A method for efficiently detecting metal ions in PTFE powder
Through the nitric acid steam extraction method and ICP-MS/MS detection, the problem of low detection rate and long time-consuming metal ion detection in PTFE powder is solved, and efficient and accurate metal ion detection is achieved, which is suitable for the high purity requirements of the semiconductor industry. .
Patent Information
- Application Number
- CN202411001569.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The existing methods for detecting metal ions in PTFE powder have low detection rates and are time-consuming, and cannot meet the high purity requirements of the semiconductor industry.
Using nitric acid steam extraction method combined with inductively coupled plasma mass spectrometry (ICP-MS/MS) detection, the PTFE powder is extracted by heating the nitric acid solution to generate steam, increasing the contact area between the solvent and the powder, and using ICP-MS/MS for depth analysis. Extraction and detection.
The detection rate of metal ions in PTFE powder is increased by more than 20%, the detection time is shortened by 60%, and the process is simple and operable, making it suitable for detection in the semiconductor field.
Smart Images

Figure CN118533592B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fluorine chemical industry, and specifically relates to a method for efficiently detecting metal ions in PTFE powder. Background Art
[0002] Polytetrafluoroethylene (PTFE) is used in aviation and military, chemical machinery, electronic appliances, 5G, semiconductors and other fields due to its excellent properties such as high purity, chemical inertness and heat resistance. However, with the rapid development of the semiconductor industry, the semiconductor field has increasingly higher requirements for the purity of various components such as fluid delivery pipes, gaskets, valves and containers used, thus putting forward stricter and more demanding requirements on the purity of PTFE resin used in the semiconductor field.
[0003] Conventional testing of metal ion content in PTFE products generally uses the inorganic acid immersion method. However, due to the strong hydrophobicity of PTFE resin powder, the PTFE powder will float on the surface of the solvent and only part of the powder can be completely immersed, resulting in a low detection rate and a long test time. For example, the PTFE powder needs to be immersed in dilute nitric acid for at least 7 days.
[0004] It can be seen that there is currently a lack of efficient and accurate methods to detect metal ions in PTFE powder materials. In the face of the rapid development of the semiconductor industry, it is extremely important to develop an efficient method for detecting metal ions in PTFE powder. Summary of the invention
[0005] The purpose of the present invention is to provide a method for efficiently detecting metal ions in PTFE powder in view of the problems that the existing methods for detecting metal ions in PTFE powder have low detection rate and are time-consuming. The detection rate of metal ions in PTFE powder detected by the method is increased by more than 20%.
[0006] The specific technical scheme is as follows: A method for efficiently detecting metal ions in PTFE powder comprises the following steps:
[0007] (1) Prepare the sample solution to be tested:
[0008] First, prepare a PFA bottle with a filter, add a nitric acid solution with a mass concentration of 8%-12% to the bottom of the PFA bottle, and then install the filter. The present invention uses nitric acid. If hydrochloric acid is used to treat PTFE powder, it will lead to the formation of several polyatomic ions, which will affect some key elements. If sulfuric acid is used, SO + The dissociation energy is high and dissociation is not likely to occur even when operating in collision mode with an inert cell gas.
[0009] Weigh the PTFE powder, spread the PTFE powder to be tested on the filter screen, and then seal another inverted empty PFA bottle at the mouth of the PFA bottle by screw sealing to obtain a sealed bottle.
[0010] Then, the sealed bottle is heated so that the nitric acid solution at the bottom of the sealed bottle forms nitric acid vapor and fills the sealed bottle. The nitric acid vapor extracts the metal ions in the PTFE powder to be tested on the filter screen for 10-15 hours. The type of metal ions detected by this method can be adjusted according to the actual needs of the PTFE product. For example, the metal ions may include barium ions, cadmium ions, chromium ions, copper ions, iron ions, manganese ions, nickel ions, and zinc ions. The nitric acid vapor penetrates and acts on the PTFE powder to be tested, and extracts the metal ions contained therein.
[0011] After the extraction is completed, wait for the sealed bottle to cool, invert and shake, and the extracted PTFE powder to be tested will fall from the filter to the bottom of another empty PFA bottle. The PTFE powder to be tested will continue to be soaked in the cooled nitric acid solution for 2-3 days to obtain the sample solution to be tested for use.
[0012] (2) Preparation of standard solution: Prepare mixed standard solutions with stepwise concentrations of the metal ions to be detected and set aside;
[0013] The nitric acid solution of the same mass concentration added to the bottom of the PFA bottle in step (1) is used as a blank control sample for later use.
[0014] (3) ICP-MS / MS test:
[0015] First, the working conditions of the inductively coupled plasma mass spectrometer were selected. In the argon mode, a blank control sample was first introduced, and then mixed standard solutions were introduced in order from low concentration to high concentration to obtain the standard curves of each metal ion.
[0016] Then, the sample solution obtained in step (1) after centrifugation is injected for testing.
[0017] (4) Calculation: Calculate the metal ion content in the sample solution according to the standard curve obtained in step (3): ;
[0018] Where c is the concentration measured by the instrument, v is the volume of nitric acid solution, m To weigh the mass of PTFE powder.
[0019] In the present invention, in step (1) of the method for efficiently detecting metal ions in PTFE powder, the mass volume ratio of PTFE powder to nitric acid is 1:15-20; and the sealed bottle is heated to a temperature of 120-130°C.
[0020] In the present invention, the mass concentration of the nitric acid solution added in step (1) of the method for efficiently detecting metal ions in PTFE powder is 10%.
[0021] In the present invention, in step (1) of the method for efficiently detecting metal ions in PTFE powder, nitric acid vapor is used to extract the metal ions in the PTFE powder to be tested on the filter for 12 hours; and the cooled nitric acid solution is used to soak the PTFE powder to be tested for 2 days.
[0022] In the present invention, the step concentrations of the mixed standard solution in step (2) of the method for efficiently detecting metal ions in PTFE powder are 10 ppb, 20 ppb, 50 ppb, and 100 ppb, respectively.
[0023] Furthermore, the preparation of the stepwise concentration mixed standard solution in step (2) is as follows:
[0024] Accurately measure 1 mL of the mixed standard solution with a concentration of 10 mg / L, dilute it to a 100 mL volumetric flask, and prepare a solution with a solubility of 100 ppb;
[0025] Accurately measure 500 μL of the mixed standard solution with a concentration of 10 mg / L, and dilute it to a 100 mL volumetric flask to make a solution with a concentration of 50 ppb;
[0026] Accurately measure 200 μL of the mixed standard solution with a concentration of 10 mg / L, and dilute it to a 100 mL volumetric flask to make a solution with a concentration of 20 ppb;
[0027] Accurately measure 100 μL of the mixed standard solution with a concentration of 10 mg / L, dilute it into a 100 mL volumetric flask, and prepare a solution with a concentration of 10 ppb.
[0028] In the present invention, the working conditions of the inductively coupled plasma mass spectrometer in step (3) of the method for efficiently detecting metal ions in PTFE powder are as follows: high frequency power is 1.2 kW, sampling depth is 5.0 mm, plasma gas is 9.0 L / min, auxiliary gas is 1.1 L / min, carrier gas is 0.7 L / min, and spray chamber temperature is 5.0°C.
[0029] In the present invention, in step (1) of the method for efficiently detecting metal ions in PTFE powder, the sealed bottle is placed on a heating plate for heating.
[0030] The beneficial effects of the present invention are as follows: the detection method of the present invention adopts a steam exposure method and an infiltration method to prepare a sample solution to be tested from PTFE powder, and uses an inductively coupled plasma mass spectrometer (ICP-MS / MS) to determine metal ions in the PTFE powder.
[0031] The PTFE powder is placed in a fully enclosed container, and the nitric acid is vaporized by heating. The nitric acid vapor fully penetrates into the pores of the powder, increasing the contact area between the nitric acid and the powder sample, achieving deep extraction of metal elements, and solving the problem of PTFE powder floating on the surface of the solution. The metal elements in the PTFE powder are enriched by a fully enclosed leaching method, effectively avoiding contamination in the intermediate process, and the test solution after centrifugation is detected by ICP-MS / MS. This method has a high detection rate, a short test cycle, a simple process, and operability. It can be widely used in the detection of metal ions in PTFE powder in the semiconductor field.
[0032] Compared with the conventional static immersion method for detecting metal ions in PTFE powder, the metal ion detection rate of PTFE powder detected by the method described in the present invention is increased by more than 20%, and the test time is shortened by 60%. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is the Ba ion concentration-intensity standard curve.
[0034] Figure 2 is the Cd ion concentration-intensity standard curve.
[0035] Figure 3 is the Cr ion concentration-intensity standard curve.
[0036] Figure 4 is the Cu ion concentration-intensity standard curve.
[0037] Figure 5 is the Fe ion concentration-intensity standard curve.
[0038] Figure 6 is the Mn ion concentration-intensity standard curve.
[0039] Figure 7 is the Ni ion concentration-intensity standard curve.
[0040] Figure 8 is the Zn ion concentration-intensity standard curve. DETAILED DESCRIPTION
[0041] The technical solution of the present invention is described in detail below in conjunction with the accompanying drawings.
[0042] Example 1
[0043] The method for efficiently detecting metal ions in PTFE powder comprises the following steps:
[0044] (1) Prepare the sample solution to be tested:
[0045] Add 30 mL of 10% nitric acid solution to the bottom of the PFA bottle equipped with a filter, weigh 2 g of PTFE powder, sieve it through a 10-mesh sieve, and spread it evenly on the filter in the PFA bottle.
[0046] After placing the sample PTFE powder and the solvent nitric acid solution, use another empty PFA bottle to spirally seal the PFA bottle containing the sample to be tested to obtain a sealed bottle, and put the sealed bottle on a heating plate. The temperature of the heating plate is set to 120°C, and the nitric acid solution is vaporized into nitric acid vapor. The sealed bottle is heated for 12 hours, that is, the nitric acid vapor extracts the metal ions in the PTFE powder to be tested for 12 hours.
[0047] After heating is completed, remove the heating plate, wait for the sealed bottle to cool, invert and shake, and the cooled nitric acid solution will soak the PTFE powder that falls from the filter screen for 2 days to complete the leaching and enrichment of metal ions in the PTFE powder.
[0048] (2) Preparation of standard solution: Accurately measure 1 mL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a solubility of 100 ppb; Accurately measure 500 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 50 ppb; Accurately measure 200 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 20 ppb; Accurately measure 100 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 10 ppb.
[0049] (3) ICP-MS / MS test samples:
[0050] The working conditions of the inductively coupled plasma mass spectrometer were selected as follows: high frequency power of 1.2 kW, sampling depth of 5.0 mm, plasma gas of 9.0 L / min, auxiliary gas of 1.1 L / min, carrier gas of 0.7 L / min, and spray chamber temperature of 5.0 °C.
[0051] After the instrument is stable, first inject the blank control sample, then inject the mixed standard solution in order from low to high concentration, and then generate a standard curve based on concentration-intensity. Figure 1 As shown, the linear correlation coefficients are all greater than 0.99, where I is the sample intensity. After obtaining the standard curve of each metal ion, the sample solution obtained in step (1) after centrifugation is injected for testing.
[0052] (4) Calculation: Calculate the metal ion content in the sample solution according to the standard curve obtained in step (3): ;
[0053] Where c is the concentration measured by the instrument,v is the volume of nitric acid solution, m To weigh the mass of PTFE powder.
[0054] By substituting the data measured by the instrument into the concentration calculation formula, the concentration of metal ions can be directly obtained.
[0055] The metal ions to be tested in this test are: barium ion, chromium ion, spacer, manganese ion, nickel ion, and zinc ion.
[0056] The ion contents detected by the method described in Example 1 are shown in Table 1.
[0057] Table 1
[0058]
[0059] The average value of the three tests in the above table can prove the accuracy of the instrument. The average of three tests is taken as the final data for each test result.
[0060] (5) In addition, 8 samples were taken that were the same as sample 1 and processed in the same way. Subsequently, the 8 samples were spiked and tested. The spiked concentration was 5 ppb.
[0061] In this embodiment, the recovery rate of the spiked sample to be tested = (measured value of the spiked sample to be tested - original value) ÷ 5 × 100%.
[0062] The specific test results are shown in Table 2 below.
[0063] Table 2
[0064]
[0065] Example 2
[0066] The difference from Example 1 is that the mass concentration of nitric acid in this embodiment is 8%, and the rest is the same as Example 1.
[0067] Example 3
[0068] The difference from Example 1 is that the mass concentration of nitric acid in this embodiment is 12%, and the rest is the same as Example 1.
[0069] Example 4
[0070] The difference from Example 1 is that the leaching time of this example is 10 hours, and the rest is the same as Example 1.
[0071] Example 5
[0072] The difference from Example 1 is that the extraction time of this example is 15 hours, and the rest is the same as Example 1.
[0073] The metal ions to be tested in this test are: barium ion, chromium ion, spacer, manganese ion, nickel ion, zinc ion. The ion contents detected by the methods described in each embodiment are shown in Table 3.
[0074] Table 3
[0075]
[0076] Comparative Example 1
[0077] In order to verify that the steam exposure method has a more positive effect on the precipitation of metal elements in PTFE powder than the static immersion method, this comparative example uses the static immersion method as a comparison, and the other steps are the same as those in Example 1.
[0078] The specific steps are as follows:
[0079] (1) Prepare the sample solution to be tested:
[0080] Take 2 g of the same PTFE powder as in Example 1, add the PTFE powder sieved through a 10-mesh sieve into a PFA bottle, take 30 g of a nitric acid solution with a mass concentration of 10% to soak the PTFE powder, and place it statically for 7 days.
[0081] (2) Preparation of standard solution: Accurately measure 1 mL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a solubility of 100 ppb; Accurately measure 500 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 50 ppb; Accurately measure 200 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 20 ppb; Accurately measure 100 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 10 ppb.
[0082] (3) ICP-MS / MS test samples:
[0083] The working conditions of the inductively coupled plasma mass spectrometer were selected as follows: high frequency power of 1.2 kW, sampling depth of 5.0 mm, plasma gas of 9.0 L / min, auxiliary gas of 1.1 L / min, carrier gas of 0.7 L / min, and spray chamber temperature of 5.0 °C.
[0084] After the instrument is stable, first inject the blank control sample, then inject the mixed standard solution in order from low to high concentration, and then generate a standard curve based on concentration-intensity. Figure 1As shown, the linear correlation coefficients are all greater than 0.99, where I is the sample intensity. After obtaining the standard curve of each metal ion, the sample solution obtained in step (1) after centrifugation is injected for testing.
[0085] (4) Calculation: Calculate the metal ion content in the sample solution according to the standard curve obtained in step (3): ;
[0086] Where c is the concentration measured by the instrument, v is the volume of nitric acid solution, m To weigh the mass of PTFE powder.
[0087] By substituting the data measured by the instrument into the concentration calculation formula, the concentration of metal ions can be directly obtained.
[0088] The metal ions to be tested in this test are: barium ion, chromium ion, spacer, manganese ion, nickel ion, and zinc ion.
[0089] The ion contents detected by the method described in this comparative example are shown in Table 4.
[0090] Comparative Example 2
[0091] In order to verify that the concentration of nitric acid will have different effects on the metal elements in the PTFE powder, this comparative example uses nitric acid with a concentration of 5% to infiltrate the PTFE powder, and the other steps are the same as those in Example 1.
[0092] The specific steps are as follows:
[0093] (1) Prepare the sample solution to be tested: add 30 mL of 5% nitric acid solution to the bottom of the PFA bottle, take 2 g of the same PTFE powder as in Example 1, sieve it through a 10-mesh sieve, and add it to the filter in the PFA bottle. After placing the sample and solvent, use another PFA bottle to screw it shut, and after sealing, put it on the heating plate. The temperature of the heating plate is set to 120°C, and the heating time of the sealed bottle is 12 hours.
[0094] After heating, remove the heating plate, cool the PFA sealed bottle, invert and shake it, and the cooled nitric acid solution will soak the powder material that falls from the filter screen. Soak for 2 days to complete the leaching and enrichment of metal ions in the powder.
[0095] (2) Preparation of standard solution: Accurately measure 1 mL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a solubility of 100 ppb; Accurately measure 500 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 50 ppb; Accurately measure 200 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 20 ppb; Accurately measure 100 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 10 ppb.
[0096] (3) ICP-MS / MS test samples:
[0097] The selected inductively coupled plasma mass spectrometry conditions were as follows: high frequency power of 1.2 kW, sampling depth of 5.0 mm, plasma gas of 9.0 L / min, auxiliary gas of 1.1 L / min, carrier gas of 0.7 L / min, and spray chamber temperature of 5.0 °C.
[0098] After the instrument is stable, first inject the blank sample, then inject the samples in order from low to high concentration, and then generate a standard curve based on concentration-intensity, such as Figure 1 As shown, the linear correlation coefficients are all greater than 0.99, where I is the sample intensity. After obtaining the standard curve of each metal ion, the sample solution obtained in step (1) after centrifugation is injected for testing.
[0099] (4) According to the concentration calculation formula, the data measured by the instrument can be directly used to obtain the concentration of metal ions. The metal ions to be measured in this test are: barium ions, chromium ions, spacers, manganese ions, nickel ions, and zinc ions.
[0100] Comparative Example 3
[0101] In order to verify that the concentration of nitric acid has different effects on the metal elements in the PTFE powder, this comparative example uses nitric acid with a concentration of 15% to wet the PTFE powder, and the other steps are the same as those in Example 1.
[0102] The specific steps are as follows:
[0103] (1) Preparation of the sample solution to be tested: Add 30 mL of 15% nitric acid solution to the bottom of the PFA bottle, weigh 2 g of the same PTFE powder as in Example 1, sieve it through a 10-mesh sieve, and add it to the filter in the PFA bottle. After placing the sample and solvent, use another PFA bottle to screw it shut, and after sealing, put it on the heating plate. The temperature of the heating plate is set to 120°C, and the heating time of the sealed bottle is 12 hours.
[0104] After heating, remove the heating plate, cool the PFA sealed bottle, invert and shake it, and the cooled nitric acid solution will soak the powder material that falls from the filter screen. Soak for 2 days to complete the leaching and enrichment of metal ions in the powder.
[0105] (2) Preparation of standard solution: Accurately measure 1 mL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a solubility of 100 ppb; Accurately measure 500 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 50 ppb; Accurately measure 200 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 20 ppb; Accurately measure 100 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 10 ppb.
[0106] (3) ICP-MS / MS test samples:
[0107] The selected inductively coupled plasma mass spectrometry conditions were as follows: high frequency power of 1.2 kW, sampling depth of 5.0 mm, plasma gas of 9.0 L / min, auxiliary gas of 1.1 L / min, carrier gas of 0.7 L / min, and spray chamber temperature of 5.0 °C.
[0108] After the instrument is stable, first inject the blank sample, then inject the samples in order from low to high concentration, and then generate a standard curve based on concentration-intensity, such as Figure 1 As shown, the linear correlation coefficients are all greater than 0.99, where I is the sample intensity. After obtaining the standard curve of each metal ion, the sample solution obtained in step (1) after centrifugation is injected for testing.
[0109] (4) According to the concentration calculation formula, the data measured by the instrument can be directly used to obtain the concentration of metal ions. The metal ions to be measured in this test are: barium ions, chromium ions, spacers, manganese ions, nickel ions, and zinc ions.
[0110] Comparative Example 4
[0111] In order to verify that the steam heating time will produce different effects on the metal elements in the PTFE powder, the heating time in this comparative example was changed to 8 hours, and the other steps were the same as those in Example 1.
[0112] The specific steps are as follows:
[0113] (1) Preparation of the sample solution to be tested: Add 30 mL of 10% nitric acid solution to the bottom of the PFA bottle, weigh 2 g of the same PTFE powder as in Example 1, sieve it through a 10-mesh sieve, and add it to the filter in the PFA bottle. After placing the sample and solvent, use another PFA bottle to screw it shut, and after sealing, put it on the heating plate. The temperature of the heating plate is set to 120°C, and the heating time of the sealed bottle is 8 hours.
[0114] After heating, remove the heating plate, cool the PFA sealed bottle, invert and shake it, and the cooled nitric acid solution will soak the powder material that falls from the filter screen. Soak for 2 days to complete the leaching and enrichment of metal ions in the powder.
[0115] (2) Preparation of standard solution: Accurately measure 1 mL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a solubility of 100 ppb; Accurately measure 500 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 50 ppb; Accurately measure 200 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 20 ppb; Accurately measure 100 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 10 ppb.
[0116] (3) ICP-MS / MS test samples:
[0117] The selected inductively coupled plasma mass spectrometry conditions were as follows: high frequency power of 1.2 kW, sampling depth of 5.0 mm, plasma gas of 9.0 L / min, auxiliary gas of 1.1 L / min, carrier gas of 0.7 L / min, and spray chamber temperature of 5.0 °C.
[0118] After the instrument is stable, first inject the blank sample, then inject the samples in order from low to high concentration, and then generate a standard curve based on concentration-intensity, such as Figure 1 As shown, the linear correlation coefficients are all greater than 0.99, where I is the sample intensity. After obtaining the standard curve of each metal ion, the sample solution obtained in step (1) after centrifugation is injected for testing.
[0119] (4) According to the concentration calculation formula, the data measured by the instrument can be directly used to obtain the concentration of metal ions. The metal ions to be measured in this test are: barium ions, chromium ions, spacers, manganese ions, nickel ions, and zinc ions.
[0120] Comparative Example 5
[0121] In order to verify that the steam heating time will produce different effects on the metal elements in the PTFE powder, the heating time in this comparative example was changed to 18 hours, and the other steps were the same as those in Example 1.
[0122] The specific steps are as follows:
[0123] (1) Preparation of the sample solution to be tested: Add 30 mL of 10% nitric acid solution to the bottom of the PFA bottle, weigh 2 g of the same PTFE powder as in Example 1, sieve it through a 10-mesh sieve, and add it to the filter in the PFA bottle. After placing the sample and solvent, use another PFA bottle to screw it shut, and after sealing, put it on the heating plate. The temperature of the heating plate is set to 120°C, and the heating time of the sealed bottle is 18 hours.
[0124] After heating, remove the heating plate, cool the PFA sealed bottle, invert and shake it, and the cooled nitric acid solution will soak the powder material that falls from the filter screen. Soak for 2 days to complete the leaching and enrichment of metal ions in the powder.
[0125] (2) Preparation of standard solution: Accurately measure 1 mL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a solubility of 100 ppb; Accurately measure 500 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 50 ppb; Accurately measure 200 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 20 ppb; Accurately measure 100 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 10 ppb.
[0126] (3) ICP-MS / MS test samples:
[0127] The selected inductively coupled plasma mass spectrometry conditions were as follows: high frequency power of 1.2 kW, sampling depth of 5.0 mm, plasma gas of 9.0 L / min, auxiliary gas of 1.1 L / min, carrier gas of 0.7 L / min, and spray chamber temperature of 5.0 °C.
[0128] After the instrument is stable, first inject the blank sample, then inject the samples in order from low to high concentration, and then generate a standard curve based on concentration-intensity, such as Figure 1 As shown, the linear correlation coefficients are all greater than 0.99, where I is the sample intensity. After obtaining the standard curve of each metal ion, the sample solution obtained in step (1) after centrifugation is injected for testing.
[0129] (4) According to the concentration calculation formula, the data measured by the instrument can be directly used to obtain the concentration of metal ions. The metal ions to be measured in this test are: barium ions, chromium ions, spacers, manganese ions, nickel ions, and zinc ions.
[0130] Comparative Example 6
[0131] In order to verify that the time for the nitric acid solution to soak the PTFE powder after cooling will affect the extraction of metal elements, the subsequent soaking time of the nitric acid solution was changed to 1 day in this comparative example, and the other steps were the same as those in Example 1.
[0132] The specific steps are as follows:
[0133] (1) Preparation of the sample solution to be tested: Add 30 mL of 10% nitric acid solution to the bottom of the PFA bottle, weigh 2 g of the same PTFE powder as in Example 1, sieve it through a 10-mesh sieve, and add it to the filter in the PFA bottle. After placing the sample and solvent, use another PFA bottle to screw it shut, and after sealing, put it on the heating plate. The temperature of the heating plate is set to 120°C, and the heating time of the sealed bottle is 12 hours.
[0134] After heating, remove the heating plate, cool the PFA sealed bottle, invert and shake it, and the cooled nitric acid solution will soak the powder material that falls from the filter screen. Soak for 1 day to complete the leaching and enrichment of metal ions in the powder.
[0135] (2) Preparation of standard solution: Accurately measure 1 mL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a solubility of 100 ppb; Accurately measure 500 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 50 ppb; Accurately measure 200 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 20 ppb; Accurately measure 100 μL of the mixed standard solution with a concentration of 10 mg / L, dilute to volume in a 100 mL volumetric flask, and prepare a solution with a concentration of 10 ppb.
[0136] (3) ICP-MS / MS test samples:
[0137] The selected inductively coupled plasma mass spectrometry conditions were as follows: high frequency power of 1.2 kW, sampling depth of 5.0 mm, plasma gas of 9.0 L / min, auxiliary gas of 1.1 L / min, carrier gas of 0.7 L / min, and spray chamber temperature of 5.0 °C.
[0138] After the instrument is stable, first inject the blank sample, then inject the samples in order from low to high concentration, and then generate a standard curve based on concentration-intensity, such as Figure 1 As shown, the linear correlation coefficients are all greater than 0.999, where I is the sample intensity. After obtaining the standard curve of each metal ion, the sample solution obtained in step (1) after centrifugation is injected for testing.
[0139] By entering the data measured by the instrument according to the concentration calculation formula, the concentration of metal ions can be directly obtained. The metal ions to be tested in this test are: barium ions, chromium ions, spacers, manganese ions, nickel ions, and zinc ions.
[0140] The metal ions to be tested in this test are: barium ion, chromium ion, spacer, manganese ion, nickel ion, zinc ion. The ion contents detected by the methods described in each comparative example are shown in Table 4.
[0141] Table 4
[0142]
[0143] From the overall experimental data in Table 4, it can be seen that the detection method of the present invention has a significant effect on the deep extraction of metal elements in powder, and the detection rate of each metal has increased by more than 20%. This process not only solves the problem of powder floating on the surface of the solution, but also increases the specific surface area between the powder and the solvent, greatly improving the detection rate of metal elements. In contrast, the powder in the static immersion method continues to float on the surface of the solution, which is not conducive to the precipitation of metal elements.
Claims
1. A method for efficiently detecting metal ions in PTFE powder, characterized in that: The following steps are involved: (1) Prepare the sample solution to be tested: First, prepare a PFA bottle equipped with a filter, add 8%-12% nitric acid solution to the bottom of the PFA bottle, and then install the filter; Weigh PTFE powder, spread the PTFE powder to be tested on the filter screen, and then seal another inverted empty PFA bottle at the mouth of the PFA bottle by screw sealing to obtain a sealed bottle; Then, the sealed bottle is heated to make the nitric acid solution at the bottom of the sealed bottle form nitric acid vapor and fill the sealed bottle, and the nitric acid vapor extracts the metal ions in the PTFE powder to be tested on the filter screen for 10-15 hours; After the extraction is completed, wait for the sealed bottle to cool, invert and shake, and the extracted PTFE powder to be tested will fall from the filter screen to the bottom of another empty PFA bottle. The PTFE powder to be tested is further infiltrated with the cooled nitric acid solution for 2-3 days to obtain a sample solution for standby use; (2) Preparation of standard solution: Prepare mixed standard solutions with stepwise concentrations of the metal ions to be detected and set aside; The nitric acid solution of the same mass concentration as added to the bottom of the PFA bottle in step (1) is used as a blank control sample for later use; (3) ICP-MS / MS test: First, the working conditions of the inductively coupled plasma mass spectrometer were selected. In the argon mode, a blank control sample was first introduced, and then mixed standard solutions were introduced in order from low concentration to high concentration to obtain the standard curves of each metal ion. Then, the sample solution obtained in step (1) after centrifugation is injected for testing; (4) Calculation: Calculate the metal ion content in the sample solution according to the standard curve obtained in step (3): ; Where c is the concentration measured by the instrument, v is the volume of nitric acid solution, m To weigh the mass of PTFE powder.
2. The method for efficiently detecting metal ions in PTFE powder according to claim 1, wherein In the step (1), the mass volume ratio of PTFE powder to nitric acid is 1:15-20; the sealed bottle is heated to a temperature of 120-130°C.
3. The method for efficiently detecting metal ions in PTFE powder according to claim 1, wherein The mass concentration of the nitric acid solution added in step (1) is 10%.
4. The method for efficiently detecting metal ions in PTFE powder according to claim 1, characterized in that: In the step (1), the nitric acid vapor extracts the metal ions in the PTFE powder to be tested on the filter screen for 12 hours; and the cooled nitric acid solution soaks the PTFE powder to be tested for 2 days.
5. The method for efficiently detecting metal ions in PTFE powder according to claim 1, characterized in that, The step concentrations of the mixed standard solution in step (2) are 10 ppb, 20 ppb, 50 ppb, and 100 ppb, respectively.
6. The method for efficiently detecting metal ions in PTFE powder according to claim 5, characterized in that: The preparation operation of the stepwise concentration mixed standard solution in step (2) is as follows: Accurately measure 1 mL of the mixed standard solution with a concentration of 10 mg / L, dilute it to a 100 mL volumetric flask, and prepare a solution with a solubility of 100 ppb; Accurately measure 500 μL of the mixed standard solution with a concentration of 10 mg / L, and dilute it to a 100 mL volumetric flask to make a solution with a concentration of 50 ppb; Accurately measure 200 μL of the mixed standard solution with a concentration of 10 mg / L, and dilute it to a 100 mL volumetric flask to make a solution with a concentration of 20 ppb; Accurately measure 100 μL of the mixed standard solution with a concentration of 10 mg / L, dilute it into a 100 mL volumetric flask, and prepare a solution with a concentration of 10 ppb.
7. The method for efficiently detecting metal ions in PTFE powder according to claim 1, characterized in that: The working conditions of the inductively coupled plasma mass spectrometer in step (3) are as follows: high frequency power of 1.2 kW, sampling depth of 5.0 mm, plasma gas of 9.0 L / min, auxiliary gas of 1.1 L / min, carrier gas of 0.7 L / min, and spray chamber temperature of 5.0°C.
8. The method for efficiently detecting metal ions in PTFE powder according to claim 1, characterized in that, In the step (1), the sealed bottle is placed on a heating plate for heating.