A low-viscosity, easy-pump, fluorine-free, alkali-free liquid quick-setting agent and preparation method thereof
By using silicone hybrid oligomers in fluorine-free and alkali-free liquid accelerators to destroy the amorphous [Al(OH)3]m micelle structure and promote cement hydration, the problems of viscosity and stability of the accelerator are solved. It achieves low-viscosity and high-strength concrete effects and meets the low-carbon and environmentally friendly requirements of industrial production.
Patent Information
- Application Number
- CN202411019035.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-29
AI Technical Summary
After increasing the Al3+ content, existing fluorine-free and alkali-free liquid accelerators are easily hydrolyzed and polymerized to form amorphous [Al(OH)3] micelles, resulting in increased system viscosity and precipitation, which cannot effectively solve the viscosity and stability of the accelerator. sexual problems, and the preparation process consumes high energy, affecting industrial production and carbon emission reduction goals.
Silicone hybrid oligomers are prepared from acrylamide, dimethyldiallylammonium chloride, methylallyl polyoxyethylene ether, ethyl orthosilicate, ascorbic acid, hydrogen peroxide and mercaptopropionic acid, with the addition of sulfuric acid The solubility of aluminum destroys the three-dimensional network structure of amorphous [Al(OH)3]m micelles, prevents the precipitation of Al(OH)3, promotes hydration of cement particles through the Si-O structure, and improves the early strength and later strength retention of concrete. Rate.
It has realized a low-viscosity fluorine-free and alkali-free liquid accelerating setting agent that meets the standards of GB/T 35159-2017 and Q/CR807-2020, reduces the system viscosity, improves the early strength and later strength retention rate of concrete, and simplifies the production process. , reduces energy consumption and meets the low-carbon environmental protection requirements of industrial production.
Smart Images

Figure CN118545936B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building admixtures and relates to a low-viscosity and easy-pump type fluorine-free and alkali-free liquid quick-setting agent and a preparation method thereof. Background Art
[0002] Accelerator is a chemical admixture that makes concrete set quickly. It is widely used in projects such as building structure reinforcement, tunnel support and bridge repair. The application of modern engineering also puts forward a lot of requirements for accelerators: (1) In order to reduce dust pollution during construction, the use of powdered accelerators should be reduced, and liquid accelerators are recommended; (2) In order to improve the durability of the structure, the alkali content in the accelerator should be reduced, and alkali-free accelerators are recommended; (3) In order to reduce the harm of accelerators to the human body during construction, the addition of fluorine raw materials in the accelerator should be reduced, and fluorine-free and alkali-free liquid accelerators should be developed; (4) In order to improve the quality of the project, fluorine-free and alkali-free liquid accelerators that can improve the hourly strength should be developed.
[0003] Based on the above requirements, in order to make the accelerator meet the construction requirements under the conditions of no fluorine and no alkali, it is necessary to increase the Al content in the liquid accelerator. 3+ However, with the Al 3+ With the increase of content, it is very easy to hydrolyze and polymerize to form amorphous [Al(OH)3] m Micelles will fix a large amount of bound water, causing the system viscosity to increase. As time goes by, the micelles are very likely to aggregate to form Al(OH)3 precipitation, causing the accelerator to precipitate and stratify, making it unusable.
[0004] CN113603384A discloses an ultra-early-strength fluorine-free and alkali-free liquid accelerator and a preparation method thereof. The raw materials and mass percentages of the accelerator are: 60% to 65% aluminum sulfate, 7% to 10% organic solvent promoter, 1% to 2% stabilizer, 1% to 2% early strength agent, 0.5% to 1% pH regulator, and the balance is water. The production process is as follows: (1) weigh each component by weight percentage and set aside; (2) add water into the reaction container, add stabilizer under stirring at room temperature, and stir for 30 minutes to 60 minutes; (3) add half of the aluminum sulfate, stir for 30 minutes to 35 minutes, add organic solvent, stir for 30 minutes to 60 minutes, add the other half of the aluminum sulfate, and continue stirring for 2 hours to 4 hours; (4) then add early strength agent under stirring, and stir at room temperature for 20 minutes to 30 minutes; (5) finally add pH adjuster, and stir for 20 minutes to 30 minutes. The obtained product is an ultra-early strength type fluorine-free and alkali-free liquid accelerator.
[0005] CN114276042A discloses an alkali-free and fluorine-free liquid accelerating setting agent, the raw materials and mass percentages of which are: 50-60% polyaluminium sulfate, 4-8% diethanolamine, 1-5% magnesium sulfate, 1-4% ethylene glycol, 2-5% modified silicon dioxide, and the balance is made up to 100% with water. The production process comprises the following steps: (1) preparing polyaluminium sulfate, diethanolamine, magnesium sulfate, ethylene glycol, modified silica, defoamer and dispersant in proportion, heating water to 40-65°C, first adding 1 / 3-2 / 3 of polyaluminium sulfate, and continuously stirring at a speed of 100-200 r / min for 3-8 minutes, and then continuously adding the remaining polyaluminium sulfate and stirring to dissolve; (2) keeping warm, while stirring, adding dropwise diethanolamine for complexation reaction for 8-15 minutes; (3) keeping warm, while stirring, adding dropwise ethylene glycol for complexation reaction for 8-15 minutes; (4) keeping warm, while stirring, adding the remaining compound components; after stirring for 8-15 minutes, stopping stirring, letting the solution stand, and allowing the solution to cool naturally to room temperature to obtain the accelerating setting agent.
[0006] CN109265064A discloses a method for preparing a high-strength alkali-free and chlorine-free quick-setting agent. The raw materials and mass percentages of the quick-setting agent are: 40-60% aluminum sulfate, 2-12% alcohol amine, 6-12% mixed solution A, and the balance is water. The preparation method is as follows: (1) 2-acrylamide-2-methylpropanesulfonic acid, acrylic acid, modified nano-silica solution initiator and water are uniformly dispersed by ultrasonication, heated to 60-80°C and reacted for 5-8h to obtain mixed solution A; (2) aluminum sulfate, alcohol amine, water and mixed solution A are heated to 60-80°C and reacted for 1-5h to obtain mixed solution B; cooled to room temperature, and then dispersed at high speed for 10 minutes using an emulsifier to obtain a high-strength alkali-free and chlorine-free quick-setting agent.
[0007] The idea of the above technologies is to improve the Al 3+ The solubility of aluminum sulfate is improved, which avoids the problem of high viscosity and poor stability when the aluminum sulfate content is too high, and does not change from amorphous [Al(OH)3] m The viscosity and stability problems of the accelerator are solved from the perspective of flocculants, and its preparation process is energy-intensive (such as heating), which is not conducive to industrial production and carbon emission reduction goals. Summary of the invention
[0008] In view of the above problems, the present invention provides a low-viscosity, easy-pump, fluorine-free and alkali-free liquid accelerator and a preparation method thereof. The accelerator is made of aluminum sulfate, diethanolamine, hydrated magnesium silicate and organosilicon hybrid oligomers, and the organosilicon hybrid oligomers are prepared from acrylamide, dimethyldiallylammonium chloride, methylallyl polyoxyethylene ether, ethyl orthosilicate, ascorbic acid, hydrogen peroxide and mercaptopropionic acid. The present invention prepares organosilicon hybrid oligomers, which, on the one hand, have more hydration groups in the aqueous solution, which can improve the solubility of aluminum sulfate in the solution, and on the other hand, can destroy the amorphous [Al(OH)3] m The three-dimensional network structure between micelles prevents the aggregation of micelles, thereby preventing the formation of Al(OH)3 precipitation, and at the same time releasing amorphous [Al(OH)3] m The free water between the micelles reduces the viscosity of the system. In addition, the organosilicon hybrid oligomer can effectively promote the hydration of cement particles and improve the early strength and late strength retention rate of concrete. The accelerator prepared by the present invention not only meets the two accelerator standards of GB / T 35159-2017 and Q / CR807-2020, but also has a viscosity of ≤300 mPa•s at 0-30°C.
[0009] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: a low-viscosity, easy-pump, fluorine-free and alkali-free liquid quick-setting agent, characterized in that it is made of the following raw materials in parts by weight: 60 to 64 parts of aluminum sulfate, 2 to 4 parts of diethanolamine, 0.3 to 1 part of hydrated magnesium silicate, 1 to 3 parts of organosilicon hybrid oligomers, and water is supplemented to 100 parts.
[0010] The organosilicon hybrid oligomer is made of the following raw materials in parts by weight: 0.7-0.9 parts of acrylamide, 1.95-2.6 parts of dimethyldiallylammonium chloride (a 65% aqueous solution is used in the embodiment, which is 3-4 parts based on the 65% aqueous solution), 14-16 parts of methyl allyl polyoxyethylene ether, 2-4 parts of ethyl orthosilicate, 0.1-0.2 parts of ascorbic acid, 0.016-0.04 parts of hydrogen peroxide (a 8% aqueous solution is used in the embodiment, which is 0.2-0.5 parts based on the 8% aqueous solution), 0.05-0.1 parts of mercaptopropionic acid, and water is added to make up to 100 parts.
[0011] The above-mentioned organosilicon hybrid oligomer is prepared by the following method: (1) mixing acrylamide with water to obtain an acrylamide aqueous solution, which is referred to as S1 solution; (2) mixing ascorbic acid and mercaptopropionic acid with water to obtain a mixed aqueous solution of ascorbic acid and mercaptopropionic acid, which is referred to as S2 solution; (3) adding water, dimethyldiallyl ammonium chloride aqueous solution, methyl allyl polyoxyethylene ether and hydrogen peroxide aqueous solution into a reaction kettle in sequence at room temperature and stirring evenly, and then simultaneously dropping S1 and S2 solutions into the reaction kettle, and continuing to stir for 0.5 to 2.0 hours after the dropping is completed; (4) adding tetraethyl orthosilicate into the reaction kettle and stirring for reaction to obtain an organosilicon hybrid oligomer.
[0012] The schematic diagram of the reaction of the organosilicon hybrid oligomer is as follows: Figure 1 As shown in the figure, the principle is: acrylamide, dimethyl diallyl ammonium chloride and methyl allyl polyoxyethylene ether undergo free radical polymerization under the redox initiation of hydrogen peroxide and ascorbic acid, and the degree of polymerization is controlled by mercaptopropionic acid to obtain a slightly cross-linked positively charged oligomer. After adding tetraethyl orthosilicate, tetraethyl orthosilicate is first hydrolyzed to produce silanol, and then dehydrated and self-polymerized; at the same time, the silanol and the hydroxyl groups in the methyl allyl polyoxyethylene ether molecules will also dehydrate and condense to form a CO-Si structure and connect together, thus forming a mesh structure with silicon atoms as cross-linking points, with positively charged polymer side chains extending all around, and cross-linking between the side chains.
[0013] The preparation process of the accelerator is as follows: water, hydrated magnesium silicate and organosilicon hybrid oligomer are sequentially added into a reaction kettle at room temperature, aluminum sulfate is added twice after stirring evenly, and then diethanolamine is added and stirred to obtain the low-viscosity, easy-pump, fluorine-free and alkali-free liquid accelerator of the present invention.
[0014] The quick-setting agent prepared by the invention not only meets the two quick-setting agent standards of GB / T 35159-2017 and Q / CR807-2020, but also has a viscosity of ≤300 mPa·s at 0-30° C. and a low dosage.
[0015] The beneficial effects of the present invention are:
[0016] 1. In the accelerator system, amorphous [Al(OH)3] m The micelles are positively charged, and the organosilicon hybrid oligomers are also positively charged. Like charges repel each other, and the organosilicon hybrid oligomers destroy the amorphous [Al(OH)3] m The three-dimensional network structure between micelles prevents the amorphous [Al(OH)3] m The aggregation of micelles prevents the formation of Al(OH)3 precipitation. At the same time, amorphous [Al(OH)3] m The free water between micelles reduces the viscosity of the system. And the organosilicon hybrid oligomers, amorphous [Al(OH)3] mA new three-dimensional network structure is formed between the micelles and the hydrated magnesium silicate micelles, which ensures the static stability of the liquid accelerating setting agent.
[0017] 2. Since the organosilicon hybrid oligomer has more hydration groups in the aqueous solution, the solubility of aluminum sulfate in the solution can be improved. High-concentration aluminum sulfate can be quickly dissolved at room temperature, shortening the dissolution time of aluminum sulfate without high-speed stirring.
[0018] 3. The production process of the liquid quick-setting agent of the present invention is simple, and any manufacturer producing concrete water reducing agent can produce it without equipment modification, thus reducing production costs. The production process does not require heating, which greatly reduces energy consumption and is low-carbon and environmentally friendly.
[0019] 4. For the shotcrete using the liquid accelerating agent of the present invention, on the one hand, the Si-O structure in the organosilicon hybrid oligomer can effectively promote the hydration of cement particles and improve the early strength of concrete; on the other hand, the organosilicon hybrid oligomer can also fill the pores in the later stage of concrete and improve the durability of the shotcrete. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of the reaction of organosilicon hybrid oligomers. DETAILED DESCRIPTION
[0021] The present invention is further described in detail below with reference to specific embodiments.
[0022] Embodiment 1:
[0023] (1) Preparation of organosilicon hybrid oligomer: 7 kg of acrylamide was mixed with 17.5 kg of water to prepare S1 solution; 2 kg of ascorbic acid, 0.5 kg of mercaptopropionic acid and 8.3 kg of water were mixed to prepare S2 solution; 769.7 kg of water, 30 kg of dimethyldiallyl ammonium chloride aqueous solution (solid content 65%), 140 kg of methyl allyl polyoxyethylene ether and 5 kg of hydrogen peroxide aqueous solution (solid content 8%) were added into a reactor in sequence at room temperature and stirred evenly, and then S1 and S2 solutions were added dropwise into the reactor at the same time, and the adding time was controlled to be 1 hour. After the addition was completed, stirring was continued for 1 hour; 20 kg of tetraethyl orthosilicate was added into the reactor and stirring was continued for 3 hours to prepare organosilicon hybrid oligomer.
[0024] (2) Preparation of liquid accelerating setting agent: 324 kg of water, 6 kg of hydrated magnesium silicate and 10 kg of organosilicon hybrid oligomer were added to a reaction kettle at room temperature in sequence, and after being stirred evenly, 413.3 kg of aluminum sulfate was added. After half an hour, the remaining 206.7 kg of aluminum sulfate was added. After stirring for 1 hour, 40 kg of diethanolamine was added. After continuing to stir for 1 hour, 1 ton of the low-viscosity, easy-pump, fluorine-free and alkali-free liquid accelerating setting agent of the present invention was obtained.
[0025] Embodiment 2:
[0026] (1) Preparation of organosilicon hybrid oligomer: 8 kg of acrylamide was mixed with 20 kg of water to prepare S1 solution; 1.5 kg of ascorbic acid, 0.7 kg of mercaptopropionic acid and 7.3 kg of water were mixed to prepare S2 solution; 744.5 kg of water, 35 kg of dimethyldiallyl ammonium chloride aqueous solution (solid content 65%), 150 kg of methyl allyl polyoxyethylene ether and 3 kg of hydrogen peroxide aqueous solution (solid content 8%) were added into a reactor in sequence at room temperature and stirred evenly, and then S1 and S2 solutions were added dropwise into the reactor at the same time, and the adding time was controlled to be 1 hour. After the addition was completed, stirring was continued for 1 hour; 30 kg of tetraethyl orthosilicate was added into the reactor and stirring was continued for 3 hours to prepare organosilicon hybrid oligomer.
[0027] (2) Preparation of liquid accelerating setting agent: 307 kg of water, 3 kg of hydrated magnesium silicate and 20 kg of organosilicon hybrid oligomer were added to a reaction kettle at room temperature in sequence, and after being stirred evenly, 426.7 kg of aluminum sulfate was added. After half an hour, the remaining 213.3 kg of aluminum sulfate was added. After stirring for 1 hour, 30 kg of diethanolamine was added. After continuing to stir for 1 hour, 1 ton of the low-viscosity, easy-pump, fluorine-free and alkali-free liquid accelerating setting agent of the present invention was obtained.
[0028] Embodiment 3:
[0029] (1) Preparation of organosilicon hybrid oligomer: 9 kg of acrylamide was mixed with 22.5 kg of water to prepare S1 solution; 1 kg of ascorbic acid, 1 kg of mercaptopropionic acid and 6.7 kg of water were mixed to prepare S2 solution; 717.8 kg of water, 40 kg of dimethyldiallyl ammonium chloride aqueous solution (solid content 65%), 160 kg of methyl allyl polyoxyethylene ether and 2 kg of hydrogen peroxide aqueous solution (solid content 8%) were added into a reactor in sequence at room temperature and stirred evenly, and then S1 and S2 solutions were added dropwise into the reactor at the same time, and the addition time was controlled to 1 hour. After the addition was completed, stirring was continued for 1 hour; 40 kg of tetraethyl orthosilicate was added into the reactor and stirring was continued for 3 hours to prepare organosilicon hybrid oligomer.
[0030] (2) Preparation of liquid accelerating setting agent: 340 kg of water, 10 kg of hydrated magnesium silicate and 30 kg of organosilicon hybrid oligomer were added to a reaction kettle at room temperature in sequence, and after being stirred evenly, 400 kg of aluminum sulfate was added. After half an hour, the remaining 200 kg of aluminum sulfate was added. After stirring for 1 hour, 20 kg of diethanolamine was added. After continuing to stir for 1 hour, 1 ton of the low-viscosity, easy-pump, fluorine-free and alkali-free liquid accelerating setting agent of the present invention was obtained.
[0031] Embodiment 4:
[0032] The method is basically the same as Example 3, except that when preparing the organosilicon hybrid oligomer, 30 kg of ethyl orthosilicate is added and the difference is made up with water.
[0033] Embodiment 5:
[0034] The method is basically the same as Example 1, except that when preparing the liquid accelerating agent, 20 kg of organosilicon hybrid oligomer is added and the difference is offset by water.
[0035] Comparative Example 1: Only slightly cross-linked oligomers were prepared, and an equal amount of ethyl orthosilicate was added when preparing the accelerator.
[0036] (1) Preparation of micro-crosslinked oligomers: 9 kg of acrylamide was mixed with 22.5 kg of water to prepare S1 solution; 1 kg of ascorbic acid, 1 kg of mercaptopropionic acid and 6.7 kg of water were mixed to prepare S2 solution; 757.8 kg of water, 40 kg of dimethyldiallyl ammonium chloride aqueous solution (solid content 65%), 160 kg of methyl allyl polyoxyethylene ether and 2 kg of hydrogen peroxide aqueous solution (solid content 8%) were added into a reactor in sequence at room temperature and stirred evenly, and then S1 and S2 solutions were added dropwise into the reactor at the same time, and the dropping time was controlled to 1 hour. After the dropping was completed, stirring was continued for 1 hour to obtain micro-crosslinked oligomers.
[0037] (2) Preparation of liquid accelerating setting agent: 380 kg of water, 10 kg of hydrated magnesium silicate, 28.8 kg of slightly cross-linked oligomer and 1.2 kg of ethyl orthosilicate were added to a reaction kettle at room temperature in sequence, and after being stirred evenly, 373.3 kg of aluminum sulfate was added. After 1 hour, the remaining 186.7 kg of aluminum sulfate was added. After stirring for 1 hour, 20 kg of diethanolamine was added. After continuing to stir for 2 hours, 1 ton of liquid accelerating setting agent of Comparative Example 1 was obtained.
[0038] Comparative Example 2:
[0039] The method is basically the same as that of Comparative Example 1, except that only slightly cross-linked oligomers are prepared. The difference is that when preparing the accelerating setting agent, 0.35 kg of nano-silicon dioxide is used instead of 1.2 kg of ethyl orthosilicate (the silicon content of both is the same), and the difference is supplemented with water. After adding diethanolamine, stirring is continued for 6 hours to obtain 1 ton of liquid accelerating setting agent of Comparative Example 2.
[0040] Comparative Example 3:
[0041] It is basically the same as Comparative Example 2, except that when preparing the liquid accelerating agent, 2.0 kg of nano-silicon dioxide is added, and the difference is offset by water.
[0042] The following is an explanation of the product effect based on the test part of this experiment.
[0043] Test Group 1: Stability and Viscosity Testing
[0044] The accelerators prepared using Examples 1 to 5 of the present invention and the accelerators prepared using Comparative Examples 1 to 2 were tested for stability in accordance with GB / T35159-2017 "Accelerators for Sprayed Concrete" and QCR 807-2020 "Liquid Alkali-Free Accelerators for Tunnel Sprayed Concrete". The viscosity of the accelerator is obtained by rheometer testing. The test conditions of 0°C, 10°C and 30°C are to place the sample in a constant temperature box and let it stand for different periods of time. Storage stability refers to the volume of the supernatant after being placed for a period of time. The fluorine-free and alkali-free liquid accelerator of the present invention does not produce sediment. The stability and viscosity of the accelerator of the embodiment are shown in Table 1, and the stability and viscosity of the accelerator of the comparative example are shown in Table 2.
[0045]
[0046]
[0047] It can be seen from the data in Table 1 that the accelerators prepared in the examples all meet the requirement that the supernatant volume is less than 5 mL in the GB / T 35159-2017 and Q / CR807-2020 standards. When the temperature is between 0 and 30°C, within 180 days, the viscosity of the accelerator is in the range of 250 to 298 mPa·s, which is relatively close to the viscosity of the fluorine-containing accelerator and meets the construction requirements of shotcrete. Compared with the data at 20°C, Example 2 with a higher aluminum sulfate content shows a higher viscosity. Compared with Example 3, as the actual content of tetraethyl orthosilicate decreases, the viscosity of the accelerator of Example 4 increases slightly. Compared with Example 1, as the actual content of organosilicon hybrid oligomer increases, the viscosity of the accelerator of Example 5 decreases. This shows that organosilicon hybrid oligomers can effectively prevent the amorphous [Al(OH)3] m The aggregation of micelles can reduce the viscosity of the system while maintaining the stability of the system. As the temperature increases, the Brownian motion of micelles increases, [Al(OH)3] m The repulsive force between micelles and organosilicon hybrid oligomers increases, which results in a decrease in the water separation volume and viscosity of the alkali-free accelerator.
[0048] It can be seen from the data in Table 2 that the addition of ethyl orthosilicate in Comparative Example 1 failed to form an organosilicon hybrid oligomer with the micro-crosslinked oligomer. The hydration volume of the micro-crosslinked oligomer is much smaller than that of the organosilicon hybrid oligomer, and it is unable to prevent the amorphous [Al(OH)3] mThe aggregation of micelles leads to poor stability. Nano-silicon dioxide has high surface activity, and the particles themselves are easy to aggregate. In the absence of ultrasound or high-speed shear, in order to stabilize the aluminum sulfate accelerator, it is necessary to increase the content of nano-silicon dioxide, such as Comparative Examples 2 and 3. Although the stability of Comparative Example 3 is improved, its viscosity is greatly increased (compared with Example 1) because the network structure formed by the aggregated nano-silicon dioxide in the system is relatively stable. Although it can stabilize the aluminum sulfate micelles, the viscosity increases and cannot meet the construction requirements. This shows that the organosilicon hybrid oligomer can not only stabilize the aluminum sulfate micelles, but also maintain the viscosity of the system at a low level.
[0049] Test Group 2: Accelerator Performance Test
[0050] According to the detection methods specified in GB / T 35159-2017 "Accelerator for Shotcrete" and Q / CR 807-2020 "Liquid Alkali-free Accelerator for Tunnel Shotcrete", the accelerators prepared in Examples 1 to 5 and Comparative Examples 1 to 3 were tested for setting time, compressive strength and other indicators. The test cement is the benchmark cement P·I42.5. The 10℃ test is as follows: the samples, materials and instruments are all measured in a walk-in constant temperature and humidity test chamber. The accelerator dosage is 7% of the cement dosage at 20℃, and the accelerator dosage is 9% of the cement dosage at 10℃. The test results are shown in Tables 3 and 4.
[0051]
[0052] It can be seen from the data in Table 3 that the alkali-free quick-setting agent prepared in the embodiment meets the requirements of GB / T 35159-2017 "Accelerator for Shotcrete" (initial setting time ≤5min, final setting time ≤12min, 1d compressive strength ≥7.0MPa, 28d compressive strength ratio ≥90%, 90d compressive strength retention rate ≥100%) and Q / CR 807-2020 "Liquid alkali-free quick-setting agent for tunnel shotcrete" (initial setting time ≤5min, final setting time ≤12min, 6h compressive strength ≥1.0MPa, 1d compressive strength ≥10.0MPa, 28d compressive strength ratio ≥90%, 90d compressive strength retention rate ≥105%). The comparative example has a higher aluminum sulfate content, and the setting time can also meet the standard. The embodiment has a greater advantage in early compressive strength, and the 6h compressive strength can reach more than 1.6Mpa, and the 1d strength can reach more than 15.6Mpa. The late strength retention is also good, the 28d compressive strength ratio can reach more than 103%, and the 90d compressive strength retention rate can reach more than 105%. This is due to the Si-O structure in the organosilicon hybrid oligomer, which can effectively promote the hydration of cement particles and improve the early strength of concrete. Although the nano silicon dioxide in the comparative example also has a Si-O structure, due to its own polymerization, the Si-O content that can effectively participate in cement hydration is greatly reduced, which also leads to the early strength of the comparative example, and the late strength retention is not as good as the embodiment.
[0053]
[0054] It can be seen from the data in Table 4 that the accelerators prepared in the examples all meet the standard requirements at 10°C. When the temperature decreases, cement hydration weakens, and increasing the dosage of the accelerator can make the accelerator meet the construction requirements. The effective Si-O content in the comparative example is small, and cement hydration cannot be promoted. After increasing the dosage, the setting time and compressive strength cannot meet the requirements.
[0055] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A low-viscosity, easy-pump, fluorine-free, alkali-free liquid quick-setting agent, characterized in that: The invention is prepared from the following raw materials in parts by weight: 60-64 parts of aluminum sulfate, 2-4 parts of diethanolamine, 0.3-1 parts of hydrated magnesium silicate, 1-3 parts of organic silicon hybrid oligomer, and water to make up to 100 parts; The organosilicon hybrid oligomer is prepared from the following raw materials in parts by weight: 0.7-0.9 parts of acrylamide, 1.95-2.6 parts of dimethyldiallyl ammonium chloride, 14-16 parts of methylallyl polyoxyethylene ether, 2-4 parts of tetraethyl orthosilicate, 0.1-0.2 parts of ascorbic acid, 0.016-0.04 parts of hydrogen peroxide, 0.05-0.1 parts of mercaptopropionic acid, and water is added to make up to 100 parts.
2. A low-viscosity, easy-pump, fluorine-free and alkali-free liquid quick-setting agent as claimed in claim 1, characterized in that: The preparation method of the organosilicon hybrid oligomer is: (1) Mixing acrylamide and water to obtain an acrylamide aqueous solution, denoted as S1 solution; (2) mixing ascorbic acid, mercaptopropionic acid and water to obtain a mixed aqueous solution of ascorbic acid and mercaptopropionic acid, denoted as S2 solution; (3) Add water, dimethyldiallyl ammonium chloride aqueous solution, methyl allyl polyoxyethylene ether and hydrogen peroxide aqueous solution into the reaction kettle in sequence at room temperature and stir evenly, then add S1 and S2 solutions dropwise into the reaction kettle at the same time, and continue stirring for 0.5 to 2.0 hours after the addition is complete; (4) Finally, add ethyl orthosilicate into the reaction kettle and stir to react to obtain organosilicon hybrid oligomer.
3. The method for preparing the low-viscosity, easy-pump, fluorine-free and alkali-free liquid quick-setting agent according to claim 1 or 2, characterized in that Water, hydrated magnesium silicate and organosilicon hybrid oligomer are sequentially added into the reaction kettle downward, and aluminum sulfate is added twice after stirring evenly, and then diethanolamine is added and stirred to obtain a low-viscosity, easy-pump, fluorine-free and alkali-free liquid accelerating setting agent.
4. The preparation method according to claim 3, characterized in that: The prepared low-viscosity and easy-pump fluorine-free and alkali-free liquid quick-setting agent has a viscosity of ≤300mPa·s at 0-30°C.