared with air cooling, the molten salt heat exchange can fully contact the wire rod, thereby reducing the temperature difference of the wire rod. On the other hand, combined with the composition characteristics of high C and a certain hardenability, the wire rod is caused to quickly drop from the spinning temperature to the bainite phase region. After a short period of molten salt controlled cooling, a small amount of high-temperature austenite in the wire rod structure is transformed into a bainite structure, thereby controlling the bainite content in the wire rod.
[0023] After the second stage of molten salt controlled cooling, on the one hand, compared with the continuous slow cooling of Stelmor insulation, the wire rod can be quickly heated from the bainite phase area to the pearlite phase area, and the wire rod is controlled to undergo a long-term isothermal transformation in the pearlite phase area. The residual austenite structure after the first stage of molten salt controlled cooling is transformed into pearlite and a small amount of ferrite structure, and the pearlite content is controlled. On the other hand, the NbC that was not completely precipitated in the controlled rolling stage can be dispersed and precipitated to play a strengthening role. The newly formed pearlite and bainite are tempered and softened under the action of high temperature isothermal for a longer time, reducing the organizational stress and dislocation density, promoting the continuous melting of pearlite lamellae at high temperature to form melting carbides, and softening the matrix. , and then adjust the organization, and finally slow cooling on a roller to further promote the softening of the organization, and obtain a mixed organization composed of tempered pearlite as the main part, a small amount of tempered bainite, ferrite and fused carbide. The high-carbon component system improves the strength of the cold heading steel wire rod. Compared with the directly doped martensite or bainite organization in the organization, the cold heading steel wire rod has higher plasticity through tempering regulation, which can avoid the brittle fracture problem in the downstream unwinding, transportation and even winding process, and the yield rate is guaranteed. Then, the high-carbon and relatively low-cost component system is appropriately applied to the cold heading steel wire rod for 13.9 grade non-quenched and tempered bolts, which has good industrial adaptability and yield rate.
[0024] Preferably, before the controlled rolling, the steel billet soaking temperature is controlled to be ≤1090°C and the soaking time is controlled to be ≤2h, which can promote uniform diffusion of components and avoid decarburization and grain growth problems caused by high soaking temperature, thus preparing for rolling.
[0025] Preferably, during the controlled rolling, the initial rolling temperature is controlled to be 1030~1070℃, the initial rolling reduction is 38%~45%, and low temperature rolling and large initial rolling reduction are used to promote the precipitation of a small amount of Nb (C, N) microalloy and inhibit the growth of austenite grains, which is beneficial to the strengthening and toughening of the wire rod. At the same time, it is avoided that the initial rolling reduction is too large, causing excessive precipitation of Nb in the early stage of rolling, the austenite cannot be sufficiently extended, and the final carbide size is larger, which is not conducive to the control of the dispersion precipitation of NbC in the online molten salt second-stage controlled cooling process.
[0026] Preferably, during the controlled rolling, the final rolling temperature is controlled to be ≥900°C, and the final rolling reduction is 25% to 36%. The appropriate final rolling temperature and a large final rolling reduction are used to promote the precipitation of Nb (C, N) microalloys and the corresponding deformation-induced precipitation pinning of grain boundaries. By inhibiting the growth of austenite grains, the segmented precipitation of Nb in the controlled rolling stage is further controlled, thereby promoting the grain refinement effect and improving the delayed fracture threshold.
[0027] Preferably, the spinning temperature is 880-920° C., which can reduce the tendency of grain growth, is beneficial to increase the pearlite phase deformation nucleation rate, and is beneficial to the melting of pearlite lamellae.
[0028] Preferably, the molten salt temperature of the first stage molten salt controlled cooling is 480~520℃, and the processing time is 5~12s. Since the wire rod is rapidly reduced from the spinning temperature to the molten salt temperature after passing through the first stage molten salt, the lower the molten salt temperature and the longer the processing time, the more austenite is converted into bainite structure. After the second stage molten salt controlled cooling, the proportion of tempered bainite increases, the strength of the cold heading steel wire rod increases, and the plasticity decreases. However, if the molten salt temperature is too low, martensite structure will be produced, which is not good for the plasticity of the wire rod. If the processing time is too long, the proportion of tempered bainite in the structure is too high, which is not good for the pearlite phase transformation. Therefore, the molten salt temperature and processing time of the first stage molten salt controlled cooling can be further regulated to control the wire rod to undergo short-term phase transformation in the bainite phase region and control the bainite content of the wire rod.
[0029] Preferably, the molten salt circulation rate of the first stage molten salt controlled cooling is 460-660 t / h, and the molten salt temperature rise is ≤10°C, which can further control the temperature accuracy of the first stage molten salt controlled cooling and control the wire rod structure.
[0030] Preferably, the molten salt temperature of the second-stage molten salt controlled cooling is 580-625°C, and the processing time is 450-650s. Since the wire rod is rapidly heated from the bainite phase region to the molten salt temperature corresponding to the pearlite phase region after passing through the second-stage molten salt, the higher the molten salt temperature, the larger the interlamellar spacing of the tempered pearlite, the higher the ferrite content, the wire rod strength decreases, the plasticity increases, and the higher energy is beneficial to the melting of the pearlite lamellae, but the molten salt temperature is too high and is not conducive to the precipitation of NbC. On the contrary, the lower the molten salt temperature, the smaller the interlamellar spacing of the tempered pearlite, the higher the tempered pearlite content, but the molten salt temperature is too low and is not conducive to the control of the content of bainite and pearlite. The longer the processing time, the more molten pearlite is melted, and the higher the ferrite content, the more ferrite is melted. The better the effect of high-temperature tempering to soften the matrix, the lower the strength of the wire rod and the higher the plasticity. However, if the treatment time is too long, there is a risk of NbC precipitation and coarsening, which is not conducive to the strength and plasticity. On the contrary, the shorter the treatment time, the weaker the high-temperature tempering softening effect, the wire rod strength increases and the plasticity decreases. However, if the treatment time is too short, it is not conducive to the inoculation of pearlite and the full tempering of pearlite and bainite structures. Therefore, further controlling the molten salt temperature and treatment time of the second-stage molten salt controlled cooling can make NbC evenly dispersed through appropriate high-temperature isothermal tempering, control the tempered pearlite content and lamellar spacing, reduce organizational stress and dislocation density, further regulate the wire rod organization and strength and plasticity matching, and improve delayed fracture resistance.
[0031] Preferably, the molten salt circulation rate of the second-stage molten salt controlled cooling is 150~360t / h, and the molten salt temperature rise is ≤5°C, which can regulate the accuracy of the long-term isothermal transformation of the wire rod in the pearlite phase region. At the same time, compared with the first-stage molten salt controlled cooling, the required molten salt circulation rate is smaller and the energy consumption is lower.
[0032] Preferably, the roller slow cooling adopts the insulation cover of the insulation roller to close, and the wire rod is controlled to be cooled to below 350°C at a cooling rate of 0.4~1.5°C / s, and then transported to the coiling station at a roller speed of 0.5~0.7m / s. Preferably, the initial roller speed is 0.15~0.4m / s. The high temperature state of the wire rod in the pearlite phase region after coming out of the second stage molten salt can be utilized. During the roller slow cooling process, the high temperature tempering softening effect of the second stage molten salt controlled cooling can be continued by slowly cooling. The matrix is further softened. The softening effect weakens after the temperature is below 350°C. By increasing the roller speed, the wire rod can be quickly transported to the coiling station so that it can be quickly offline and the production rhythm can be improved.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) In view of the fact that there is little development of existing 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts, the present invention adopts C-Si-Mn-Cr-Nb chemical composition design, uses C as the main strengthening component, reduces the content of alloys such as Mn and Cr, reduces material costs, retains the moderate strength of pearlite by tempering pearlite, combines the dispersion precipitation of NbC to strengthen the matrix and a small amount of tempered bainite to provide matrix strength, significantly reduces the microstructure stress and dislocation density under tempering control, and promotes the The lamellar melting forms fused pearlite, and a mixed structure composed mainly of tempered pearlite, a small amount of tempered bainite, ferrite and fused carbide is obtained, so that the strength and plasticity of the cold heading steel wire rod can be matched, and the tensile strength can reach 1260~1310MPa, the cross-sectional shrinkage rate is 46%~50%, and the network carbide is level 0. It can be suitable for 13.9 grade non-quenched and tempered bolts, reduce the risk of wire breakage during drawing and cracking during cold heading, improve the delayed fracture resistance, and has good application prospects.
[0035] (2) The manufacturing method of the present invention is based on the composition and further combines the online molten salt two-stage controlled cooling and roller slow cooling technology after spinning. The rapid cooling after spinning is used to significantly reduce the level of network carbides. At the same time, the wire rod is first controlled to undergo a short-term phase transformation in the bainite phase region to control the bainite content of the wire rod. The wire rod is then controlled to undergo a long-term isothermal transformation in the pearlite phase region to control the pearlite content of the wire rod. The bainite and pearlite structures are then promoted to undergo high-temperature tempering, the pearlite lamellae are melted, the matrix is softened, and the wire rod structure is further softened through roller slow cooling. The cold heading steel wire rod structure is regulated to match strength and plasticity, and has good industrial adaptability and yield rate.
[0036] (3) The manufacturing method of the present invention utilizes controlled rolling to promote the precipitation of Nb (C, N) microalloys, which induces the precipitation to pin the grain boundaries and promote the grain refinement effect, which is beneficial to the melting of pearlite lamellae and reduces the tendency of delayed fracture. The Nb that is not completely precipitated during the controlled rolling process is further dispersed and precipitated to form a nano-scale NbC precipitation phase through the online molten salt two-stage controlled cooling control, which can better play the microalloying role of Nb, further improve the matrix strength and delayed fracture threshold of the material, and has good industrial adaptability. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0038] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;
[0039] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;
[0040] Figure 3 It is the metallographic structure diagram of Example 3 of the present invention. DETAILED DESCRIPTION
[0041] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention. They should not be construed as limiting the scope of the present invention, which is limited only by the appended claims. Embodiment 1:
[0042] A preferred embodiment of the manufacturing method of the 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include C: 0.72%, Si: 0.35%, Mn: 0.67%, Cr: 0.3%, Nb: 0.026%, P: 0.012%, S: 0.015%, and the rest are Fe and unavoidable impurities; the manufacturing method thereof is manufactured according to the process flow of controlled rolling → wire laying → online molten salt two-stage controlled cooling → roller slow cooling → coiling, specifically:
[0043] The controlled rolling and controlled cooling is used to heat a steel billet with a specification of 180mm×180mm through a heating furnace to promote the homogenization of the steel billet composition and avoid decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 10mm through a rolling line. Appropriate rolling temperature and reduction are selected to promote the precipitation of Nb (C, N) microalloys, corresponding deformation-induced segmented precipitation, pinning of grain boundaries, grain refinement, and increased delayed fracture threshold. Specifically: the steel billet soaking temperature is controlled to be 1075°C, the soaking time is 1.5h, the initial rolling temperature is 1055°C, the initial rolling reduction is 39%, the final rolling temperature is 935°C, and the final rolling reduction is 29%.
[0044] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller. Through an appropriate spinning temperature, the wire rod is prevented from precipitating network carbides during the spinning stage, the tendency of grain growth is reduced, and conditions are created for the pearlite phase deformation nucleus. Specifically, the spinning temperature is controlled to be 915°C.
[0045] The online molten salt two-stage controlled cooling adopts two salt bath tanks with molten salt inside. The wire rod after spinning is conveyed by rollers through the first salt bath tank, and is quickly cooled to the molten salt temperature, and the first stage of molten salt controlled cooling is performed, so that the wire rod is cooled to the bainite phase region at a cooling rate of 38°C / s, and the temperature range in which carbides precipitate from austenite along grain boundaries in a network is quickly skipped, and the wire rod is controlled to undergo a short-term phase transformation in the bainite phase region, and the bainite content of the wire rod is controlled. The wire rod coming out of the first salt bath tank is then conveyed by rollers through the second salt bath tank, and is quickly transformed to the molten salt temperature, and the second stage of molten salt controlled cooling is performed, and the wire rod is controlled to undergo a long-term isothermal transformation in the pearlite phase region. , control the pearlite content of the wire rod, and promote high-temperature tempering of bainite and pearlite, the melting of pearlite lamellae is transformed into melting pearlite, and the dispersion and precipitation of NbC are controlled, and the high-temperature softening and tempering state are regulated, the organizational stress and dislocation density are reduced, the matrix is softened, and the delayed fracture resistance is improved. Specifically: the molten salt temperature of the first stage molten salt controlled cooling is 509°C, the processing time is 8s, the molten salt circulation volume is 515t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the second stage molten salt controlled cooling is 593°C, the processing time is 625s, the molten salt circulation volume is 220t / h, and the molten salt temperature rise is ≤5°C.
[0046] The roller slow cooling process adopts the roller insulation cover to be closed, and the wire rod coming out of the second salt bath tank is conveyed by rollers into the insulation cover for slow cooling treatment to promote further softening of the wire rod structure. Specifically: the initial roller speed is 0.2m / s, and the wire rod is cooled to 340°C at a cooling rate of 0.6°C / s, and then the roller speed is increased to 0.65m / s for conveying until coiling; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 304°C. After packaging and storage, the cold heading steel wire rod product is obtained, and its metallographic structure diagram is as follows Figure 1 shown.
[0047] Comparative Example 1:
[0048] A method for manufacturing hot-rolled wire rod, which differs from Example 1 in that: the method is manufactured according to the process flow of controlled rolling → wire laying → Stelmor rapid cooling → roller slow cooling → coiling. Specifically: the Stelmor rapid cooling is to open 1~6# fans at 95%, so that the wire rod is cooled to 615°C at a cooling rate of 9.7°C / s; the roller slow cooling is to close all fans and insulation covers, so that the wire rod completes phase change at a cooling rate of 1.6°C / s in the cover, and the finished wire rod is obtained after coiling off the line.
[0049] Comparative Example 2:
[0050] A method for manufacturing a hot-rolled wire rod, which differs from Example 1 in that: the steel billet soaking temperature is controlled to be 1100°C, the soaking time is 2h, the initial rolling temperature is 1080°C, the initial rolling reduction is 52%, the final rolling temperature is 950°C, the final rolling reduction is 40%, the wire laying temperature is 930°C, and the finished wire rod is obtained after coiling and rolling off the line.
[0051] Comparative Example 3:
[0052] A method for manufacturing a hot-rolled wire rod, which differs from Example 1 in that: the steel billet soaking temperature is controlled to be 950°C, the soaking time is 2h, the initial rolling temperature is 915°C, the final rolling temperature is 885°C, the spinning temperature is 860°C, the wire rod is cooled to a bainite phase region at a cooling rate of 34°C / s, and the finished wire rod is obtained after being rolled off the line. Embodiment 2:
[0053] A preferred embodiment of the manufacturing method of the 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include C: 0.71%, Si: 0.33%, Mn: 0.77%, Cr: 0.32%, Nb: 0.043%, P: 0.014%, S: 0.012%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt two-stage controlled cooling → roller slow cooling → coiling, specifically:
[0054] The controlled rolling and controlled cooling is used to heat a steel billet with a specification of 180mm×180mm through a heating furnace to promote the homogenization of the steel billet composition and avoid decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 8mm through a rolling line. Appropriate rolling temperature and reduction are selected to promote the precipitation of Nb (C, N) microalloys, corresponding deformation-induced segmented precipitation, pinning of grain boundaries, grain refinement, and increased delayed fracture threshold. Specifically: the steel billet soaking temperature is controlled to be 1065°C, the soaking time is 2h, the initial rolling temperature is 1040°C, the initial rolling reduction is 42%, the final rolling temperature is 915°C, and the final rolling reduction is 33%.
[0055] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller. Through an appropriate spinning temperature, the wire rod is prevented from precipitating network carbides during the spinning stage, the tendency of grain growth is reduced, and conditions are created for the pearlite phase deformation nucleus. Specifically, the spinning temperature is controlled to be 895°C.
[0056] The online molten salt two-stage controlled cooling adopts two salt bath tanks with molten salt inside. The wire rod after spinning is conveyed by rollers through the first salt bath tank, and is quickly cooled to the molten salt temperature, and the first stage of molten salt controlled cooling is performed, so that the wire rod is cooled to the bainite phase region at a cooling rate of 37°C / s, and the temperature range in which carbides precipitate from austenite along grain boundaries in a network is quickly skipped, and the wire rod is controlled to undergo a short-term phase transformation in the bainite phase region, and the bainite content of the wire rod is controlled. The wire rod coming out of the first salt bath tank is then conveyed by rollers through the second salt bath tank, and is quickly transformed to the molten salt temperature, and the second stage of molten salt controlled cooling is performed, and the wire rod is controlled to undergo a long-term isothermal transformation in the pearlite phase region. , control the pearlite content of the wire rod, and promote high-temperature tempering of bainite and pearlite, the melting of pearlite lamellae is transformed into melting pearlite, and the dispersion and precipitation of NbC are controlled, and the high-temperature softening and tempering state are regulated, the organizational stress and dislocation density are reduced, the matrix is softened, and the delayed fracture resistance is improved. Specifically: the molten salt temperature of the first stage molten salt controlled cooling is 493°C, the processing time is 10s, the molten salt circulation volume is 485t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the second stage molten salt controlled cooling is 625°C, the processing time is 450s, the molten salt circulation volume is 330t / h, and the molten salt temperature rise is ≤5°C.
[0057] The roller slow cooling process adopts the roller insulation cover to be closed, and the wire rod coming out of the second salt bath tank is conveyed by rollers into the insulation cover for slow cooling treatment to promote further softening of the wire rod structure. Specifically: the initial roller speed is 0.4m / s, and the wire rod is cooled to 315℃ at a cooling rate of 1.5℃ / s, and then the roller speed is increased to 0.5m / s for conveying until coiling; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 300℃. After packaging and storage, the finished cold heading steel wire rod is obtained, and its metallographic structure diagram is as follows Figure 2 shown.
[0058] Comparative Example 4:
[0059] A method for manufacturing a hot-rolled wire rod, which differs from Example 2 in that: the molten salt temperature of the first stage molten salt controlled cooling is 460°C, the processing time is 16s, the wire rod is cooled to the bainite phase region at a cooling rate of 38°C / s, the molten salt circulation rate is 680t / h, and the molten salt temperature rise is ≤10°C; the finished wire rod is obtained after the coil is rolled off the line.
[0060] Comparative Example 5:
[0061] A method for manufacturing a hot-rolled wire rod, which differs from Example 2 in that: the molten salt temperature of the first stage molten salt controlled cooling is 535°C, the processing time is 5s, the wire rod is cooled to the bainite phase region at a cooling rate of 35°C / s, the molten salt circulation rate is 470t / h, and the molten salt temperature rise is ≤10°C; the finished wire rod is obtained after the coil is rolled off the line. Embodiment 3:
[0062] A preferred embodiment of the manufacturing method of the 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include C: 0.7%, Si: 0.15%, Mn: 0.65%, Cr: 0.28%, Nb: 0.034%, P: 0.015%, S: 0.012%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt two-stage controlled cooling → roller slow cooling → coiling, specifically:
[0063] The controlled rolling and controlled cooling is used to heat a steel billet with a specification of 180mm×180mm through a heating furnace to promote the homogenization of the steel billet composition and avoid decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 6mm through a rolling line. Appropriate rolling temperature and reduction are selected to promote the precipitation of Nb (C, N) microalloys, corresponding deformation-induced segmented precipitation, pinning of grain boundaries, grain refinement, and increased delayed fracture threshold. Specifically: the steel billet soaking temperature is controlled to be 1090°C, the soaking time is 2h, the initial rolling temperature is 1070°C, the initial rolling reduction is 45%, the final rolling temperature is 945°C, and the final rolling reduction is 36%.
[0064] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller. Through an appropriate spinning temperature, the wire rod is prevented from precipitating network carbides during the spinning stage, the tendency of grain growth is reduced, and conditions are created for the pearlite phase deformation nucleus. Specifically, the spinning temperature is controlled to be 920°C.
[0065] The online molten salt two-stage controlled cooling adopts two salt bath tanks with molten salt inside. The wire rod after spinning is conveyed by rollers through the first salt bath tank, and is quickly cooled to the molten salt temperature, and the first stage of molten salt controlled cooling is performed, so that the wire rod is cooled to the bainite phase region at a cooling rate of 39°C / s, and the temperature range in which carbides precipitate from austenite along grain boundaries in a network is quickly skipped, and the wire rod is controlled to undergo a short-term phase transformation in the bainite phase region, and the bainite content of the wire rod is controlled. The wire rod coming out of the first salt bath tank is then conveyed by rollers through the second salt bath tank, and is quickly transformed to the molten salt temperature, and the second stage of molten salt controlled cooling is performed, and the wire rod is controlled to undergo a long-term isothermal transformation in the pearlite phase region. , control the pearlite content of the wire rod, and promote high-temperature tempering of bainite and pearlite, the melting of pearlite lamellae is transformed into melting pearlite, and the dispersion and precipitation of NbC are controlled, and the high-temperature softening and tempering state are regulated, the organizational stress and dislocation density are reduced, the matrix is softened, and the delayed fracture resistance is improved. Specifically: the molten salt temperature of the first stage molten salt controlled cooling is 480°C, the processing time is 12s, the molten salt circulation volume is 660t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the second stage molten salt controlled cooling is 613°C, the processing time is 542s, the molten salt circulation volume is 360t / h, and the molten salt temperature rise is ≤5°C.
[0066] The roller slow cooling process adopts the roller insulation cover to be closed, and the wire rod coming out of the second salt bath tank is conveyed by rollers into the insulation cover for slow cooling treatment to promote further softening of the wire rod structure. Specifically: the initial roller speed is 0.3m / s, and the wire rod is cooled to 335℃ at a cooling rate of 1.2℃ / s, and then the roller speed is increased to 0.6m / s for conveying until coiling; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 305℃. After packaging and storage, the finished cold heading steel wire rod is obtained, and its metallographic structure diagram is as follows Figure 3 shown.
[0067] Comparative Example 6:
[0068] A method for manufacturing a hot-rolled wire rod, which differs from Example 3 in that: the molten salt temperature of the two-stage molten salt controlled cooling is 640°C, the processing time is 380s, the molten salt circulation rate is 410t / h, and the molten salt temperature rise is ≤5°C; the finished wire rod is obtained after the coil is rolled off the line.
[0069] Comparative Example 7:
[0070] A method for manufacturing a hot-rolled wire rod, which differs from Example 3 in that: the molten salt temperature of the two-stage molten salt controlled cooling is 560°C, the processing time is 700s, the molten salt circulation volume is 180t / h, and the molten salt temperature rise is ≤5°C; the finished wire rod is obtained after the coil is rolled off the line.
[0071] Comparative Example 8:
[0072] A method for manufacturing a hot-rolled wire rod, the manufacturing method of which is different from that of Example 3 in that the treatment time of the second-stage molten salt controlled cooling is 800s, and the finished wire rod is obtained after the coil is rolled off the production line. Embodiment 4:
[0073] A preferred embodiment of the manufacturing method of the 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include C: 0.74%, Si: 0.28%, Mn: 0.57%, Cr: 0.2%, Nb: 0.05%, P: 0.015%, S: 0.014%, and the rest are Fe and unavoidable impurities; the manufacturing method thereof is manufactured according to the process flow of controlled rolling → wire laying → online molten salt two-stage controlled cooling → roller slow cooling → coiling, specifically:
[0074] The controlled rolling and controlled cooling is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to promote the homogenization of the components of the steel billet and avoid decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 12mm through a rolling line. Appropriate rolling temperature and reduction are selected to promote the precipitation of Nb (C, N) microalloys, corresponding deformation-induced segmented precipitation, pinning of grain boundaries, grain refinement, and increased delayed fracture threshold. Specifically, the steel billet soaking temperature is controlled to be 1045°C, the soaking time is 1.8h, the initial rolling temperature is 1030°C, the initial rolling reduction is 38%, the final rolling temperature is 900°C, and the final rolling reduction is 25%.
[0075] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller. Through an appropriate spinning temperature, the wire rod is prevented from precipitating network carbides during the spinning stage, the tendency of grain growth is reduced, and conditions are created for the deformation nucleus of the pearlite phase. Specifically, the spinning temperature is controlled to be 880°C.
[0076] The online molten salt two-stage controlled cooling adopts two salt bath tanks with molten salt inside. The wire rod after spinning is conveyed by rollers through the first salt bath tank, and is quickly cooled to the molten salt temperature, and the first stage of molten salt controlled cooling is performed, so that the wire rod is cooled to the bainite phase region at a cooling rate of 35°C / s, and the temperature range in which carbides precipitate from austenite along grain boundaries in a network is quickly skipped, and the wire rod is controlled to undergo a short-term phase transformation in the bainite phase region, and the bainite content of the wire rod is controlled. The wire rod coming out of the first salt bath tank is then conveyed by rollers through the second salt bath tank, and is quickly transformed to the molten salt temperature, and the second stage of molten salt controlled cooling is performed, and the wire rod is controlled to undergo a long-term isothermal transformation in the pearlite phase region. , control the pearlite content of the wire rod, and promote high-temperature tempering of bainite and pearlite, the melting of pearlite lamellae is transformed into melting pearlite, and the dispersion and precipitation of NbC are controlled, and the high-temperature softening and tempering state are regulated, the organizational stress and dislocation density are reduced, the matrix is softened, and the delayed fracture resistance is improved. Specifically: the molten salt temperature of the first stage molten salt controlled cooling is 520°C, the processing time is 5s, the molten salt circulation volume is 460t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the second stage molten salt controlled cooling is 580°C, the processing time is 650s, the molten salt circulation volume is 150t / h, and the molten salt temperature rise is ≤5°C.
[0077] The roller slow cooling process adopts the roller insulation cover to be closed, and the wire rod coming out of the second salt bath tank is conveyed by rollers into the insulation cover for slow cooling treatment to promote further softening of the wire rod structure. Specifically: the initial roller speed is 0.15m / s, and the wire rod is cooled to 348°C at a cooling rate of 0.4°C / s, and then the roller speed is increased to 0.7m / s for conveying until it is coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 310°C. After packaging and warehousing, the finished cold heading steel wire rod is obtained.
[0078] Comparative Example 9:
[0079] A method for manufacturing a hot-rolled wire rod, which differs from Example 4 in that: the method is manufactured according to the process flow of controlled rolling → spinning → online molten salt two-stage controlled cooling → air cooling → coiling, and the air cooling process adopts a roller insulation cover to open, and the wire rod coming out of the second salt bath tank is transported by a roller for air cooling treatment. The roller speed is 0.7m / s, the wire rod is cooled at a cooling rate of 2.5℃ / s, the coiling temperature is 300℃, and the finished wire rod is obtained after the coiling is off the line.
[0080] The wire rods obtained in the above embodiments and comparative examples were subjected to organizational and performance tests: the tensile test was conducted using "GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organizational test was conducted according to the metal microstructure test method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:
[0081] Table 1. Comparison of the microstructure and properties of cold heading steel wire rods with different compositions and manufacturing methods
[0082]
[0083] From the comparison results of Example 1 and Comparative Example 1, it can be seen that compared with the Stelmore fast cooling + slow cooling process, although a certain proportion of troostite structure with finer interlamellar spacing can be obtained, the level of network carbide is still relatively high. At the same time, the high carbon content makes the bainite phase transition temperature higher. The bainite content obtained by continuous cooling on the Stelmore air cooling line is relatively high, and the organizational stress and dislocation density are relatively high, which seriously affects the plasticity and toughness properties and yield rate of the wire rod. The present invention adopts the C-Si-Mn-Cr-Nb chemical composition design, combined with the online molten salt two-stage controlled cooling and roller slow cooling technology after spinning, and the rapid cooling significantly reduces the level of network carbide, and at the same time controls the wire rod in the bainite The short-term phase transformation in the bulk phase region is controlled to control the bainite content of the wire rod. The wire rod is then controlled to undergo a long-term isothermal transformation in the pearlite phase region to control the pearlite content of the wire rod, and high-temperature tempering of the bainite and pearlite structures is promoted. The pearlite lamellar layers are melted, which effectively solves the problem of matrix strength and plasticity matching. The high-carbon component system is applied to the cold heading steel wire rod, which can achieve a tensile strength of 1260~1310MPa and a cross-sectional shrinkage rate of 46%~50%. The network carbide is level 0, which can be suitable for 13.9-level non-quenched and tempered bolts, reducing the risk of wire breakage during drawing and cold heading cracking, and improving the delayed fracture resistance. It has good application prospects.
[0084] From the comparison results of Example 1 and Comparative Example 2, it can be seen that compared with high temperature rolling and large initial rolling reduction, the present invention uses appropriate initial rolling, final rolling temperature and reduction to promote the precipitation of Nb (C, N) microalloy phase transformation induced precipitation pinning grain boundaries, which can further control the segmented precipitation of Nb in the controlled rolling stage, promote the grain refinement effect, play the role of fine grain strengthening and toughening, and improve the delayed fracture threshold; from the comparison results of Example 1 and Comparative Example 3, it can be seen that compared with the low temperature spinning, which is unfavorable for controlling the precipitation of net carbon, the present invention can further use a suitable spinning temperature to reduce the tendency of grain growth, and is beneficial to increasing the pearlite phase deformation nucleation rate, which is beneficial to the melting of pearlite lamellae and reducing the wear of the rolling line.
[0085] From the comparison results of Examples 1 to 4 and Comparative Example 4, it can be seen that the lower the molten salt temperature of the first stage molten salt controlled cooling and the longer the treatment time, the more austenite is converted into bainite structure, and the proportion of tempered bainite increases after the second stage molten salt controlled cooling, and the strength of the cold heading steel wire rod increases and the plasticity decreases; from the comparison results of Examples 1 to 4 and Comparative Example 5, it can be seen that the higher the molten salt temperature of the first stage molten salt controlled cooling and the shorter the treatment time, the proportion of tempered bainite decreases, the strength of the cold heading steel wire rod decreases, and the plasticity increases.
[0086] From the comparison results of Examples 1 to 4 and Comparative Example 6, it can be seen that the higher the molten salt temperature of the two-stage molten salt controlled cooling and the shorter the treatment time, the larger the lamellar spacing of the tempered pearlite, the higher the ferrite content, the lower the strength of the wire rod, and the higher the plasticity. If the treatment time is too short, it is not conducive to the inoculation of pearlite, the sufficient tempering of pearlite and bainite structures, and the melting of pearlite lamellae; from the comparison results of Examples 1 to 4 and Comparative Example 7, it can be seen that the lower the molten salt temperature of the two-stage molten salt controlled cooling, the smaller the lamellar spacing of the tempered pearlite, the higher the tempered pearlite content, and the NbC is uniformly dispersed and distributed through appropriate high-temperature isothermal tempering. As the treatment time is longer, the melting pearlite increases, and the effect of high-temperature tempering to soften the matrix is better; from the comparison results of Example 3 and Comparative Example 8, it can be seen that if the treatment time is too long, there is a risk of NbC precipitation and coarsening, which is not conducive to the strong and plastic properties. Further control of the molten salt temperature and treatment time of the two-stage molten salt controlled cooling can further regulate the matching of the wire rod structure and the strong and plastic properties, and improve the delayed fracture resistance.
[0087] From the comparison results of Example 4 and Comparative Example 9, it can be seen that the high-temperature tempering softening effect of the second-stage molten salt controlled cooling can be continued by slow cooling during the roller slow cooling process, thereby further softening the matrix.
[0088] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts, It is characterized in that The chemical composition and mass percentage of the cold heading steel wire rod include C: 0.70% to 0.74%, Si: 0.15% to 0.35%, Mn: 0.57% to 0.77%, Cr: 0.20% to 0.32%, Nb: 0.026% to 0.050%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities; its microstructure includes tempered pearlite accounting for 80% to 86% by volume, tempered bainite accounting for ≥7% by volume, and the rest are ferrite and fused pearlite; The manufacturing method comprises: controlling and rolling the wire rod according to the chemical composition of the 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts, spinning the wire rod into a wire rod at a spinning temperature of ≥880°C, and then performing an online molten salt two-stage controlled cooling treatment, so that the wire rod first undergoes a first stage of molten salt controlled cooling, and is cooled to a bainite phase region at a cooling rate of ≥35°C / s for a short phase transformation, and then undergoes a second stage of molten salt controlled cooling, and is heated to a pearlite phase region for isothermal transformation, while promoting the bainite and pearlite to undergo isothermal transformation. High temperature tempering, pearlite lamellae melt and transform into fused pearlite, soften the matrix, disperse and precipitate NbC, and finally slowly cool through rollers to produce cold heading steel wire rods with a microstructure including tempered pearlite, tempered bainite, ferrite and fused pearlite; the molten salt temperature of the first stage molten salt controlled cooling is 480-520°C, and the processing time is 5-12s; the molten salt temperature of the second stage molten salt controlled cooling is 580-625°C, and the processing time is 450-650s.
2. The 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 1, It is characterized in that The interlamellar spacing of the tempered pearlite is 150-200 nm, the volume percentage of the tempered bainite is 7%-13%, the volume percentage of the ferrite is 2%-6%, and the network carbide of the cold heading steel wire rod is level 0.
3. The 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 1, It is characterized in that The cold heading steel wire rod has a diameter of 6.0-12.0 mm, a tensile strength of 1260-1310 MPa, and a cross-sectional shrinkage of 46%-50%.
4. A method for manufacturing a cold heading steel wire rod for non-quenched and tempered bolts of grade 13.9, It is characterized in that The manufacturing method comprises: producing a wire rod by controlled rolling according to the chemical composition of the 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts as claimed in claim 1, after the wire rod is spun into a wire rod at a spinning temperature of ≥880°C, an online molten salt two-stage controlled cooling treatment is performed, the wire rod is first subjected to a first stage of molten salt controlled cooling, cooled to a bainite phase region at a cooling rate of ≥35°C / s for a short phase transformation, then subjected to a second stage of molten salt controlled cooling, heated to a pearlite phase region for an isothermal transformation, and at the same time, high temperature tempering of bainite and pearlite is promoted, and pearlite lamellar melting is performed. The steel wire rod is made of a cold heading steel wire rod, wherein the steel wire rod is transformed into fused pearlite, the matrix is softened, NbC is dispersed and precipitated, and finally it is slowly cooled by a roller to form a microstructure including 80% to 86% tempered pearlite by volume, ≥7% tempered bainite by volume, and the rest is ferrite and fused pearlite; the molten salt temperature of the first stage molten salt controlled cooling is 480 to 520°C, and the processing time is 5 to 12s; the molten salt temperature of the second stage molten salt controlled cooling is 580 to 625°C, and the processing time is 450 to 650s.
5. The method for manufacturing the 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 4, It is characterized in that Before the controlled rolling, the steel billet soaking temperature is controlled to be ≤1090°C and the soaking time is controlled to be ≤2h.
6. The method for manufacturing the 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 4, It is characterized in that During the controlled rolling, the initial rolling temperature is controlled to be 1030-1070° C., and the initial rolling reduction is 38%-45%.
7. The method for manufacturing the 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 4, It is characterized in that During the controlled rolling, the final rolling temperature is controlled to be ≥900°C, the final rolling reduction is 25%-36%, and the wire laying temperature is 880-920°C.
8. The method for manufacturing the 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 4, It is characterized in that The molten salt circulation volume of the first stage molten salt controlled cooling is 460~660t / h, and the molten salt temperature rise is ≤10°C; the molten salt circulation volume of the second stage molten salt controlled cooling is 150~360t / h, and the molten salt temperature rise is ≤5°C.
9. The method for manufacturing the 13.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 4, It is characterized in that The roller slow cooling adopts the insulation cover of the insulation roller to close, and controls the wire rod to be cooled to below 350°C at a cooling rate of 0.4~1.5°C / s, and then transported to the coil at a roller speed of 0.5~0.7m / s.