A preparation method of embedded silicon-carbon material
By embedding silicon nanomaterials into a carbon network skeleton and subjecting it to high temperature treatment, embedded SiOx-C nanomaterials are prepared, which solves the problem of volume expansion of silicon materials, improves the specific capacitance and cycle life of lithium-ion batteries, and achieves a more stable Electrochemical properties.
Patent Information
- Application Number
- CN202411009164.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Silicon materials have volume expansion problems when storing lithium ions, which leads to rupture of electrode materials and degradation of battery performance. Existing silicon-carbon composite materials perform poorly in terms of cycle stability and specific capacitance.
By evenly embedding silicon nanomaterials into the carbon network skeleton, surface modification and catalyst treatment are used to form an embedded SiO2-organic wet gel, and SiOx-C nanomaterials are produced through high-temperature carbonization and activation treatments to control the size and pores of silicon nanoparticles. structure to achieve the synergy of silicon and carbon materials.
It improves the specific capacitance and cycle life of silicon-carbon materials, inhibits the volume expansion of silicon particles, enhances the electrochemical performance and stability of the battery, and is suitable for lithium-ion battery anode materials.
Smart Images

Figure CN118545725B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, and in particular to a method for preparing an embedded silicon-carbon material. Background Art
[0002] As a new type of material, silicon-carbon composites have broad application prospects in the fields of batteries, energy storage, electric vehicles, etc. Silicon materials have a high theoretical specific capacity (the number of lithium ions stored per unit mass), which is much higher than traditional carbon materials. This means that using silicon-carbon composites as negative electrode materials can increase the energy density of batteries, enable batteries to store more electrical energy, and extend the use time of equipment or the mileage of electric vehicles. Compared with some other negative electrode materials, silicon resources in silicon-carbon composites are relatively abundant, which helps to reduce dependence on scarce resources. In addition, the use of high-energy-density silicon-carbon negative electrode materials can reduce the overall weight and size of the battery system, thereby reducing the resource consumption of the battery and helping to build a more environmentally friendly battery system. Silicon materials have the problem of volume expansion when storing lithium ions, which can easily cause the rupture of electrode materials and the attenuation of battery performance. By compounding silicon with materials such as carbon, the expansion rate of silicon can be slowed down, the stability and cycle life of the material can be improved, and the performance of the battery can be enhanced. Summary of the invention
[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing an embedded silicon-carbon material. The preparation process of the embedded silicon-carbon material is reasonably designed and can evenly embed silicon nanomaterials into the carbon network skeleton, thereby playing a synergistic role of silicon and carbon materials during the charge and discharge process, and having high specific capacity and stable cycle performance.
[0004] The present invention solves the technical problem by adopting the following technical solutions:
[0005] A method for preparing an embedded silicon-carbon material comprises the following steps:
[0006] S1, dissolving the surface-modified silicon source in an aqueous solution under the catalytic action of a catalyst, and stirring evenly to obtain a silica sol;
[0007] S2, adding the organic raw materials to the silica sol prepared in step S1, uniformly dispersing them in the solution, and allowing the silica sol and the organic sol to co-grow to form an embedded SiO2-organic wet gel;
[0008] S3, sealing, aging, and drying the embedded SiO2-organic gel prepared in step S2 to obtain an embedded SiO2-organic aerogel;
[0009] S4, subjecting the embedded SiO2-organic aerogel prepared in step S3 to a first high temperature treatment to carbonize and generate an embedded SiO2-C aerogel;
[0010] S5, subjecting the embedded SiO2-C aerogel prepared in step S4 to a second high temperature treatment to obtain an embedded SiO x -C nanomaterials.
[0011] Moreover, the silicon source described in step S1 is one of SiO2 aerogel powder, gas-phase SiO2 powder, alkaline or acidic silica sol, and organic silicon, or a mixture of at least two of them.
[0012] Moreover, the catalyst in step S1 is ammonia water, urea, hydrochloric acid or nitric acid solution.
[0013] Moreover, the surface modification treatment is a gas phase or liquid phase modification treatment method such as siloxane, silanization, and silane biomimetic.
[0014] Moreover, the particle size of the silica sol in step S1 is 2nm-500nm, and the stirring time is 5min-20min.
[0015] Moreover, the mass percentage of the silica sol in step S2 is 5%-30%.
[0016] Furthermore, a polymer surfactant is added to the silica sol in step S2, and the polymer surfactant is polyvinyl pyrrolidone or polyethylene imine.
[0017] Moreover, the organic raw material described in step S2 is one or a mixture of at least two of polyurethane, polyimide, phloroglucinol-formaldehyde, resorcinol-formaldehyde, phenol-formaldehyde, melamine-formaldehyde, cellulose, and chitosan. The organic raw material includes at least one of polyurethane, polyimide, phenolic resin, cellulose, chitosan, and starch. All proportions of polyurethane, polyimide, and phenolic resin (preparation of precursors hydroquinone-formaldehyde, melamine-formaldehyde, and phenol-formaldehyde) prepared in the prior art are suitable for the present invention, and the gel formed by polyurethane, polyimide, and phenolic resin in the preparation are suitable for the present invention. Or the organic matter used to prepare carbon aerogel in the prior art is also acceptable. The present invention has no special limitation on organic sol, and only makes a carbon skeleton material. Sols of different proportions or original components of different proportions do not affect the final material combination and structure, because they are all carbonized at high temperature, and therefore do not affect the structure of the final product.
[0018] Moreover, the carbonization temperature of the first high temperature treatment is 600-1050°C, and the temperature of the second high temperature treatment is 1300-1600°C.
[0019] Moreover, the prepared embedded SiO x -C nanomaterials, 0≤x<2.
[0020] The advantages and positive effects of the present invention are:
[0021] 1. The preparation design of the present invention is ingenious, the process is simple, and large-scale production can be achieved. The prepared embedded silicon-carbon material is microscopically regulated in terms of nanoparticle size and pore structure, and silicon nanoparticles can be uniformly embedded in the carbon skeleton. The size of silicon nanoparticles can be regulated by controlling the reaction time of the fresh silicon source under the catalyst; the specific surface area and pore size of the silicon-carbon material can be regulated by controlling the solid content of the organic gel and the amount of the catalyst.
[0022] 2. In the preparation process of the present invention, as the silicon nanoparticles increase, the specific surface area of the silicon-carbon material decreases and the specific capacitance gradually increases; when the proportion of silicon nanoparticles is 20%, the specific surface area of the silicon-carbon material is 1358 m 2 / g, the electrochemical performance is the best; as the proportion of silicon nanoparticles gradually increases to 30%, the specific surface area of silicon-carbon materials decreases to 56 m 2 / g, the specific capacity and cycle life of the silicon-carbon negative electrode decreased.
[0023] 3. The embedded SiO prepared by the present invention x -C nanomaterials, 0≤x<2. During the charge and discharge process, SiOx reacts with lithium ions to form nano-Si, Li2O and lithium silicates. The generated Li2O and lithium silicates mainly inhibit the agglomeration of nano-Si particles and play a role in buffering volume expansion. When x is closer to 1, the electrochemical performance is better.
[0024] 4. In step S2 of the present invention, when the silica sol and the organic sol co-grow to form an embedded SiO2-organic wet gel, the silica sol accounts for 5%-30%, which is more conducive to the carbonization reduction reaction in step S5 to form SiO x , making SiO x The x is as close to 1 as possible, thus having a high specific capacity and stable cycle performance.
[0025] 5. The present invention uses a polymer surfactant, polyvinyl pyrrolidone or polyethyleneimine, in the process of forming an embedded SiO2-organic wet gel to evenly disperse the gel particles, ensuring that the silicon particles are evenly embedded in the carbon particles without agglomeration. The silicon content of the prepared silicon-carbon material reaches 60%, and the silicon nanoparticles are evenly dispersed. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a TEM image of the embedded silicon-carbon material prepared in accordance with the present invention.
[0027] Figure 2 This is the EDX element ratio diagram of the embedded silicon-carbon material prepared in accordance with the present invention.
[0028] Figure 3 This is a N2 adsorption-desorption curve diagram of the embedded silicon-carbon material prepared in accordance with the present invention.
[0029] Figure 4 This is a pore size distribution diagram of the embedded silicon-carbon material prepared in accordance with the present invention.
[0030] Figure 5 This is the first capacitance performance diagram of the embedded silicon-carbon material prepared in the present invention as a negative electrode material for lithium-ion batteries.
[0031] Figure 6 This is a graph showing the cycle life and coulombic efficiency of the embedded silicon-carbon material prepared in accordance with the present invention as a negative electrode material for lithium-ion batteries. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto. Example 1
[0033] A method for preparing an embedded silicon-carbon material, wherein a silicon source is surface-modified and dissolved in an aqueous solution to form a silica sol which can be evenly dispersed in an organic sol, and the size of silicon nanoparticles can be effectively controlled. The co-growth of the silica sol and the organic sol can embed the silicon nanoparticles into the organic gel. The embedded SiO x -C nanomaterials have high energy density, excellent cycle stability and safety in lithium-ion batteries.
[0034] A method for preparing an embedded silicon-carbon material comprises the following steps:
[0035] S1. 12 g of SiO2 aerogel powder was modified with 10 ml of γ-propyltrimethoxysilane, dissolved in 100 ml of aqueous solution, 3 ml of 0.08 mol / L ammonia solution was added, and stirred evenly for 30 min to form silica sol;
[0036] S2, adding 20g of phloroglucinol and 36ml of formaldehyde to SiO2 sol, wherein the molar ratio of phloroglucinol to sodium bicarbonate is 300:1, stirring for 30min, and allowing to stand to form SiO2-phloroglucinol-formaldehyde gel;
[0037] S3, the SiO2-phloroglucinol-formaldehyde gel obtained in step S2 is sealed, aged at 90°C for 3 days and subjected to supercritical carbon dioxide drying to obtain an embedded SiO2-phloroglucinol-formaldehyde aerogel;
[0038] S4, carbonizing the SiO2-phloroglucinol-formaldehyde aerogel at 800°C for 3 hours in a nitrogen atmosphere to obtain a SiO2-C aerogel;
[0039] S5. Activate the SiO2-C aerogel at 1600° C. for 3 hours in an argon atmosphere to obtain SiOx-C aerogel.
[0040] The embedded SiOx-C aerogel prepared in Example 1 of the present invention has an x value of 1.3, a silicon content of 13%, and a specific surface area of 237 m 2 / g, with an average pore size of 5.3 nm. The embedded silicon-carbon material prepared by this method is used in lithium-ion batteries, and its specific capacity can reach 838 mAh / g. In the test of this material as a lithium-ion half-cell, the specific capacity gradually increased in the first 235 cycles, reaching 473 mAh / g, and then gradually decreased. After 400 cycles, the specific capacity was still 252 mAh / g. Example 2
[0041] A method for preparing an embedded silicon-carbon material comprises the following steps:
[0042] S1. Add 10 ml of acidic silica sol to 3 ml of methyltrimethoxysilane for modification, dissolve in 100 ml of aqueous solution, add 3 ml of 0.05 mol / L ammonia solution, and stir evenly for 30 min to form silica sol;
[0043] S2, add 10g phloroglucinol, 3g chitosan and 38ml formaldehyde to SiO2 sol, add 0.3ml polyvinyl pyrrolidone (0.5wt%), wherein the molar ratio of phloroglucinol to sodium bicarbonate is 200:1, stir for 30min, and let it stand to form SiO2-phloroglucinol-chitosan-formaldehyde gel;
[0044] S3, sealing the SiO2-phloroglucinol-chitosan-formaldehyde gel obtained in step 2, aging at 85°C for 4 days and supercritical drying with carbon dioxide to obtain an embedded SiO2-phloroglucinol-chitosan-formaldehyde aerogel;
[0045] S4, carbonizing the SiO2-phloroglucinol-chitosan-formaldehyde aerogel at 900°C for 3 hours in a nitrogen atmosphere to obtain SiO2-C aerogel;
[0046] S5. Activate the SiO2-C aerogel at 1500° C. for 3 hours in an argon atmosphere to obtain SiOx-C aerogel.
[0047] The embedded SiOx-C aerogel prepared in Example 2 of the present invention has an x value of 0.9, a silicon content of 19%, and a specific surface area of 446 m 2 / g, with an average pore size of 1.8 nm. The embedded silicon-carbon material prepared by this method is used in lithium-ion batteries, and its specific capacity can reach 3357 mAh / g. In the test of this material as a lithium-ion half-cell, the specific capacity gradually increased in the first 285 cycles, reaching 811 mAh / g, and then gradually decreased. After 400 cycles, the specific capacity was still 592 mAh / g.
[0048] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.
Claims
1. A method for preparing an embedded silicon-carbon material, characterized in that: The steps include: S1, dissolving the surface-modified silicon source in an aqueous solution under the catalytic action of a catalyst, stirring evenly, to obtain a silica sol, wherein the particle size of the silica sol is 2nm-500nm, the stirring time is 5min-20min, and the surface modification treatment is a gas phase or liquid phase modification treatment method of siloxane or silanization; S2, adding organic raw materials to the silica sol prepared in step S1, uniformly dispersing the organic raw materials in the solution, and co-grow the silica sol and the organic sol to form an embedded SiO2-organic wet gel, wherein the mass percentage of the silica sol to the embedded SiO2-organic wet gel is 5%-30%, and a polymer surfactant is also added to the silica sol, and the polymer surfactant is polyvinyl pyrrolidone or polyethyleneimine; S3, sealing, aging, and drying the embedded SiO2-organic wet gel prepared in step S2 to obtain an embedded SiO2-organic aerogel; S4, subjecting the embedded SiO2-organic aerogel prepared in step S3 to a first high temperature treatment, wherein the carbonization temperature of the first high temperature treatment is 600-1050° C., and carbonization generates an embedded SiO2-C aerogel; S5, subjecting the embedded SiO2-C aerogel prepared in step S4 to a second high temperature treatment, wherein the temperature of the second high temperature treatment is 1300-1600°C, to obtain an embedded SiO x -C nanomaterials; The embedded SiO x -C nanomaterials, 0≤x<2.
2. The method for preparing an embedded silicon-carbon material according to claim 1, characterized in that: The silicon source described in step S1 is one of SiO2 aerogel powder, gas phase SiO2 powder, alkaline or acidic silica sol, and organic silicon, or a mixture of at least two of them.
3. The method for preparing an embedded silicon-carbon material according to claim 1, characterized in that: The catalyst in step S1 is aqueous ammonia, urea, hydrochloric acid or nitric acid solution.
4. The method for preparing an embedded silicon-carbon material according to claim 1, characterized in that: The organic raw material described in step S2 is one or a mixture of at least two of polyurethane, polyimide, phloroglucinol-formaldehyde, resorcinol-formaldehyde, phenol-formaldehyde, melamine-formaldehyde, cellulose, and chitosan.
Citation Information
Patent Citations
Silicon-oxygen-carbon negative electrode material taking cellulose / silicon dioxide aerogel as precursor and preparation method thereof
CN113410450A