Preparation method of environmentally friendly heat stabilizer for PVC foamed artificial leather

Through the combination of calcium zinc composite heat stabilizer, rare earth heat stabilizer and modified antioxidant, an environmentally friendly PVC foamed artificial leather heat stabilizer with excellent thermal stability and antioxidant properties is prepared, which solves the problem of existing heat stabilizers. Solve the problem of insufficient performance and achieve environmental protection and performance improvement.

CN118546432BActive Publication Date: 2024-10-15SHANDONG ZHENXI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410993008.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-15
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The existing calcium-zinc composite heat stabilizers and rare earth heat stabilizers have unsatisfactory thermal stabilization effects and insufficient antioxidant properties in practical applications, and traditional lead salt heat stabilizers cause harm to the environment and human health. An environmentally friendly heat stabilizer is needed. Special heat stabilizer for PVC foamed artificial leather.

Method used

Using a combination of calcium zinc composite heat stabilizer, rare earth heat stabilizer, modified hindered phenolic antioxidant, light stabilizer and lubricant, the environmentally friendly heat stabilizer is prepared through high-speed mixing and twin-screw extrusion granulation processes to enhance resistance to Oxidation properties and thermal stability.

Benefits of technology

It significantly improves the thermal stability and anti-oxidation performance of PVC materials, extends the service life of the product, meets the requirements of environmental regulations, and avoids the environmental and health hazards of traditional heat stabilizers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a method for preparing a special environmentally friendly heat stabilizer for PVC foamed artificial leather, and relates to the technical field of polymer materials. The heat stabilizer is prepared by mixing, melt blending and cooling granulation with calcium zinc composite heat stabilizer, rare earth heat stabilizer, antioxidant, light stabilizer and lubricant. The prepared heat stabilizer has excellent thermal stability and oxidation resistance, meets environmental protection requirements, and can be widely used in the production of PVC foamed artificial leather.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a method for preparing a special environmentally friendly heat stabilizer for PVC foamed artificial leather. Background Art

[0002] PVC foamed leather is a synthetic material that is formed by adding foaming agents and other additives to PVC resin and then heating and foaming. It is widely used in furniture, automobiles, clothing, shoes and other fields. PVC foamed leather has become a substitute for traditional leather due to its advantages such as light weight, softness, wear resistance and water resistance. However, PVC materials are prone to degradation during processing, especially under high temperature conditions, resulting in a decrease in material performance. Therefore, heat stabilizers play an important role in the production of PVC foamed leather.

[0003] The patent application with the publication number CN1420141A discloses an inorganic composite heat stabilizer for polyvinyl chloride processing and a preparation method thereof. The heat stabilizer comprises an inorganic carrier of zeolite, molecular sieve, and layered phosphate, and the carrier is embedded with lead-containing ultrafine particles. The surface of the ultrafine particles is lead oxide, and the center is metallic lead. The particle size is 1-100 nanometers, belonging to the category of nano materials.

[0004] The patent with the authorization announcement number CN105385072B discloses a PVC calcium zinc heat stabilizer and its auxiliary heat stabilizer, wherein the weight ratio of each component is: 40-60 parts of zinc stearate or calcium stearate or a mixture of the two; 2-5 parts of auxiliary heat stabilizer; 5-10 parts of internal lubricant; 5-10 parts of external lubricant; 1-5 parts of antioxidant; 1-5 parts of ultraviolet absorber; 1-5 parts of dispersant. The auxiliary heat stabilizer of the PVC calcium zinc heat stabilizer is an adduct of fatty alcohol or fatty acid and triglycidyl isocyanurate.

[0005] The patent with the authorization announcement number CN102093654B discloses a zinc-aluminum rare earth hydrotalcite composite heat stabilizer for PVC and its preparation and application. The composite heat stabilizer is formed by optimizing the compounding of zinc-aluminum rare earth hydrotalcite and magnesium-aluminum hydrotalcite in a certain proportion. Zinc-aluminum rare earth hydrotalcite and magnesium-aluminum hydrotalcite have good compatibility with PVC after being surface-modified by sodium stearate. The composite heat stabilizer utilizes the synergistic effect between the two types of hydrotalcites, the synergistic effect between zinc and rare earth elements in zinc-aluminum rare earth hydrotalcite, and the excellent performance of rare earth elements themselves, thereby improving the thermal stability of PVC.

[0006] Traditional PVC heat stabilizers are mainly lead salt stabilizers. Although these stabilizers have good heat stabilization effects, the heavy metal lead they contain is extremely harmful to the environment and human health. Lead and its compounds will pollute the soil, water and atmosphere during production, use and disposal, and can easily enter the human body through the food chain, causing damage to the nervous system, blood system and kidneys. In recent years, with the improvement of people's environmental awareness and the increasingly stringent relevant regulations, especially the implementation of the EU RoHS Directive and REACH regulations, the use of traditional lead salt heat stabilizers has been strictly restricted.

[0007] In this context, research and development of environmentally friendly PVC heat stabilizers has become an important topic in the field of PVC materials. Calcium zinc composite heat stabilizers, as a non-toxic and environmentally friendly heat stabilizer, have gradually become a substitute for lead salt heat stabilizers due to their excellent thermal stability and comprehensive performance. At the same time, rare earth heat stabilizers also show good application prospects in PVC heat stabilizers due to their unique structure and performance. In addition, the rational use of additives such as antioxidants, light stabilizers, lubricants and auxiliary stabilizers can further improve the comprehensive performance of heat stabilizers and meet the needs of PVC foamed artificial leather in different application fields.

[0008] However, the calcium zinc composite heat stabilizers and rare earth heat stabilizers currently available on the market still have certain limitations in practical applications, such as unsatisfactory heat stabilization effects and insufficient antioxidant properties. Therefore, a method for preparing a special environmentally friendly heat stabilizer for PVC foamed artificial leather with a reasonable formula and excellent performance is provided, which can not only meet the processing and use requirements of PVC materials, but also comply with the requirements of environmental protection regulations, and has important practical significance and broad application prospects. Summary of the invention

[0009] The invention provides a method for preparing a special environmentally friendly heat stabilizer for PVC foamed artificial leather. The heat stabilizer can not only improve the thermal stability and oxidation resistance of PVC materials, but also meet environmental protection requirements and avoid the harm of traditional heat stabilizers to the environment and health.

[0010] In order to achieve the above-mentioned invention object, the present invention proposes the following solution:

[0011] The preparation method of the environmentally friendly heat stabilizer for PVC foamed artificial leather comprises the following steps:

[0012] S1: According to the mass proportions, weigh 20-40 parts of calcium zinc composite heat stabilizer, 5-15 parts of rare earth heat stabilizer, 2-10 parts of antioxidant, 2-10 parts of light stabilizer, and 5-15 parts of lubricant;

[0013] S2: Mix the weighed materials at high speed in a mixing device for 5-10 minutes;

[0014] S3: adding the uniformly mixed materials into a twin-screw extruder for extrusion and granulation to obtain an environmentally friendly heat stabilizer for PVC foamed artificial leather.

[0015] The antioxidant in S1 is selected from modified hindered phenol antioxidants, and the preparation method thereof is as follows:

[0016] According to weight, 25-50 parts of allyl-2,6-di-tert-butylphenol, 4-8 parts of 6-vinyl indolin-2-one (CAS: 297756-30-0), 3.5-6.5 parts of 2-5-dimercapto-1-3-4-thiadiazolyl lanthanum, 2-4 parts of triethylamine and 200-400 parts of toluene are reacted at 50-70° C. for 50-100 minutes, and the toluene is removed by distillation to obtain a modified hindered phenol antioxidant.

[0017] Specifically, the calcium-zinc composite heat stabilizer in S1 is selected from one or more of calcium stearate, zinc stearate, calcium benzoate and zinc benzoate.

[0018] Specifically, the rare earth heat stabilizer in S1 is selected from one or more of rare earth benzoate, rare earth stearate, cerium benzoate and cerium stearate.

[0019] Specifically, the light stabilizer in S1 is selected from one or more of benzophenone, triazine and hindered amine light stabilizers.

[0020] Specifically, the lubricant in S1 is selected from one or more of stearic acid, paraffin, polyethylene wax and talc.

[0021] Specifically, the temperature of the twin-screw extruder in S3 is 120-160°C.

[0022] The reaction mechanism of the present invention is specifically as follows:

[0023] 1. Addition reaction: Allyl-2,6-di-tert-butylphenol and 6-vinylindolin-2-one undergo thiol-olefin addition reaction with 2-5-dimercapto-1-3-4-thiadiazolyl lanthanum;

[0024] 2. Formation mechanism: In the addition reaction, the carbon-carbon double bonds of allyl-2,6-di-tert-butylphenol and 6-vinylindolin-2-one are opened and added to the thiol group in 2-5-dimercapto-1-3-4-thiadiazolyl lanthanum to form new thiol-terminated compounds.

[0025] The beneficial effects of the present invention are as follows:

[0026] The structure and properties of indoline enable it to act as an effective free radical scavenger, blocking free radical chain reactions and thus slowing down the oxidation process. When lanthanum thiadiazole is combined with indoline, it can enhance the antioxidant activity through synergistic effects, providing additional electrons to neutralize free radicals and further prevent oxidation. This modification process enhances the antioxidant properties of the original hindered phenolic compounds, making them more suitable for use in heat stabilizers for PVC.

[0027] The newly formed antioxidant can effectively prevent PVC materials from degradation due to oxidation during high-temperature processing and use, significantly extending the service life of the product. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0029] Example 1: A method for preparing a special environmentally friendly heat stabilizer for PVC foamed artificial leather, wherein the steps are as follows:

[0030] S1: weigh 20kg calcium zinc composite heat stabilizer, 5kg rare earth heat stabilizer, 2kg antioxidant, 2kg light stabilizer, and 5kg lubricant;

[0031] S2: Mix the weighed materials at high speed in a mixing device for 5 minutes;

[0032] S3: adding the uniformly mixed materials into a twin-screw extruder for extrusion and granulation to obtain an environmentally friendly heat stabilizer for PVC foamed artificial leather.

[0033] The calcium-zinc composite heat stabilizer in S1 is selected from calcium stearate.

[0034] The rare earth heat stabilizer in S1 is selected from rare earth benzoate.

[0035] The antioxidant in S1 is selected from modified hindered phenol antioxidants, and the preparation method thereof is as follows:

[0036] 25 kg of allyl-2,6-di-tert-butylphenol, 4 kg of 6-vinyl indolin-2-one CAS: 297756-30-0, 3.5 kg of 2-5-dimercapto-1-3-4-thiadiazolyl lanthanum, 2 kg of triethylamine, and 200 kg of toluene were reacted at 50° C. for 50 minutes, and the toluene was removed by distillation to obtain a modified hindered phenol antioxidant.

[0037] Among them, the reference: Synthesis and characterization of 2,5-dimercapto-1,3,4-thiadiazole rare earth organic complexes, Xie Meihua, Zhang Lixin, Ma Huaizhu - Rare Earth 1999 No. 03, page P12, Section 1.2: Synthesis of complexes, the synthesis method in the second paragraph is to prepare 2-5-dimercapto-1-3-4-thiadiazole lanthanum.

[0038] The light stabilizer in S1 is selected from dihydroxybenzophenone.

[0039] The lubricant in S1 is selected from stearic acid.

[0040] The temperature of the twin-screw extruder in S3 is 120°C.

[0041] Embodiment 2: The preparation method of the environmentally friendly heat stabilizer for PVC foamed artificial leather, the operation steps are as follows:

[0042] S1: weigh 30kg calcium zinc composite heat stabilizer, 10kg rare earth heat stabilizer, 5kg antioxidant, 4kg light stabilizer, and 10kg lubricant;

[0043] S2: Mix the weighed materials at high speed in a mixing device for 7 minutes;

[0044] S3: adding the uniformly mixed materials into a twin-screw extruder for extrusion and granulation to obtain an environmentally friendly heat stabilizer for PVC foamed artificial leather.

[0045] The calcium-zinc composite heat stabilizer in S1 is selected from zinc stearate.

[0046] The rare earth heat stabilizer in S1 is selected from rare earth stearate.

[0047] The antioxidant in S1 is selected from modified hindered phenol antioxidants, and the preparation method thereof is as follows:

[0048] 35 kg of allyl-2,6-di-tert-butylphenol, 6 kg of 6-vinyl indolin-2-one CAS: 297756-30-0, 4.5 kg of 2-5-dimercapto-1-3-4-thiadiazolyl lanthanum, 3 kg of triethylamine, and 300 kg of toluene were reacted at 60° C. for 75 minutes, and the toluene was removed by distillation to obtain a modified hindered phenol antioxidant.

[0049] Among them, the reference: Synthesis and characterization of 2,5-dimercapto-1,3,4-thiadiazole rare earth organic complexes, Xie Meihua, Zhang Lixin, Ma Huaizhu - Rare Earth 1999 No. 03, page P12, Section 1.2: Synthesis of complexes, the synthesis method in the second paragraph is to prepare 2-5-dimercapto-1-3-4-thiadiazole lanthanum.

[0050] The light stabilizer in S1 is selected from 2,2'-dihydroxy-4-methoxybenzophenone.

[0051] The lubricant in S1 is selected from stearic acid.

[0052] The temperature of the twin-screw extruder in S3 is 135°C.

[0053] Embodiment 3: The preparation method of the environmentally friendly heat stabilizer for PVC foamed artificial leather, the operation steps are as follows:

[0054] S1: weigh 30kg calcium zinc composite heat stabilizer, 10kg rare earth heat stabilizer, 8kg antioxidant, 7.5kg light stabilizer, and 10kg lubricant;

[0055] S2: Mix the weighed materials at high speed for 8 minutes in a mixing device;

[0056] S3: adding the uniformly mixed materials into a twin-screw extruder for extrusion and granulation to obtain an environmentally friendly heat stabilizer for PVC foamed artificial leather.

[0057] The calcium-zinc composite heat stabilizer in S1 is selected from zinc stearate.

[0058] The rare earth heat stabilizer in S1 is selected from rare earth stearate.

[0059] The antioxidant in S1 is selected from modified hindered phenol antioxidants, and the preparation method thereof is as follows:

[0060] 45 kg of allyl-2,6-di-tert-butylphenol, 6 kg of 6-vinylindolin-2-one (CAS: 297756-30-0), 5.5 kg of 2-5-dimercapto-1-3-4-thiadiazolyl lanthanum, 3 kg of triethylamine, and 300 kg of toluene were reacted at 60° C. for 75 minutes, and the toluene was removed by distillation to obtain a modified hindered phenol antioxidant.

[0061] Among them, the reference: Synthesis and characterization of 2,5-dimercapto-1,3,4-thiadiazole rare earth organic complexes, Xie Meihua, Zhang Lixin, Ma Huaizhu - Rare Earth 1999 No. 03, page P12, Section 1.2: Synthesis of complexes, the synthesis method in the second paragraph is to prepare 2-5-dimercapto-1-3-4-thiadiazole lanthanum.

[0062] The light stabilizer in S1 is selected from bis-2-ethylhexyl-4-methoxyaminobenzoyl triazine.

[0063] The lubricant in S1 is selected from polyethylene wax.

[0064] The temperature of the twin-screw extruder in S3 is 140°C.

[0065] Embodiment 4: The preparation method of the environmentally friendly heat stabilizer for PVC foamed artificial leather, the operation steps are as follows:

[0066] S1: weigh 40kg calcium zinc composite heat stabilizer, 15kg rare earth heat stabilizer, 10kg antioxidant, 10kg light stabilizer, and 15kg lubricant;

[0067] S2: Mix the weighed materials at high speed in a mixing device for 10 minutes;

[0068] S3: adding the uniformly mixed materials into a twin-screw extruder for extrusion and granulation to obtain an environmentally friendly heat stabilizer for PVC foamed artificial leather.

[0069] The calcium-zinc composite heat stabilizer in S1 is selected from calcium benzoate.

[0070] The rare earth heat stabilizer in S1 is selected from cerium benzoate.

[0071] The antioxidant in S1 is selected from modified hindered phenol antioxidants, and the preparation method thereof is as follows:

[0072] 50 kg of allyl-2,6-di-tert-butylphenol, 8 kg of 6-vinylindolin-2-one (CAS: 297756-30-0), 6.5 kg of 2-5-dimercapto-1-3-4-thiadiazolyl lanthanum, 4 kg of triethylamine, and 400 kg of toluene were reacted at 70° C. for 100 minutes, and the toluene was removed by distillation to obtain a modified hindered phenol antioxidant.

[0073] Among them, the reference: Synthesis and characterization of 2,5-dimercapto-1,3,4-thiadiazole rare earth organic complexes, Xie Meihua, Zhang Lixin, Ma Huaizhu - Rare Earth 1999 No. 03, page P12, Section 1.2: Synthesis of complexes, the synthesis method in the second paragraph is to prepare 2-5-dimercapto-1-3-4-thiadiazole lanthanum.

[0074] The light stabilizer in S1 is selected from 1,6-hexanediol bis(3,5-di-tert-butyl-4-hydroxyphenyl) malonate.

[0075] The lubricant in S1 is selected from talc.

[0076] The temperature of the twin-screw extruder in S3 is 160°C.

[0077] Comparative Example 1: A method for preparing an environmentally friendly heat stabilizer for PVC foamed artificial leather, wherein the steps are as follows:

[0078] S1: weigh 20kg calcium zinc composite heat stabilizer, 5kg rare earth heat stabilizer, 2kg antioxidant, 2kg light stabilizer, and 5kg lubricant;

[0079] S2: Mix the weighed materials at high speed in a mixing device for 5 minutes;

[0080] S3: adding the uniformly mixed materials into a twin-screw extruder for extrusion and granulation to obtain the thermal stabilizer.

[0081] The calcium-zinc composite heat stabilizer in S1 is selected from calcium stearate.

[0082] The rare earth heat stabilizer in S1 is selected from rare earth benzoate.

[0083] The antioxidant in S1 is selected from allyl-2,6-di-tert-butylphenol.

[0084] The light stabilizer in S1 is selected from dihydroxybenzophenone.

[0085] The lubricant in S1 is selected from stearic acid.

[0086] The temperature of the twin-screw extruder in S3 is 120°C.

[0087] Comparative Example 2: A method for preparing an environmentally friendly heat stabilizer for PVC foamed artificial leather, wherein the steps are as follows:

[0088] S1: weigh 20kg calcium zinc composite heat stabilizer, 5kg rare earth heat stabilizer, 2kg antioxidant, 2kg light stabilizer, and 5kg lubricant;

[0089] S2: Mix the weighed materials at high speed in a mixing device for 5 minutes;

[0090] S3: adding the uniformly mixed materials into a twin-screw extruder for extrusion and granulation to obtain the thermal stabilizer.

[0091] The calcium-zinc composite heat stabilizer in S1 is selected from calcium stearate.

[0092] The rare earth heat stabilizer in S1 is selected from rare earth benzoate.

[0093] The antioxidant in S1 is selected from modified hindered phenol antioxidants, and the preparation method thereof is as follows:

[0094] 25 kg of allyl-2,6-di-tert-butylphenol, 3.5 kg of 2-5-dimercapto-1-3-4-thiadiazole lanthanum, 2 kg of triethylamine, and 200 kg of toluene were reacted at 50° C. for 50 minutes, and the toluene was removed by distillation to obtain a modified hindered phenol antioxidant.

[0095] Among them, the reference: Synthesis and characterization of 2,5-dimercapto-1,3,4-thiadiazole rare earth organic complexes, Xie Meihua, Zhang Lixin, Ma Huaizhu - Rare Earth 1999 No. 03, page P12, Section 1.2: Synthesis of complexes, the synthesis method in the second paragraph is to prepare 2-5-dimercapto-1-3-4-thiadiazole lanthanum.

[0096] The light stabilizer in S1 is selected from dihydroxybenzophenone.

[0097] The lubricant in S1 is selected from stearic acid.

[0098] The temperature of the twin-screw extruder in S3 is 120°C.

[0099] Comparative Example 3: A method for preparing an environmentally friendly heat stabilizer for PVC foamed artificial leather, wherein the steps are as follows:

[0100] S1: weigh 20kg calcium zinc composite heat stabilizer, 5kg rare earth heat stabilizer, 2kg antioxidant, 2kg light stabilizer, and 5kg lubricant;

[0101] S2: Mix the weighed materials at high speed in a mixing device for 5 minutes;

[0102] S3: adding the uniformly mixed materials into a twin-screw extruder for extrusion and granulation to obtain the thermal stabilizer.

[0103] The calcium-zinc composite heat stabilizer in S1 is selected from calcium stearate.

[0104] The rare earth heat stabilizer in S1 is selected from rare earth benzoate.

[0105] The antioxidant in S1 is selected from modified hindered phenol antioxidants, and the preparation method thereof is as follows:

[0106] 25 kg of allyl-2,6-di-tert-butylphenol, 4 kg of 6-vinylindolin-2-one (CAS: 297756-30-0), 2 kg of triethylamine and 200 kg of toluene were reacted at 50° C. for 50 minutes, and the toluene was removed by distillation to obtain a modified hindered phenol antioxidant.

[0107] The light stabilizer in S1 is selected from dihydroxybenzophenone.

[0108] The lubricant in S1 is selected from stearic acid.

[0109] The temperature of the twin-screw extruder in S3 is 120°C.

[0110] Test methods and results:

[0111] Sample preparation: Weigh 5 parts of the heat stabilizer prepared in the above examples and comparative examples and mix them evenly with 100 parts of PVC, and prepare sheet samples through a twin-screw extruder.

[0112] 1. Thermal stability test

[0113] Thermogravimetric analyzer (TGA) was used to test the thermogravimetric changes of PVC samples at different temperatures. The temperature was raised from room temperature to 800°C at a heating rate of 10°C / min. The thermogravimetric curve of the sample was recorded, and its thermal decomposition temperature and thermal weight loss rate were analyzed.

[0114] Table 1: Thermal stability test results of various embodiments and comparative examples

[0115]

[0116] 2. Antioxidant test

[0117] The oxidation induction time (OIT) test of PVC samples was used to measure the oxidation induction time of the samples in an oxygen environment by differential scanning calorimetry (DSC). The test was carried out at a constant temperature of 200°C.

[0118] Table 2: Antioxidant test results of various embodiments and comparative examples

[0119]

[0120] In summary, through the test results of different embodiments and comparative examples, it can be seen that the environmentally friendly heat stabilizer for PVC foamed artificial leather prepared by the present invention has excellent thermal stability and oxidation resistance.

[0121] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0122] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0123] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing a special environmentally friendly heat stabilizer for PVC foamed artificial leather, characterized in that: The operation steps are: S1: According to the mass proportions, weigh 20-40 parts of calcium zinc composite heat stabilizer, 5-15 parts of rare earth heat stabilizer, 2-10 parts of antioxidant, 2-10 parts of light stabilizer, and 5-15 parts of lubricant; S2: Mix the weighed materials at high speed in a mixing device for 5-10 minutes; S3: adding the uniformly mixed materials into a twin-screw extruder for extrusion and granulation to obtain an environmentally friendly heat stabilizer for PVC foamed artificial leather; The antioxidant in S1 is selected from modified hindered phenol antioxidants, and the preparation method thereof is as follows: According to weight, 25-50 parts of allyl-2,6-di-tert-butylphenol, 4-8 parts of 6-vinyl indolin-2-one, 3.5-6.5 parts of 2-5-dimercapto-1-3-4-thiadiazolyl lanthanum, 2-4 parts of triethylamine and 200-400 parts of toluene are reacted at 50-70° C. for 50-100 minutes, and the toluene is removed by distillation to obtain a modified hindered phenol antioxidant.

2. The method for preparing the environmentally friendly heat stabilizer for PVC foamed artificial leather according to claim 1, characterized in that: The calcium-zinc composite heat stabilizer in S1 is selected from one or more of calcium stearate, zinc stearate, calcium benzoate and zinc benzoate.

3. The method for preparing the environmentally friendly heat stabilizer for PVC foamed artificial leather according to claim 1, characterized in that: The rare earth heat stabilizer in S1 is selected from one or more of rare earth benzoate and rare earth stearate.

4. The method for preparing the environmentally friendly heat stabilizer for PVC foamed artificial leather according to claim 1, characterized in that: The light stabilizer in S1 is selected from one or more of benzophenone, triazine and hindered amine light stabilizers.

5. The method for preparing the environmentally friendly heat stabilizer for PVC foamed artificial leather according to claim 1, characterized in that: The lubricant in S1 is selected from one or more of stearic acid, paraffin, polyethylene wax and talc.

6. The method for preparing the environmentally friendly heat stabilizer for PVC foamed artificial leather according to claim 1, characterized in that: The temperature of the twin-screw extruder in S3 is 120-160°C.