Low melting point lead-free solder and preparation method and application thereof

By adding a specific proportion of nanoparticles and fluoride to lead-free solder, the problem of high melting point of Sn-Ag-Cu-based solder is solved, and a lead-free solder with low melting point and high stability is achieved, which is suitable for welding of precision electronic equipment. , reducing the risk and cost of thermal damage.

CN118544027BActive Publication Date: 2024-11-15SUZHOU TONYSHARE ELECTRONICS MATERIALS TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411028648.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The melting point of existing lead-free solders such as Sn-Ag-Cu-based solder is higher than that of tin-lead solder, resulting in an increase in soldering temperature, which easily causes thermal damage and bending deformation of the substrate, and has poor thermal fatigue resistance and ductility in precision electronic equipment. , limits its application.

Method used

Bismuth 10-30%, nanosilver particles 0.6-1.8%, nanoferrous oxide particles 0.3-0.8%, dysprosium 0.02-0.1%, indium 0.2-0.9%, germanium 0.02-0.1%, and nanoboron particles 0.08-0.12 are used. % and 0.02-0.1% of low-melting point lead-free solder with sodium fluoride, the melting point is reduced and the soldering stability and signal transmission performance are improved.

Benefits of technology

It realizes high denitrification efficiency and stability of low-melting point lead-free solder, reduces costs, improves the temperature resistance and signal transmission performance of welding equipment, and is suitable for welding of precision electronic equipment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of solder, and in particular to a low melting point lead-free solder and a preparation method and application thereof. The solder comprises, by mass, 10-30% of bismuth, 0.6-1.8% of nano silver particles, 0.3-0.8% of nano iron oxide particles, 0.02-0.1% of vanadium, 0.02-0.1% of dysprosium, 0.2-0.9% of indium, 0.02-0.1% of germanium, 0.08-0.12% of nano boron particles, 0.02-0.1% of sodium fluoride, and the balance is tin. The particle size of the nano iron oxide particles is 10-50nm. The particle size of the nano silver particles is 10-50nm. Only a small amount of elements such as In, Ag, Dy and fluoride and fluoride need to be added, which can reduce the cost, improve the gloss of the solder alloy, and refine the grains.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solder, and in particular to a low melting point lead-free solder and a preparation method and application thereof. Background Art

[0002] Sn-Pb solder has been used in the electronics industry for quite a long time. Due to its low melting point, high cost-effectiveness and easy availability, it has become the most important low-temperature solder system and is widely used in the welding of non-ferrous metals, food containers, construction, machinery and pipeline installations.

[0003] At present, the lead-free solders that are more recognized by the industry are mainly Sn-Ag-Cu and Sn-Bi, especially the former. Because Sn-Ag-Cu alloy solders are easy to obtain, have fewer technical problems, good compatibility with traditional solders, and high reliability of solder joints. However, it is unrealistic to completely replace tin-lead solders with Sn-Ag-Cu alloy solders. Apart from cost factors, the most important thing is that the melting point of Sn-Ag-Cu solders is higher than that of tin-lead solders, which leads to an increase in welding temperature. It is easy to cause thermal damage to components with poor heat resistance, causing the flat substrate to bend and deform, increasing the possibility of damage. This means that the use of Sn-Ag-Cu lead-free solders poses severe challenges to a series of projects such as welding equipment, welding processes, and the temperature resistance of electronic components and substrate materials.

[0004] For electronic equipment, chip circuit boards and other devices in the high-end communication field, the requirements for solder or solder are relatively high, especially for equipment in the photovoltaic field, especially some precision photovoltaic components, such as the welding of precision photovoltaic panels, or communication equipment and control equipment in photovoltaic components, which may need to work under long-term lighting conditions. Therefore, the solder is required to have a lower melting point and good anti-aging performance. Although many solders have good conductivity and anti-aging properties, good signal transmission performance is still required for communication equipment, control equipment, etc.

[0005] The eutectic melting point of Sn-Bi solder is very low, only 139°C, which is lower than the traditional Sn-37Pb solder alloy (183°C). The low melting point makes it very advantageous in the outer layer of graded packaging and close to the temperature-sensitive inner layer. It also shows excellent properties in the 100°C temperature cycle test after surface assembly, and its application in precision electronic equipment also shows that it has good signal transmission performance. Due to the poor thermal fatigue resistance and ductility of SnBi eutectic solder, its welding reliability is insufficient and the wire processing is difficult, which limits its further promotion and application. Summary of the invention

[0006] Based on this, the present invention proposes a low-melting-point lead-free solder and a preparation method and application thereof, which has high denitrification efficiency and stability, and has good economy and environmental friendliness.

[0007] According to a first aspect of the present invention, a low-melting-point lead-free solder is provided, which comprises, by mass, 10-30% bismuth, 0.6-1.8% nano-silver particles, 0.3-0.8% nano-ferric oxide particles, 0.02-0.1% dysprosium, 0.2-0.9% indium, 0.02-0.1% germanium, 0.08-0.12% nano-boron particles, 0.02-0.1% sodium fluoride, and the balance is tin.

[0008] According to an embodiment of the present invention, the particle size of the nano-iron oxide particles is 10-50 nm.

[0009] According to an embodiment of the present invention, the particle size of the nano-silver particles is 10-50 nm.

[0010] According to an embodiment of the present invention, the alloy further contains 0.0002% to 0.0005% cobalt by weight.

[0011] According to a second aspect of the present invention, there is provided a method for preparing the above-mentioned low melting point lead-free solder, comprising the following steps:

[0012] Weighing bismuth, dysprosium, indium, germanium and tin according to preset mass fractions and putting them into a preparation container, heating and melting them to obtain a molten alloy;

[0013] Dispersing nano silver particles and nano ferric oxide particles into the molten alloy to obtain alloy liquid;

[0014] Adding sodium fluoride and nano-boron particles into a preparation container, and stirring so that the sodium fluoride and the nano-boron particles are dispersed in the alloy liquid; and

[0015] The preparation container is kept at a certain temperature for a predetermined time, and cooled to room temperature in air to obtain the lead-free solder.

[0016] According to an embodiment of the present invention, the step of weighing bismuth, dysprosium, indium, germanium and tin according to preset mass fractions and placing them in a preparation container, heating and melting them to obtain a molten alloy comprises:

[0017] Weigh bismuth, dysprosium, indium, germanium and tin according to preset mass fractions, put them into a blender and mix them evenly, pour them out after ball milling, filter them, and dry them in low-temperature vacuum to obtain a mixed powder;

[0018] Add the dried mixed powder into a preparation container, and heat to 1300° C.-1500° C. under nitrogen protection to melt the mixed powder;

[0019] The alloy is melted uniformly under stirring, turned over after being solidified by water cooling, and heated to 1300° C.-1500° C. under nitrogen protection to melt, thereby obtaining the molten alloy.

[0020] According to an embodiment of the present invention, the nano silver particles and nano ferric oxide particles are dispersed into the molten alloy to obtain an alloy liquid;

[0021] heating the molten alloy to 1500-1600° C. under stirring;

[0022] The nano silver particles and the nano ferric oxide particles are dispersed in the molten alloy to obtain the alloy liquid.

[0023] According to an embodiment of the present invention, the preparation container is kept at a certain temperature for a predetermined time, and cooled to room temperature in air to obtain the lead-free solder;

[0024] The temperature of the alloy liquid is lowered to 200-280° C., kept warm for 15-30 minutes, and the tin slag on the surface is removed;

[0025] The temperature of the alloy liquid is lowered to 170-180° C., kept warm for 15-30 minutes, the tin slag on the surface is removed, and the alloy liquid is cooled to room temperature in air to obtain the lead-free solder.

[0026] According to an embodiment of the present invention, sodium fluoride and nano-boron particles are added into a preparation container, and stirred so that the sodium fluoride and the nano-boron particles are dispersed in the alloy liquid, comprising:

[0027] Lowering the temperature of the alloy liquid to 600-800° C.;

[0028] Under stirring conditions, the sodium fluoride and nano-boron particles are dispersed into the alloy liquid.

[0029] According to a third aspect of the present invention, there is provided a use of the above-mentioned low melting point lead-free solder in precision electronic devices in the photovoltaic field.

[0030] It can be seen from the above technical scheme that the low melting point lead-free solder and its preparation method and application provided by the present invention have the following beneficial effects:

[0031] The present invention discloses a low melting point lead-free solder and a preparation method and application thereof. The low melting point lead-free solder alloy of the present invention only needs to add a small amount of elements such as In, Ag, Dy, and fluoride, and does not need to add a large amount of precious metals such as In, Dy, and other elements, thereby reducing costs, improving the glossiness of the solder alloy, refining the grains, further reducing the temperature and ensuring the shear strength, and by adding the above elements, the ductility of the alloy can be increased, while increasing reliability and facilitating processing, and its application in precision electronic equipment also shows that it has good signal transmission performance.

[0032] The invention plays a role of dispersion strengthening by adding nanometer iron oxide particles, improves the shear resistance of the solder part in the welding joint, and greatly improves the stability of the solder alloy. The invention adds nanometer boron particles, can generate new intermetallic compounds or act as particles themselves, provide non-uniform nucleation sites for the matrix phase, refine the grains and each phase structure, improve the performance of the material, and the addition of nanometer boron can significantly affect the organizational structure of the solder. The boron element of nanometer size is concentrated at the grain boundary of the intermetallic compound (IMC), so that the interface morphology tends to be thin and flat, and refines the IMC grains. In addition, the addition of trace boron can also improve the plasticity of the solder, and when the addition amount is high, the strength and hardness of the material can be improved. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0034] According to a first aspect of the present invention, a low-melting-point lead-free solder is provided, which comprises, by mass, 10-30% bismuth, 0.6-1.8% nano-silver particles, 0.3-0.8% nano-ferric oxide particles, 0.02-0.1% dysprosium, 0.2-0.9% indium, 0.02-0.1% germanium, 0.08-0.12% nano-boron particles, 0.02-0.1% sodium fluoride, and the balance is tin.

[0035] Tin is a very commonly used solder metal, especially as the main component in tin-lead alloys. Tin has good soldering properties and a low melting point. Silver solder is widely used due to its excellent electrical and thermal conductivity. Silver is also often used to increase the strength and corrosion resistance of the solder.

[0036] Bismuth (Bi), tin (Sn), dysprosium (Dy), indium (In), silver (Ag) and germanium (Ge) elements can form eutectic low-melting-point alloys. Dysprosium metal can be used as a magneto-optical storage material with high recording speed and reading sensitivity, improving the magnetic and thermal properties of the alloy. The addition of dysprosium will indirectly affect the melting point by forming a solid solution or affecting the microstructure of the alloy.

[0037] Fluorides are added to alloys as fluxes to form low-melting alloys. These fluorides can form low-melting eutectic mixtures with alloys, thereby lowering the melting point of the alloy, facilitating smelting or welding at lower temperatures, improving the corrosion resistance and wear resistance of the solder, and helping to improve current efficiency. Sodium fluoride can form low-melting alloys with bismuth. The formation principle of these eutectic mixtures is based on the interaction between different components, resulting in a lower melting point for the mixture than the melting point of each component alone. Sodium fluoride plays a role in lowering the melting point and improving performance in these mixtures.

[0038] According to an embodiment of the present invention, the particle size of the nano-iron oxide particles is 10-50 nm.

[0039] According to an embodiment of the present invention, the particle size of the nano-boron particles is 10-50 nm.

[0040] According to the embodiment of the present invention, the particle size of the nano silver particles is 10-50 nm. The nano silver particles with such fine structure can more effectively improve the conductivity of the battery.

[0041] Nano silver and nano ferric oxide particles may exhibit different physical and chemical properties from macroscopic materials due to their unique size effect, including thermal properties. If nano silver is used as a dispersed phase in an alloy, it will affect the melting point of the alloy by affecting the grain size, grain boundary characteristics or phase distribution of the alloy. The present invention adds nano ferric oxide particles to play a role of dispersion strengthening, improves the shear resistance of the solder part in the welded joint, and greatly improves the stability of the solder alloy.

[0042] Nano boron is a nano-sized boron particle. As a particle itself, it can provide non-uniform nucleation sites for the matrix phase, refine the grains and each phase structure, and improve the performance of the material. The addition of nano boron can significantly affect the organizational structure of the solder. The nano-sized boron element is concentrated at the grain boundary of the intermetallic compound (IMC), making the interface morphology tend to be thin and flat, and refining the IMC grains. In addition, the addition of trace boron can also improve the plasticity of the solder, and when the addition amount is high, it can improve the strength and hardness of the material.

[0043] According to an embodiment of the present invention, the alloy further contains 0.0002% to 0.0005% cobalt by weight.

[0044] According to a second aspect of the present invention, there is provided a method for preparing the above-mentioned low melting point lead-free solder, comprising the following steps:

[0045] Weighing bismuth, dysprosium, indium, germanium and tin according to preset mass fractions and putting them into a preparation container, heating and melting them to obtain a molten alloy;

[0046] Dispersing nano silver particles and nano ferric oxide particles into molten alloy to obtain alloy liquid;

[0047] Adding sodium fluoride and nano-boron particles into a preparation container, and stirring to disperse the sodium fluoride and nano-boron particles in the alloy liquid; and

[0048] The preparation container is kept at a certain temperature for a predetermined time, and cooled to room temperature in air to obtain the lead-free solder.

[0049] According to an embodiment of the present invention, bismuth, dysprosium, indium, germanium and tin are weighed according to preset mass fractions and put into a preparation container, and heated and melted to obtain a molten alloy, including:

[0050] Weigh bismuth, dysprosium, indium, germanium and tin according to preset mass fractions, put them into a blender and mix them evenly, pour them out after ball milling, filter them, and dry them in low-temperature vacuum to obtain a mixed powder;

[0051] Add the dried mixed powder into the preparation container and heat to 1300°C-1500°C under nitrogen protection to melt the mixed powder;

[0052] The alloy is melted evenly under stirring, turned over after being cooled and solidified, and heated to 1300°C-1500°C under nitrogen protection to melt to obtain a molten alloy.

[0053] According to an embodiment of the present invention, nano silver particles and nano ferric oxide particles are dispersed into a molten alloy to obtain an alloy liquid;

[0054] The molten alloy is heated to 1500-1600°C under stirring;

[0055] The nano silver particles and nano ferric oxide particles are dispersed in the molten alloy to obtain alloy liquid.

[0056] According to an embodiment of the present invention, the preparation container is kept at a certain temperature for a predetermined time, and cooled to room temperature in air to obtain the lead-free solder;

[0057] Lower the temperature of the alloy liquid to 200-280℃, keep it warm for 15-30 minutes, and remove the tin slag on the surface;

[0058] The temperature of the alloy liquid is lowered to 170-180°C, kept warm for 15-30 minutes, the tin slag on the surface is removed, and the alloy liquid is cooled to room temperature in air to obtain lead-free solder.

[0059] According to an embodiment of the present invention, sodium fluoride and nano-boron particles are added into a preparation container, and stirred so that the sodium fluoride and the nano-boron particles are dispersed in the alloy liquid, comprising:

[0060] Lower the temperature of the alloy liquid to 600-800°C;

[0061] Under stirring conditions, sodium fluoride and nano-boron particles are dispersed into the alloy liquid.

[0062] According to a third aspect of the present invention, there is provided a use of the above-mentioned low melting point lead-free solder in precision electronic devices in the photovoltaic field.

[0063] The technical solution of the present invention is described in detail below through preferred embodiments. It should be noted that the specific embodiments below are only used for illustration and are not used to limit the present invention.

[0064] A method for preparing a low melting point lead-free solder is provided, comprising the following steps:

[0065] Weigh bismuth, dysprosium, indium, germanium and tin according to preset mass fractions, put them into a blender and mix them evenly, pour them out after ball milling, filter them, and dry them in low-temperature vacuum to obtain a mixed powder;

[0066] Add the dried mixed powder into the preparation container and heat to 1300°C-1500°C under nitrogen protection to melt the mixed powder;

[0067] The alloy is melted evenly under stirring, turned over after being solidified by water cooling, and heated to 1300℃-1500℃ to melt under nitrogen protection to obtain a molten alloy;

[0068] The molten alloy is heated to 1500-1600°C under stirring;

[0069] Dispersing nano silver particles and nano ferric oxide particles into molten alloy to obtain alloy liquid;

[0070] Lowering the temperature of the alloy liquid to 600-800° C.;

[0071] Dispersing the sodium fluoride and nano-boron particles into the alloy liquid under stirring; and

[0072] Lower the temperature of the alloy liquid to 200-280℃, keep it warm for 15-30 minutes, and remove the tin slag on the surface;

[0073] The temperature of the alloy liquid is lowered to 170-180°C, kept warm for 15-30 minutes, the tin slag on the surface is removed, and the alloy liquid is cooled to room temperature in air to obtain lead-free solder.

[0074] Experimental Example 1

[0075] A low melting point lead-free solder comprises, by mass percentage, 30% bismuth, 1.8% nano silver particles, 0.8% nano ferric oxide particles, 0.1% dysprosium, 0.9% indium, 0.1% germanium, 0.12% nano boron particles, 0.1% sodium fluoride, and the balance is tin. The particle size of the nano ferric oxide particles is 10nm. The particle size of the nano silver particles is 10nm. The solder provided in this embodiment has a tensile strength of 22.1MPa, a plastic strain ratio of 2.64mm / mm, a shear strength of 34.2MPa, a melting point of 164.26°C, a wetting angle of 26°, and an elongation of 26.3%.

[0076] Experimental Example 2

[0077] A low melting point lead-free solder comprises, by mass percentage, 20% bismuth, 1% nano silver particles, 0.5% nano ferric oxide particles, 0.05% dysprosium, 0.5% indium, 0.05% germanium, 0.1% nano boron particles, 0.05% sodium fluoride, and the balance is tin. The particle size of the nano ferric oxide particles is 20nm. The particle size of the nano silver particles is 20nm. The solder provided in this embodiment has a tensile strength of 21.7MPa, a plastic strain ratio of 2.62mm / mm, a shear strength of 33.6MPa, a melting point of 178.26°C, a wetting angle of 24°, and an elongation of 25.3%.

[0078] Experimental Example 3

[0079] A low melting point lead-free solder comprises, by mass percentage, 10% bismuth, 0.6% nano silver particles, 0.3% nano ferric oxide particles, 0.02% dysprosium, 0.2% indium, 0.02% germanium, 0.08% nano boron particles, 0.02% sodium fluoride, and the balance is tin. The particle size of the nano ferric oxide particles is 50nm. The particle size of the nano silver particles is 50nm. The solder provided in this embodiment has a tensile strength of 21.1MPa, a plastic strain ratio of 2.68mm / mm, a shear strength of 34.2MPa, a melting point of 182.26°C, a wetting angle of 22°, and an elongation of 25.3%.

[0080] Comparative Example 1:

[0081] A solder comprises, by mass fraction, 30% bismuth, 10% silver, 0.02% dysprosium and the balance tin.

[0082] Comparative Example 2:

[0083] Sn-Ag-Cu solder is commercially available.

[0084] Experimental example:

[0085] The effects of LED chip packaging using the solders of Examples 1-3 and Comparative Examples 1-2 are compared, and the results are shown in the table below.

[0086] Brightness of solder joints Welding void rate (%) Thermal conductivity (%) Leakage / short circuit defect rate (%) Example 1 good 6.5 67 0.2 Example 2 good 7.7 61 0.3 Example 3 good 8.2 63 0.2 Comparative Example 1 generally 19.6 52 0.8 Comparative Example 2 good 11.2 62 0.4

[0087] The results show that the use of the solder prepared in Examples 1-3 of the present invention for LED chip packaging can effectively reduce the soldering void rate and leakage / short circuit defect rate, and the solder joints are full, bright, and have high thermal conductivity, which is conducive to heat dissipation.

[0088] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A low melting point lead-free solder, characterized in that: The invention comprises, by mass percentage, 10-30% bismuth, 0.6-1.8% nano silver particles, 0.3-0.8% nano ferric oxide particles, 0.02-0.1% dysprosium, 0.2-0.9% indium, 0.02-0.1% germanium, 0.08-0.12% nano boron particles, 0.02-0.1% sodium fluoride, and the balance is tin.

2. The low melting point lead-free solder according to claim 1, characterized in that: The particle size of the nano-iron oxide particles is 10-50 nm.

3. The low melting point lead-free solder according to claim 1, characterized in that: The particle size of the nano silver particles is 10 to 50 nm.

4. The low melting point lead-free solder according to claim 1, characterized in that: It also contains 0.0002% to 0.0005% cobalt by weight.

5. A method for preparing the low melting point lead-free solder according to any one of claims 1 to 4, characterized in that: The steps include: Weighing bismuth, dysprosium, indium, germanium and tin according to preset mass fractions and putting them into a preparation container, heating and melting them to obtain a molten alloy; Dispersing nano silver particles and nano ferric oxide particles into the molten alloy to obtain alloy liquid; Adding sodium fluoride and nano-boron particles into a preparation container, and stirring so that the sodium fluoride and the nano-boron particles are dispersed in the alloy liquid; as well as The preparation container is kept at a certain temperature for a predetermined time, and cooled to room temperature in air to obtain the lead-free solder.

6. The preparation method according to claim 5, characterized in that: The method comprises weighing bismuth, dysprosium, indium, germanium and tin according to a preset mass fraction, placing them in a preparation container, heating and melting them to obtain a molten alloy, comprising: Weigh bismuth, dysprosium, indium, germanium and tin according to preset mass fractions, put them into a blender and mix them evenly, pour them out after ball milling, filter them, and dry them in low-temperature vacuum to obtain a mixed powder; Add the dried mixed powder into a preparation container, and heat to 1300° C.-1500° C. under nitrogen protection to melt the mixed powder; The alloy is melted uniformly under stirring, turned over after being solidified by water cooling, and heated to 1300° C.-1500° C. under nitrogen protection to melt, thereby obtaining the molten alloy.

7. The preparation method according to claim 5, characterized in that: The step of dispersing nano silver particles and nano ferric oxide particles into the molten alloy to obtain alloy liquid; heating the molten alloy to 1500-1600° C. under stirring; The nano silver particles and the nano ferric oxide particles are dispersed in the molten alloy to obtain the alloy liquid.

8. The preparation method according to claim 5, characterized in that: The preparation container is kept at a certain temperature for a predetermined time, and cooled to room temperature in air to obtain the lead-free solder; The temperature of the alloy liquid is lowered to 200-280° C., kept warm for 15-30 minutes, and the tin slag on the surface is removed; The temperature of the alloy liquid is lowered to 170-180° C., kept warm for 15-30 minutes, the tin slag on the surface is removed, and the alloy liquid is cooled to room temperature in air to obtain the lead-free solder.

9. The preparation method according to claim 5, characterized in that: Adding sodium fluoride and nano-boron particles into a preparation container and stirring so that the sodium fluoride and the nano-boron particles are dispersed in the alloy liquid, comprising: Lowering the temperature of the alloy liquid to 600-800° C.; Under stirring conditions, the sodium fluoride and nano-boron particles are dispersed into the alloy liquid.

10. Use of the low melting point lead-free solder according to any one of claims 1 to 4 in precision electronic devices in the photovoltaic field.